Amino acid-based compound vapor phase corrosion inhibitor as well as preparation method and application thereof

By preparing amino acid-based composite gas-phase corrosion inhibitors, using polymetal atom adsorption center and highly volatile alanine, a synergistic hydrophobic membrane is formed, which solves the toxicity and low volatility of existing gas-phase corrosion inhibitors and achieves high efficiency Carbon steel anti-rust effect.

CN118880339APending Publication Date: 2024-11-01QINGDAO UNIV OF SCI & TECH +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411112694.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

Existing gas-phase corrosion inhibitors have toxicity and low volatility limitations in the field of rust prevention, making them difficult to effectively apply to metal products of complex shapes and structures, and lacks modified amino acids and BCAU, thiourea and sodium dodecylbenzenesulfonate. combination development.

Method used

By preparing bicyclohexylamine methylurea, thiourea, sodium dodecylbenzenesulfonate and alanine ternary complexes, an amino acid-based compound gas-phase corrosion inhibitor is prepared, utilizing the high volatility and greenness of ALA-T Environmentally friendly characteristics, combining the polymetal atomic adsorption center of BCAU, thiourea and SDBS to form a synergistic hydrophobic film to prevent the formation of electrolyte liquid film and corrosive ion erosion.

Benefits of technology

It has achieved efficient rust prevention of carbon steel materials, with a corrosion inhibition efficiency of 95.52%, low toxicity, easy to obtain, uniform volatility and stable, significantly reducing the risks of metal electrochemical reactions and electrochemical corrosion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118880339A_ABST
    Figure CN118880339A_ABST
Patent Text Reader

Abstract

The invention discloses a gas phase corrosion inhibitor for carbon steel and a preparation method of the gas phase corrosion inhibitor. The compound vapor phase corrosion inhibitor is prepared from dicyclohexylamine methylurea, thiourea, sodium dodecyl benzene sulfonate and an alanine ternary complex according to the mass ratio of (10 to 30): (20 to 40): (3 to 10): (1 to 3). And the alanine ternary complex is added, so that the compound vapor phase corrosion inhibitor has a remarkable corrosion inhibition effect on atmospheric corrosion of carbon steel and has a lasting protection effect. The vapor phase corrosion inhibitor provided by the invention has the advantages of easily available raw materials, simple preparation method, convenience in use, simplicity in operation, small corrosion inhibitor dosage, low cost, excellent antirust effect on carbon steel products and the like. The compound vapor phase corrosion inhibitor does not contain toxic chemical substances, and has the advantages of being green and environmentally friendly.
Need to check novelty before this filing date? Find Prior Art

Description

Technical field:

[0001] The invention relates to the technical field of metal vapor phase rust prevention, and specifically refers to an amino acid-based composite vapor phase corrosion inhibitor, a preparation method thereof, and application in rust-proof paper. Background technology:

[0002] Metal corrosion is a common and ongoing problem. For many years, people have been committed to finding more effective anti-corrosion measures to reduce the losses caused by metal corrosion and improve the life and reliability of equipment and infrastructure. Vapor corrosion inhibitors (VCI) can volatilize gases at room temperature or lower temperatures, and act on the metal surface through corrosion-inhibiting molecules or corrosion-inhibiting groups, thereby slowing down or even preventing atmospheric corrosion of metals. For metal products with special shapes and complex structures, VCI and its technology have absolute advantages over contact rust prevention. Compared with traditional corrosion inhibition methods such as organic and inorganic coatings, the main advantage of VCI is that it can cover the entire surface of carbon steel, even very small areas, and it can form a protective film on carbon steel. Because the VCI film is very thin, it will not affect subsequent use. However, the toxicity and low corrosion inhibition of VCI limit its application. Therefore, the development of an environmentally friendly and efficient VCI is crucial to people's production and life and scientific and technological development.

[0003] Biscyclohexylamine methyl urea (BCAU) contains more N atoms and O atoms and has a strong adsorption capacity on the surface of carbon steel. BCAU has a larger molecular volume, a larger bonding area with the metal, and more atoms bonded to the metal. The lone pair of electrons in the BCAU structure coordinates with the empty orbitals in the metal, enhancing its bonding ability with the metal. Therefore, the adsorption protective film formed on the metal surface is denser and can better inhibit electrochemical corrosion on the metal surface.

