Corrosion-resistant biphase titanium-based medium-entropy alloy and preparation method thereof

By optimizing the component ratio and preparation process of Ti, Zr, Hf, and Hf, a corrosion-resistant biphasic titanium-based medium-entropy alloy is designed, which solves the problem of insufficient performance of traditional titanium alloys in extreme corrosion environments and realizes high-performance and low-cost materials application.

CN118880109APending Publication Date: 2024-11-01NORTHEAST DIANLI UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410934433.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

Traditional titanium alloys have insufficient mechanical properties and corrosion resistance under extreme corrosion environments and high temperature conditions. The high-entropy alloys have complex composition and high preparation costs. There is little research on corrosion performance of medium-entropy alloys.

Method used

Design a corrosion-resistant biphasic titanium-based medium entropy alloy, optimize the composition ratios of Ti, Zr, Hf to Ti 75%, Zr 12.5%, Hf, or other proportions, and repeat the smelting by vacuum arc smelting and flipped ingots. Cooling and heat treatment preparation, suitable for high corrosion environments.

Benefits of technology

It significantly improves the hardness, strength and corrosion resistance of the alloy, reduces production costs, is suitable for shallow sea environments and acidic media environments in chemical plants, and is suitable for aerospace, medical devices and automobile industries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118880109A_ABST
    Figure CN118880109A_ABST
Patent Text Reader

Abstract

The invention discloses a corrosion-resistant biphase titanium-based medium-entropy alloy and a preparation method thereof, and belongs to the technical field of material science and alloy engineering. The corrosion-resistant double-phase titanium-based medium-entropy alloy comprises the following components in percentage by atom: 75% of Ti, 12.5% of Zr and 12.5% of Hf, or 77.8% of Ti, 11.1% of Zr and 11.1% of Hf; or 80% of Ti, 10% of Zr and 10% of Hf. According to the invention, a novel alloy material with high corrosion resistance is designed by optimizing the component proportion of Ti, Zr and Hf, and the solution strengthening effect of the alloy is optimized, so that the hardness and strength of the material are improved. The new alloy achieves a balance between high strength and high hardness, and can meet the application requirements in a high-stress environment. And meanwhile, the stability and durability of the alloy in a corrosion environment are improved through a new alloy proportion optimized microstructure. Through reasonable alloy design, the production cost is controlled, and it is ensured that the new alloy has high cost performance while the performance is improved. The new alloy can be used for aerospace engines, medical instrument bone implants or automobile suspension systems and the like, and economic and efficient material selection is provided for industrial production and application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of material science and alloy engineering, and specifically relates to a corrosion-resistant dual-phase titanium-based medium-entropy alloy and a preparation method thereof. Background Art

[0002] Titanium and titanium alloys have many excellent properties such as low density, high specific strength, and good corrosion resistance. They are a new type of functional material with great development potential and application prospects. They are extremely important structural materials in the aerospace industry and are known as the emerging "third metal" and "smart metal". Although titanium alloys have many excellent properties, the mechanical properties and corrosion resistance of traditional titanium alloys still need to be improved in certain extreme corrosive environments and high temperature conditions. In addition, with the continuous increase in industrial demand, the development of titanium alloys with higher strength, better corrosion resistance and better thermal stability has become an important research direction in the field of materials science.

[0003] In recent years, high entropy alloys have become a research hotspot in the field of materials science due to their unique multi-primary element composition and excellent comprehensive properties. However, their composition is complex, the preparation cost is high, and some systems still have certain limitations in practical applications. As a new type of alloy system, medium entropy alloys take into account the excellent performance of high entropy alloys and the cost advantages of traditional alloys by maintaining a low entropy value in the composition design and introducing multiple main elements. Medium entropy alloys in the Ti-Zr-Hf system have gradually attracted widespread attention due to their potential excellent properties. However, the current research on the Ti-Zr-Hf system is relatively limited, especially in terms of specific corrosion properties. Summary of the invention

[0004] In order to solve the insufficient performance of existing titanium alloys in extreme corrosion environments, the present invention provides a corrosion-resistant dual-phase titanium-based medium-entropy alloy and a preparation method thereof. The alloy is a dual-phase TiZrHf titanium-based medium-entropy alloy. By optimizing the composition ratio of Ti, Zr, and Hf, an alloy material with high corrosion resistance is designed. In addition, the alloy also shows significant advantages in mechanical properties and is suitable for long-term use in highly corrosive environments such as artificial seawater solutions simulating shallow sea environments and acidic medium environments in simulated chemical plants. Through the present invention, it is intended to provide an alloy material with high cost-effectiveness and excellent performance to meet the market demand for high-performance corrosion-resistant materials, thereby promoting the application and development of new materials in the engineering field.

