Wear-resistant filler for coating as well as preparation method and application of wear-resistant filler
Through the method of grafting volcanic rocks by organic acid, the problem of poor compatibility between inorganic wear-resistant fillers and resin matrix is solved, the wear resistance and thermal stability of the coating are improved, the service life of lithium batteries is extended and the cost is reduced.
Patent Information
- Application Number
- CN202411107603.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-11-01
AI Technical Summary
The existing inorganic wear-resistant fillers have poor compatibility with resin matrix, resulting in uneven dispersion, inconsistent local performance, and problems such as low bonding strength, easy powder loss, and internal short circuit risk, limiting the safety performance and application range of lithium batteries.
Using organic acid grafted volcanic rocks as wear-resistant fillers, chemical grafting is performed through silane coupling agents to improve the dispersion and adhesion properties of volcanic rocks, increase the adhesion and thermal stability of the coating, and use volcanic rocks as filler substrates to improve resistance. Heat and corrosion resistance.
Improves the compatibility of fillers and resins, enhances the wear resistance, thermal stability and corrosion resistance of the coating, extends service life, and reduces costs.
Smart Images

Figure BDA0004991261170000041 
Figure BDA0004991261170000051
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of filler surface treatment, and in particular to a wear-resistant filler for coatings, a preparation method and application thereof. Background Art
[0002] Safety is one of the most concerned issues in the design and use of lithium batteries. When the active material of the negative electrode plate contacts the foil of the positive electrode, a short circuit will occur, which may easily cause safety accidents such as fire or explosion. Researchers have found that coating the edge of the active material of the positive electrode plate with insulating material can avoid the short circuit problem. Most of the existing technologies use epoxy resin, polyvinylidene fluoride and ceramic insulating materials. However, all of the above materials have certain problems and shortcomings, such as the limited adhesion of fluorine-containing materials, high prices and insufficient supply of raw materials; epoxy resin, nitrile rubber and other polymer materials have low bonding strength after being soaked in electrolyte, and are prone to powdering and leaking metal aluminum, resulting in the risk of internal short circuit; ceramic materials have the disadvantages of high hardness, poor flexibility and difficult processing. As the battery industry enters the large-scale practical stage, the development of insulating fillers and insulating adhesive materials restricts the improvement of battery safety performance and limits the scope of battery application.
[0003] Therefore, focusing on the research and development of a wear-resistant filler that can increase the wear resistance, corrosion resistance and high temperature resistance of the coating is an irreversible trend in the development of the lithium battery industry.
[0004] Patent CN 115818688 A discloses a method for preparing nano-boehmite, the preparation process of which is to mix an aluminum salt solution and an aluminate solution to obtain a mixed solution; subject the mixed solution to a slurry reaction at a set temperature to obtain a slurry material; subject the slurry material to a homogenization treatment to obtain a boehmite precursor; and subject the boehmite precursor to a slurrying and hydrothermal reaction to obtain nano-boehmite.
[0005] Patent CN116333555A discloses an epoxy alloy powder coating and its preparation method and application. The epoxy alloy powder coating comprises 20-50 parts of epoxy resin and 40-80 parts of zinc-aluminum-magnesium alloy powder by weight; the mass percentage of zinc in the zinc-aluminum-magnesium alloy powder is ≥50%.
[0006] The above patents all use inorganic materials as wear-resistant fillers, but inorganic materials have serious agglomeration, are difficult to disperse, have high salt content, and have poor compatibility, which need to be further resolved. Summary of the invention
[0007] Purpose of the invention: The purpose of the present invention is to provide a wear-resistant filler for coatings, a preparation method and an application thereof, so as to overcome the problem of poor compatibility of existing inorganic wear-resistant fillers with resin matrices, and to further improve the corrosion resistance and wear resistance of the inorganic filler.
[0008] The technical solution of the present invention:
[0009] In one aspect, the present invention provides a wear-resistant filler for coatings, wherein the wear-resistant filler is obtained by grafting volcanic rock with an organic acid.
[0010] In some embodiments, the organic acid is selected from one or more combinations of acrylic acid, methacrylic acid, cinnamic acid, linoleic acid, isoprene acid, maleic acid, and fumaric acid.
[0011] In some embodiments, the volcanic rock is selected from one or more combinations of andesite, andesite, trachyte, alkali-long trachyte, quartz andesite, quartz trachyte, and quartz-alkali-long trachyte.
[0012] In some embodiments, the grafting is chemical grafting using a silane coupling agent; further, the silane coupling agent is silane coupling agent KH-550.
[0013] In a second aspect, the present invention also provides a method for preparing the wear-resistant filler, which specifically comprises the following steps:
[0014] Step 1: Pre-treat the volcanic rock by soaking it in dilute acid;
[0015] Step 2: dissolving the silane coupling agent in a solvent and allowing the solution to stand; after the solution is allowed to stand, soaking the solution in volcanic rock, and washing and drying the solution to obtain pretreated volcanic rock;
[0016] Step 3: dissolving an organic acid in a solvent to obtain an organic acid solution; placing the pretreated volcanic rock and the same solvent into a reactor, slowly dropping the organic acid solution, reacting under heating conditions, cooling, filtering, washing and drying after the reaction to obtain the wear-resistant filler.