[0004] As an easily available and decomposable natural organic matter, the corrosion inhibition performance of amino acids has been confirmed in many studies. However, due to its low volatility, its application in the field of gas phase corrosion inhibition is limited. Its volatility can be improved by intramolecular chemical modification. The compounding can be adjusted according to the specific corrosion environment and the requirements of metal materials to improve the performance and adaptability of the corrosion inhibitor. So far, there has been no report on the development of compound VCI by combining modified amino acids with BCAU, thiourea and sodium dodecylbenzene sulfonate. Summary of the invention:

[0005] In view of the deficiencies in the prior art and the needs of research and application in the field, one of the purposes of the present invention is to provide an amino acid-based composite vapor phase corrosion inhibitor, which is characterized by being prepared by preparing a mixed aqueous solution of dicyclohexylamine methyl urea, thiourea, sodium dodecylbenzene sulfonate and alanine ternary complex, wherein the mass ratio of dicyclohexylamine methyl urea: thiourea: sodium dodecylbenzene sulfonate: alanine ternary complex is 10-30: 20-40: 3-10: 1-3; wherein dicyclohexylamine methyl urea is recorded as BCAU, sodium dodecylbenzene sulfonate is recorded as SDBS, and alanine ternary complex is recorded as ALA-T;

[0006] The second object of the present invention is to provide a method for preparing an amino acid-based composite vapor phase corrosion inhibitor, which specifically comprises the following steps:

[0007] Step 1, preparation of ALA-T by solvent-free method: 2-8 g of L-alanine and 4-10 mL of phosphoric acid were added to a reaction bottle, and magnetic stirring was performed at room temperature for 10 minutes until the product was a viscous liquid, and dibutylamine was added dropwise under stirring, and the reaction process was observed until the product changed from a viscous liquid to a granular solid, and vacuum dried for 3 hours. The obtained white powder was ALA-T, and the yield was 74.23% to 92.65%;

[0008] Step 2, weighing four vapor phase corrosion inhibitor components of BCAU, thiourea, SDBS and ALA-T respectively in a mass ratio of 10-30:20-40:3-10:1-3;

[0009] Step 3, dissolving the BCAU, thiourea, SDBS and ALA-T weighed in step 2 with 1 / 4 volume of distilled water respectively, stirring evenly, to obtain the desired BCAU solution, thiourea solution, SDBS solution and ALA-T solution respectively;

[0010] Step 4: The BCAU solution, thiourea solution, SDBS solution and ALA-T solution obtained in step 3 are allowed to stand for 10 minutes respectively, and then the four solutions are mixed and stirred evenly.

[0011] The stirring time of BCAU, thiourea, SDBS and ALA-T solutions in step 1 is 5 to 10 minutes; the mixing temperature of BCAU solution in step 2 is 50° C., and the concentrations of BCAU solution, thiourea solution, SDBS solution and ALA-T solution are preferably 8 g / L, 12 g / L, 2 g / L and 0.8 g / L; the temperature of the four solutions in step 3 for mixing and stirring evenly is 50° C.

[0012] The third object of the present invention is to provide an application of an amino acid-based composite vapor-phase corrosion inhibitor, characterized in that the application comprises the following steps: placing a neutral base paper in the composite vapor-phase corrosion inhibitor mixed aqueous solution according to claim 1, immersing it at 55 to 120°C for 1 to 10 minutes, and then taking it out and drying it; the loading amount of the vapor-phase anti-rust paper surface corrosion inhibitor is 15 to 30 g / m 2 .