[0005] To achieve the above object, the present invention provides the following technical solutions:

[0006] One of the technical solutions of the present invention is to provide a corrosion-resistant dual-phase titanium-based medium-entropy alloy, which, in atomic percentage, comprises: 75% Ti, 12.5% ​​Zr and 12.5% ​​Hf; or 77.8% Ti, 11.1% Zr and 11.1% Hf; or 80% Ti, 10% Zr and 10% Hf.

[0007] The second technical solution of the present invention is to provide a method for preparing the above-mentioned corrosion-resistant dual-phase titanium-based medium-entropy alloy, which is characterized in that the steps include: melting the metal raw material and then casting it, turning the ingot over and repeatedly melting it 4 to 5 times, cooling and heat treating it to obtain the corrosion-resistant dual-phase titanium-based medium-entropy alloy.

[0008] Preferably, the smelting is carried out in an argon atmosphere.

[0009] The third technical solution of the present invention is to provide an application of the above-mentioned corrosion-resistant dual-phase titanium-based medium-entropy alloy in a corrosive environment.

[0010] Preferably, the corrosive environment includes an artificial seawater solution in a shallow sea environment and an acidic medium environment in a chemical plant.

[0011] Technical solution 4 of the present invention: provides an application of the above-mentioned corrosion-resistant dual-phase titanium-based medium-entropy alloy in aerospace, medical equipment or automotive industry.

[0012] The beneficial technical effects of the present invention are as follows:

[0013] The present invention designs a new alloy material with high corrosion resistance by optimizing the composition ratio of Ti, Zr and Hf, optimizes the solid solution strengthening effect of the alloy, and thus improves the hardness and strength of the material. The new alloy achieves a balance between high strength and high hardness, and can meet the application requirements in high stress environments. At the same time, the microstructure of the new alloy ratio is optimized to improve its stability and durability in a corrosive environment.

[0014] The present invention controls production costs through reasonable alloy design, ensuring that the new alloy has a high cost-effectiveness while improving performance. The new alloy can be used in corrosive environments such as artificial seawater solutions in shallow sea environments and acidic media environments in chemical plants, as well as in aerospace engines, medical device bone implants, or automotive industrial suspension systems that have high performance requirements for alloys, providing economical and efficient material selection for industrial production and application. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 The Vickers hardness test results of the four alloys prepared in Examples 1-3 and Comparative Example 1 are shown.

[0016] Figure 2 Engineering stress-strain curves of four alloys prepared in Examples 1-3 and Comparative Example 1.

[0017] Figure 3 Polarization curves of four alloys prepared in Examples 1-3 and Comparative Example 1.

[0018] Figure 4 Graph showing EIS test results of four alloys prepared in Examples 1-3 and Comparative Example 1.

[0019] Figure 5 The ECCI diagrams of the four alloys prepared in Examples 1-3 and Comparative Example 1, wherein (a1) is the ECCI diagram of TZH6, (a2) is the ECCI diagram of TZH7, (a3) ​​is the ECCI diagram of TZH8, and (a4) is the ECCI diagram of TC4. DETAILED DESCRIPTION

[0020] Now, various exemplary embodiments of the present invention are described in detail, and this detailed description should not be considered as a limitation of the present invention, but should be understood as a more detailed description of certain aspects, characteristics and embodiments of the present invention. It should be understood that the terms described in the present invention are only for describing specific embodiments and are not used to limit the present invention.

[0021] In addition, for the numerical range in the present invention, it is understood that each intermediate value between the upper and lower limits of the range is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0022] Unless otherwise specified, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which the invention pertains. Although only preferred methods and materials are described herein, any methods and materials similar or equivalent to those described herein may also be used in the practice or testing of the present invention.