[0017] In some embodiments, the mass ratio of the silane coupling agent to the pretreated volcanic rock is 0.5-5%; further, the mass ratio of the silane coupling agent to the pretreated volcanic rock is 0.5-2%.
[0018] In some embodiments, the molar ratio of the organic acid to the silane coupling agent is 1:1-2.
[0019] In some embodiments, the reaction is carried out under heating conditions, specifically the reaction temperature is 60-80° C., and the reaction time is 2-4 h.
[0020] In a third aspect, the present invention also provides use of the wear-resistant filler in a wear-resistant ceramic coating.
[0021] Beneficial effects:
[0022] 1. The wear-resistant filler provided by the present invention uses volcanic rock as a base, which has strong heat resistance, wear resistance and corrosion resistance. The volcanic rock used as the base of the filler has a wide source and saves costs.
[0023] 2. By surface-modifying volcanic rock to obtain a wear-resistant filler, the dispersibility and bonding properties of the volcanic rock in the composite material can be improved. Compared with the existing inorganic wear-resistant filler, the wear-resistant filler provided by the present invention has better compatibility with the resin, reducing the problem of inconsistent local performance caused by uneven dispersion.
[0024] 3. Further grafting organic acid on the surface of volcanic rock, the grafting of organic acid can enhance the adhesion of the coating, thereby providing better shielding protection, enhancing the thermal stability of the coating, and slowing down thermal decomposition and thermal oxidation.
[0025] Therefore, the wear-resistant material obtained by the technical solution of the present invention has excellent wear resistance, thermal stability and corrosion resistance, thereby extending the service life. DETAILED DESCRIPTION
[0026] The present invention will be described below in conjunction with specific embodiments. It should be noted that the following embodiments are examples of the present invention and are only used to illustrate the present invention, but not to limit the present invention. Other combinations and various modifications within the concept of the present invention may be performed without departing from the spirit or scope of the present invention.
[0027] Unless otherwise specified, the chemical reagents used in the present invention are all commercially available analytically pure.
[0028] Example 1
[0029] Step 1: Pre-treat 10 g of anchovy rock by soaking it in excess 5% HCl for 2 h;
[0030] Step 2: Dissolve 0.05g of silane coupling agent KH-550 in 50ml of a mixed solvent of ethanol and water (volume ratio of ethanol: water = 95:5), and let it stand; after standing, put 10g of pre-treated anchovy rock into it for soaking, and after soaking, wash and dry it to obtain grafted anchovy rock;
[0031] Step 3: dissolve 0.05 g of acrylic acid in 30 ml of toluene to obtain an acrylic acid solution; put the pretreated anhydrous rock obtained in step 2 and 30 ml of toluene into a reactor, slowly drop the acrylic acid solution, react at 60° C. for 2 h, cool, filter, wash and dry after the reaction to obtain the wear-resistant filler 1.
[0032] Fourier transform infrared spectroscopy (FTIR) data: 1000-1100cm -1 Si-O-Si stretching vibration; 1700cm -1C=O stretching vibration; 2800-3000cm -1 CH3 stretching vibration; no C=C stretching vibration occurs. This indicates that acrylic acid is successfully grafted onto the surface of the anthracite through KH-550.
[0033] Example 2
[0034] The preparation method of the wear-resistant filler 2 is similar to that of the wear-resistant filler 1, except that methacrylic acid is used instead of acrylic acid.
[0035] Example 3
[0036] The preparation method of wear-resistant filler 3 is similar to that of wear-resistant filler 1, except that fumaric acid is used instead of acrylic acid.
[0037] Example 4
[0038] The preparation method of wear-resistant filler 4 is similar to that of wear-resistant filler 1, except that the added amount of silane coupling agent is 0.5 g and the added amount of acrylic acid is 0.46 g.
[0039] Example 5
[0040] The preparation method of wear-resistant filler 5 is similar to that of wear-resistant filler 1, except that the added amount of silane coupling agent is 0.2 g and the added amount of acrylic acid is 0.19 g.
[0041] Comparative Example 1
[0042] The preparation method of wear-resistant filler 6 is similar to that of wear-resistant filler 1, except that step 3 is omitted, and the same weight of acrylic acid is physically mixed with the grafted anhydrite obtained in step 2 to obtain wear-resistant filler 6.
[0043] Comparative Example 2
[0044] The preparation method of wear-resistant filler 7 is similar to that of wear-resistant filler 1, except that the added amount of silane coupling agent is 1 g and the added amount of acrylic acid is 0.93 g.
[0045] Comparative Example 3
[0046] An rough rock is recorded as wear-resistant filler 8.