[0013] The composite gas phase corrosion inhibitor for carbon steel provided by the present invention is prepared by uniformly mixing BCAU, thiourea, SDBS and ALA-T. Taking advantage of the good volatility and green environmental protection of ALA-T, it is used as a gas phase corrosion inhibitor component for carbon steel for the first time, and is combined with the other three components to obtain a composite gas phase corrosion inhibitor. The molecular structure of the VCI component has multiple metal atom adsorption centers such as N, O, and S, and each component is firmly adsorbed on the metal surface through synergistic action. Among them, the hydrophilic group of SDBS adsorbs the metal surface, and the hydrophobic end is arranged on the metal surface; on the other hand, ALA-T with good volatility can be quickly volatilized to the metal surface, and the lone pair of electrons in its carboxyl and amino groups is combined with the metal; each component forms a hydrophobic film on the metal surface through synergistic action, making it difficult to form an electrolyte film on its surface, hindering the erosion and diffusion of corrosive ions, and reducing the ability of the metal electrochemical reaction and the risk of electrochemical corrosion. The corrosion inhibition rate of the rust-proof paper made of the composite gas phase corrosion inhibitor for carbon steel reaches 95.52%. The invention provides an effective vapor phase corrosion inhibitor for carbon steel material, which has the advantages of high corrosion inhibition efficiency, low toxicity, easy availability, uniform and stable volatilization and good corrosion inhibition performance. Description of the drawings:

[0014] Figure 1 The carbon steel samples were prepared without adding VCI and with adding the corresponding ternary composite VCI (m BCAU :m 硫脲 :m SDBS =2:3:0.5), add the corresponding quaternary composite VCI (m BCAU :m 硫脲 :m SDBS :m ALA-T =2:3:0.5:0.2) in an electrolyte with a potential polarization curve (A) and an electrochemical impedance spectrum (B).

[0015] Figure 2 The results of seven cycles of gas phase identification experiment of carbon steel samples: A, B, and C are respectively without adding VCI, adding the ternary composite VCI corresponding to Example 1 (m BCAU :m 硫脲 :m SDBS =2:3:0.5), add the corresponding quaternary composite VCI (m BCAU :m 硫脲 :m SDBS:m ALA-T =2:3:0.5:0.2) corresponding optical photograph of carbon steel sample.

[0016] Figure 3 The base paper and the ternary composite VCI (m BCAU :m 硫脲 :m SDBS =2:3:0.5) made of rust-proof paper, Example 2 corresponding to the four-component compound VCI (m BCAU :m 硫脲 :m SDBS :m ALA-T =2:3:0.5:0.2) after steel contact angle protection by anti-rust paper.

[0017] Figure 4 The results of the 75-cycle gas phase identification experiment of carbon steel samples are shown in Figure 1. A, B, and C are respectively the results of the gas phase identification experiment of carbon steel samples without adding VCI and adding the ternary composite VCI corresponding to Example 1 (m BCAU :m 硫脲 :m SDBS =2:3:0.5), add the corresponding quaternary composite VCI (m BCAU :m 硫脲 :m SDBS :m ALA-T =2:3:0.5:0.2) corresponding optical photograph of carbon steel sample.

[0018] Figure 5 SEM images of carbon steel surfaces protected by carbon steel sample base paper (A), ternary vapor phase anti-rust paper (B) and quaternary vapor phase anti-rust paper (C). Specific implementation method:

[0019] The present invention is described below with reference to specific examples. It will be appreciated by those skilled in the art that these examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention in any way.

[0020] Embodiment 1:

[0021] In this example, the corrosion inhibition efficiency obtained by volatilization reduction experiment, electrochemical impedance and dynamic potential polarization curve calculation was determined, and three factors of BCAU, thiourea and SDBS were determined, represented by A, B and C respectively; three levels of each factor were determined; and an orthogonal comparison experimental table of three factors and three levels was established. The details are as follows:

[0022]

[0023] 1) Closed space reduction and volatilization experiment

[0024] Experimental method: Weigh 2g of the drug, spread it evenly on a watch glass, and heat it continuously at a constant temperature of 50℃ in an oven for 72 hours. Weigh it every 24 hours and calculate the weight loss rate. The measurement results are shown in Table 1.

[0025] Table 1 Comparison of closed space volatilization reduction test results

[0026]

[0027] From the results in Table 1, it can be seen that the volatility of ALA-T is relatively high. After 24 hours, the mass volatility reaches 2.43%, 2.95% after 48 hours, and 3.36% after 72 hours. It can evaporate to the metal surface in a short time, adsorb to form a film, and play a protective role. The volatility of BCAU and thiourea is relatively weak, which can effectively prolong the release period of the compound corrosion inhibitor.