[0023] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0024] Example 1

[0025] The corrosion-resistant dual-phase titanium-based medium entropy alloy of this embodiment contains three elements: Ti, Zr, and Hf, and the atomic percentage of each element is: Ti 75%, Zr 12.5%, and Hf 12.5%, denoted as TZH6.

[0026] The preparation process is as follows: the purity of the metal raw materials used is 99.9% or above. Before weighing, the oxide film on the surface of the raw materials is first removed to avoid the oxide film affecting the metal forming process and component accuracy during the smelting process. In order to accurately weigh the proportion of the components, an FA1004 electronic balance with a resolution of 0.0001g is used for operation. After weighing, the raw materials are packaged and placed in a vacuum drying kettle for storage; the alloy ingot is melted in a vacuum arc furnace and high vacuum is drawn to 7×10 -3 Pa, high-purity argon was filled as a protective gas. In order to ensure uniform composition, the alloy ingot was repeatedly smelted 4 times before casting, and a stirring rod was used for stirring during the smelting process. Finally, the alloy sample was prepared.

[0027] The smelting in this embodiment adopts vacuum arc melting, and the specific steps are as follows:

[0028] 1. Preparation:

[0029] Sample preparation: weigh the required raw materials (such as metal powder or bulk raw materials) in proportion and mix them evenly. If powder is used, it is usually necessary to pre-press it into blocks for smelting.

[0030] Preparation of melting furnace: Check all parts of vacuum arc melting furnace to ensure the equipment is normal. Clean the melting chamber, check the condition of electrodes and crucibles, and replace new electrodes and crucibles if necessary.

[0031] 2. Loading:

[0032] Put the prepared raw materials into the crucible, place it on the workbench in the melting chamber, close the melting chamber and ensure it is sealed. Make sure the materials are evenly distributed to avoid eccentricity.

[0033] 3. Vacuuming:

[0034] Close the door of the melting chamber, start the vacuum pump, and evacuate the melting chamber. Evacuate to a high vacuum of 7×10 -3 Pa or less to remove oxygen and other impurities in the air and prevent the metal from being oxidized during the smelting process.

[0035] 4. Filling with inert gas:

[0036] Under high vacuum, inert gas argon is filled in to further protect the metal materials during the smelting process. The function of the inert gas is to prevent oxidation and impurity contamination of the materials during the melting process.

[0037] 5. Preheating:

[0038] The material is preheated to reduce the temperature stress and gas evolution generated during the smelting process.

[0039] 6. Arc:

[0040] Adjust the distance between the electrode and the raw material, start the arc power supply, and start melting through the electrode arc. The arc voltage is set to 25V, and the arc melting temperature is about 5000℃, which makes the metal melt quickly.

[0041] 7. Melting:

[0042] Control the position of the arc and the melting time to make the materials completely melted and mixed evenly. Depending on the characteristics of the molten material and the target composition, the melting time and arc power need to be precisely controlled.

[0043] 8. Stirring and alloying:

[0044] During the melting process, mechanical stirring is used to promote the uniform distribution of alloying elements, and the melt is kept at the melting temperature for 25 minutes to ensure full alloying.

[0045] 9. Casting:

[0046] After the initial smelting is completed, the current is gradually reduced to allow the melt to cool and solidify in the mold.

[0047] A water-cooled rapid cooling device is used to accelerate the solidification process to obtain a fine-grained structure.

[0048] 10. Cooling and unloading:

[0049] After the melt solidifies, the arc melting system is turned off and the pressure in the melting chamber is gradually restored.

[0050] After the mold and alloy ingot have cooled to a safe temperature, open the smelting chamber and take out the alloy ingot.

[0051] 11. Remelting:

[0052] After the initial smelting is completed and cooled, open the smelting chamber and carefully remove the alloy ingot from the crucible using special tools. Carefully check the appearance of the alloy ingot to ensure that there are no obvious defects or inclusions. If serious defects are found, it may be necessary to re-formulate the raw materials and re-smelt. Clean the residue in the crucible to ensure that the crucible is clean and free of contamination. If the crucible is damaged or worn, it needs to be replaced with a new crucible. Put the alloy ingot back into the crucible, ensuring that the position of the alloy ingot is changed so that it can be heated and mixed more evenly during the next smelting process. If necessary, the alloy ingot can be turned 180 degrees or its placement angle can be changed. If the alloy ingot is large in size, it can be cut into smaller pieces for re-smelting and uniform mixing.