[0047] The above-mentioned wear-resistant filler and resin are mixed with the following materials respectively to obtain the wear-resistant coating:
[0048] 100 parts of epoxy resin E-44, 50 parts of wear-resistant filler, 1 part of defoamer BKY-024, 2 parts of leveling agent Digo 760w, 2 parts of P123 nonionic surfactant, 8 parts of deionized water, and 10 parts of curing agent hexamethylenediamine. Wear-resistant coatings were obtained respectively.
[0049] The wear-resistant coating is evenly sprayed on the surface of the metal substrate by an air pump spraying method to obtain a corresponding coating.
[0050] The prepared coating was placed in air and cured at room temperature for 10 hours, then at 120°C for 6 hours, and finally at 150°C for 2 hours. The composite coating was completely cured by gradually increasing the temperature. The following tests were performed:
[0051] 1. Abrasion test: Refer to GB / T 1768-2006 for the determination of abrasion resistance of paint and varnish, and the equipment used is Taber abrasion tester. The test cycle is 1000 times, and the applied weight is 1000g.
[0052] 2. Liquid resistance test: Refer to the provisions of GB / T9274-2021, immerse in 10% H2SO4 solution or 10% NaOH for 30 days, take out the sample and wipe it dry with filter paper, and visually observe the paint film under scattered sunlight. Discoloration and gloss loss are allowed. If there is no abnormal phenomenon of the paint film such as blistering, cracking, peeling, rusting, etc., it will be rated as "no abnormality".
[0053] 3. Heat resistance test: Add the sample to a muffle furnace, heat to 600°C, and keep it for 10 hours. After cooling to room temperature, observe the sample surface to see if there are any cracks or paint film shedding. If there is no paint film shedding or cracking, it is rated as "no abnormality".
[0054] 4.Hardness test: Test the hardness of the coating in accordance with GB / T6739-1996.
[0055] The above experimental results are shown in Table 1.
[0056] Table 1 Test results
[0057]
[0058]
[0059] In summary, compared with Examples 1-5, since the wear-resistant filler 6 in Comparative Example 1 was not modified by organic acid grafting, the effects in the heat resistance and liquid resistance tests were worse than those of the wear-resistant filler provided in the Examples, resulting in partial cracking, paint film shedding or blistering on the coating surface, thereby affecting the normal operation of the coating in high-temperature batteries.
[0060] By comparing Examples 1-5, it can be seen that when acrylic acid is selected as the type of organic acid, and the added mass ratio of anchoyanite, organic acid and silane coupling agent KH-550 is about 10:0.2:0.2, the number of organic side chains grafted on the surface can have good liquid resistance and heat resistance without affecting the mechanical properties of the coating itself, such as hardness and brittleness, thereby achieving a more excellent effect.
[0061] The present invention can also have many other embodiments. Without departing from the spirit and essence of the present invention, those skilled in the art can make various corresponding changes and modifications based on the present invention, but these corresponding changes and modifications should all fall within the scope of protection of the claims attached to the present invention.
Claims
1. A wear-resistant filler for coating, characterized in that: The wear-resistant filler is obtained by grafting organic acid onto volcanic rock.
2. The wear-resistant filler according to claim 1, characterized in that: The organic acid is selected from one or more combinations of acrylic acid, methacrylic acid, cinnamic acid, linoleic acid, isoprene acid, maleic acid, and fumaric acid.
3. The wear-resistant filler according to claim 1, characterized in that: The volcanic rock is selected from one or more combinations of andesite, andesite, trachyte, alkali-long trachyte, quartz andesite, quartz trachyte, and quartz-alkali-long trachyte.
4. The wear-resistant filler according to claim 1, characterized in that: The grafting is carried out chemically by using a silane coupling agent.
5. The wear-resistant filler according to claim 4, characterized in that: The silane coupling agent is silane coupling agent KH-550.
6. The method for preparing the wear-resistant filler according to any one of claims 1 to 5, characterized in that: The steps include: Step 1: Pre-treat the volcanic rock by soaking it in dilute acid; Step 2: dissolving the silane coupling agent in a solvent and allowing the solution to stand; after the solution is allowed to stand, soaking the solution in volcanic rock, and washing and drying the solution to obtain pretreated volcanic rock; Step 3: dissolving an organic acid in a solvent to obtain an organic acid solution; placing the pretreated volcanic rock and the same solvent into a reactor, slowly dropping the organic acid solution, reacting under heating conditions, cooling, filtering, washing and drying after the reaction is completed to obtain the wear-resistant filler.
7. The method for preparing the wear-resistant filler according to claim 6, characterized in that: The added mass ratio of the silane coupling agent to the pretreated volcanic rock is 0.5-5%.
8. The method for preparing the wear-resistant filler according to claim 6, characterized in that: The added molar ratio of the organic acid to the silane coupling agent is 1:1-2.
9. The method for preparing the wear-resistant filler according to claim 6, characterized in that: The reaction is carried out under the heating conditions, specifically the reaction temperature is 60-80° C., and the reaction time is 2-4 hours.
10. Use of the wear-resistant filler according to any one of claims 1 to 5 in a wear-resistant ceramic coating.