[0053] Repeat steps 3 to 11 three times to ensure the uniformity and purity of the alloy, wherein the time for the melt in step 8 to be kept at the melting temperature during the remelting process is adjusted from 25 min to 15 min.

[0054] 12. Cast again

[0055] After remelting, the current is gradually reduced again to allow the melt to cool and solidify in the mold.

[0056] A water-cooled rapid cooling device is used to accelerate the solidification process to obtain a fine-grained structure.

[0057] 13. Cooling and removing from oven

[0058] After the remelted melt solidifies, the arc melting system is turned off and the pressure in the melting chamber is gradually restored.

[0059] After the mold and alloy ingot have cooled to a safe temperature, open the smelting chamber and take out the alloy ingot.

[0060] Example 2

[0061] Compared with Example 1, the difference is that the atomic percentage of each element is Ti 77.8%, Zr 11.1% and Hf 11.1%, which is recorded as TZH7.

[0062] Example 3

[0063] Compared with Example 1, the difference is that the atomic percentage of each element is Ti 80%, Zr 10% and Hf 10%, which is recorded as TZH8.

[0064] Comparative Example 1

[0065] Compared with Example 1, the difference is that the atomic percentage of each element is Ti 86.2%, Al 10.2% and V 3.6%, which is recorded as TC4 (conventional TC4 titanium alloy).

[0066] Preparation of samples to be tested:

[0067] The titanium alloy prepared in Examples 1-3 and Comparative Example 1 was cut into blocks of 10×10×5 mm and small strips of 5×5×10 mm. The cut alloy samples were packaged in a tube for heat treatment (specifically, at a temperature of 1200°C, the alloy samples were homogenized for 2 hours and then the alloy samples were rapidly cooled by breaking the quartz tube.), the heat-treated alloy samples were immersed in liquid nitrogen at -196°C for 3 minutes, and the surfaces were observed to be unresponsive and then taken out, and allowed to stand at room temperature, thereby obtaining the alloy samples to be tested, and the mechanical properties and electrochemical properties were tested respectively. Before the test, the samples needed to be polished to ensure that they reached a state suitable for testing. The sample surface was polished with 600#, 1000#, 2000# and 3000# water-abrasive sandpaper in turn to make the surface smooth and tidy, and then rinsed with anhydrous ethanol, and finally the alloy sample was placed in anhydrous ethanol for ultrasonic vibration for 2 minutes, and the surface was washed with deionized water after being taken out with tweezers, and then the surface was left to stand and dried with a hair dryer to obtain the alloy sample to be tested. A three-electrode system was used in the electrochemical test experiment, in which the working electrode was prepared by inlaying the prepared alloy sample, the reference electrode was a saturated calomel electrode, and the auxiliary electrode was a platinum electrode. The three electrodes were assembled on the same horizontal line and placed in a closed electrolytic cell containing 3.5wt.% NaCl solution. After ensuring that the test was correct, the three electrodes were connected to the electrochemical workstation and the experiment began.

[0068] Figure 1 The Vickers hardness test results of the four alloys prepared in Examples 1-3 and Comparative Example 1 are shown below. The hardness test can provide information about the material's ability to resist deformation and wear, which is particularly important for alloys used in high stress environments. Figure 1 It can be observed that the TZH7 alloy shows excellent wear resistance with the highest hardness of 464HV, which is significantly better than the traditional TC4 alloy (435HV) and other new alloys, indicating that the alloy has advantages in resisting deformation and wear, and is suitable for applications in aerospace engines, medical device bone implants or automotive suspension systems. The solid solution strengthening effect of the TZH7 alloy is optimal. At this ratio, the alloy elements are evenly distributed in the matrix, and the effect of hindering dislocation movement is the strongest, so the hardness is the highest.

[0069] Figure 2 The engineering stress-strain curves of the four alloys prepared in Examples 1-3 and Comparative Example 1. During the whole process, the alloys experienced three stages: elastic deformation, yielding and fracture. Figure 2 It is observed that TZH7 alloy exhibits higher ductility under high stress, indicating its superior performance in high stress applications. In contrast, TC4 alloy has relatively low ductility despite its higher strength.

[0070] Figure 3 The results of polarization curve tests of the four alloys prepared in Examples 1-3 and Comparative Example 1 at room temperature in a 3.5wt.% NaCl aqueous solution from -2V to 2V. The corrosion potential indicates the potential at which the alloy begins to corrode. The higher the corrosion potential, the better the corrosion resistance of the material. Figure 3 It can be seen that the highest corrosion potential of TZH8 is -1.45V, and the corrosion potentials of the remaining three alloys are relatively close, which indicates that they have similar corrosion resistance in the initial corrosion stage. The corrosion current density can be determined by the current density of the curve at the corrosion potential. The lower the corrosion current density, the lower the corrosion rate of the material and the better the corrosion resistance. Figure 3 It can be seen that the corrosion current density of TZH7 and TZH8 is lower, indicating that they have better corrosion resistance. In particular, TZH8 has the lowest current density near the corrosion potential, indicating that its corrosion resistance is the best. All the tested alloys did not break down during the polarization process, indicating that they formed a stable passivation film within the test potential range. The passivation film is a protective oxide layer that can effectively prevent the direct contact between the corrosive medium and the alloy matrix, thereby significantly reducing the corrosion rate. Figure 3 It can be seen that each alloy exhibits obvious passivation behavior in the positive potential region, that is, at higher potentials, the current density remains at a lower level. This indicates that the passivation film can remain stable at high potentials, preventing further corrosion of the alloy.

[0071] Figure 4 The electrochemical impedance spectroscopy (EIS) test results of the four alloys prepared in Examples 1-3 and Comparative Example 1. The size of the arc in the electrochemical impedance spectrum reflects the size of the charge transfer resistance. Figure 4 The results show that the arc of TZH8 alloy is the largest, indicating that it has the highest charge transfer resistance, indicating that its passivation film is the most stable and dense, and can effectively protect the alloy matrix from corrosion. The arc of TC4 alloy is the smallest, the charge transfer resistance is the lowest, the passivation film stability is poor, and the corrosion resistance is not as good as the new titanium-based medium entropy alloy.

[0072] The above results show that by adjusting the ratio of Ti, Zr and Hf, the present invention can significantly improve the corrosion resistance of titanium-based medium entropy alloys. TZH8 and TZH7 alloys are particularly suitable for applications in highly corrosive environments and exhibit excellent corrosion resistance.

[0073] Figure 5 The ECCI diagrams of the four alloys prepared in Examples 1-3 and Comparative Example 1, wherein (a1) is the ECCI diagram of TZH6, (a2) is the ECCI diagram of TZH7, (a3) ​​is the ECCI diagram of TZH8, and (a4) is the ECCI diagram of TC4. Figure 5It is shown that the new titanium-based medium-entropy alloy provided by the present invention has a more uniform and stable two-phase structure in microstructure. This two-phase structure can improve the mechanical properties and corrosion resistance of the alloy because the interface between different phases can hinder the movement of dislocations, thereby increasing the strength and hardness of the material.

[0074] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A corrosion-resistant dual-phase titanium-based medium-entropy alloy, characterized in that: Calculated by atomic percentage, the components of the corrosion-resistant dual-phase titanium-based medium entropy alloy are: Ti 75%, Zr 12.5% ​​and Hf 12.5%; or Ti 77.8%, Zr 11.1% and Hf 11.1%; or Ti 80%, Zr 10% and Hf 10%.

2. A method for preparing the corrosion-resistant dual-phase titanium-based medium-entropy alloy according to claim 1, characterized in that the steps include: The metal raw material is melted and then cast, the ingot is turned over and the melting is repeated 4 to 5 times, and the corrosion-resistant dual-phase titanium-based medium-entropy alloy is obtained after cooling and heat treatment.

3. The method for preparing the corrosion-resistant dual-phase titanium-based medium-entropy alloy according to claim 2, characterized in that: The smelting is carried out in an argon atmosphere.

4. Application of the corrosion-resistant dual-phase titanium-based medium entropy alloy according to claim 1 in a corrosive environment.

5. The use according to claim 4, characterized in that: The corrosive environment includes an artificial seawater solution in a shallow sea environment and an acidic medium environment in a chemical plant.

6. Application of the corrosion-resistant dual-phase titanium-based medium entropy alloy according to claim 1 in aerospace engines, medical device bone implants or automotive industrial suspension systems.