[0028] 2) Gas phase identification experiment

[0029] Experimental method: The experiment adopts the test tube solution method. 40mL of ionized water is used to prepare corrosion inhibitor solutions of different concentrations, which are poured into the bottom of a clean glass test tube with a specification of Φ30mm×20cm. The polished carbon steel sample is hung on it and plugged with a rubber stopper. The test tube is placed in a test tube rack and then put into a 50°C oven. Each cycle is heated for 8 hours and naturally cooled for 16 hours, and this cycle is repeated for seven cycles. After the experiment, it is evaluated by qualitative visual inspection and weight loss method. The mass changes of the metal samples before the experiment and after the pickling solution removes the rust are recorded, and the corrosion inhibition efficiency (IE) is calculated.

[0030] The corrosion inhibition efficiency is calculated according to the formula:

[0031] Where: Δm0 is the mass change (g) of the metal matrix without VCI after seven cycles of experiment; Δm is the mass change (g) of the metal matrix with VCI after seven cycles.

[0032] Table 2 Comparison of gas phase identification experimental results

[0033]

[0034] The IE obtained by calculating the corrosion inhibition efficiency of different formulas by the gas phase identification experiment weight loss method is used as the response. The K value can be obtained by performing range analysis on the data obtained by the weight loss method. After determining the optimal level, the optimal combination can be determined to be A2B2C1, that is, the optimal ratio is m BCAU :m 硫脲 :m SDBS =2:3:0.5.

[0035] Embodiment 2:

[0036] Preparation of ALA-T: Using a solvent-free method, 5 g of L-alanine and 8.5 mL of phosphoric acid were added to a reaction bottle, and magnetic stirring was performed at room temperature for 10 minutes until the product was a viscous liquid. Dibutylamine was added dropwise under stirring conditions, and the reaction process was observed until the product changed from a viscous liquid to a granular solid. The product was vacuum dried for 3 hours, and the obtained white powder was ALA-T with a yield of 87.46%;

[0037] In this example, electrochemical impedance spectroscopy, potentiodynamic polarization curve and gas phase identification experiments were performed on the experimental group containing ALA-T, the experimental group without ALA-T and the blank control experiment. The mass ratio of each component in the ALA-T group is: m BCAU :m 硫脲 :m SDBS :m ALA-T =2:3:0.5:0.2, the mass ratio of each component in the group without ALA-T is: m BCAU :m 硫脲 :m SDBS =2:3:0.5.

[0038] 1) Electrochemical experiments

[0039] Experimental method: A three-electrode system was used: the reference electrode was a saturated calomel electrode, the counter electrode was a carbon rod, and the working electrode was a homemade 45# steel electrode. Sodium sulfate solution (ω=7.1%) with or without different VCI was used as the electrolyte solution, in which BCAU needed to be dissolved in a small amount of ethanol. Potentiodynamic polarization curves and electrochemical impedance were tested respectively.

[0040] The corrosion inhibition efficiency is calculated according to the formula:

[0041]

[0042] Figure 1 The carbon steel samples were prepared without adding VCI and with adding the corresponding ternary composite VCI (m BCAU :m 硫脲 :m SDBS =2:3:0.5), add the corresponding quaternary composite VCI (m BCAU :m 硫脲 :m SDBS :m ALA-T=2:3:0.5:0.2) in the electrolyte. The corresponding electrochemical parameters calculated according to the test curve are listed in Table 3. It can be seen that compared with the blank, the addition of the compound VCI promotes the positive shift of the corrosion potential and reduces the corrosion current density; the polarization resistance increases, inhibits the electrochemical corrosion reaction, and improves the corrosion resistance. The corrosion inhibition efficiency of the two experimental tests corresponding to the quaternary compound VCI containing ALA-T has increased significantly. Specifically, after adding ALA-T, the corrosion inhibition efficiency of the quaternary compound VCI increased from 55.79% and 84.87% of the ternary compound VCI to 83.55% and 87.93%, respectively.

[0043] Table 3 Electrochemical parameters

[0044]

[0045] 2) Gas phase identification experiment

[0046] Experimental method: Same as the gas phase identification experiment in Example 1.

[0047] Table 4 Corrosion inhibition efficiency calculated from weight loss in gas phase identification experiment

[0048]

[0049] The results in Table 4 show that compared with the ternary composite VCI without ALA-T, the quaternary composite VCI containing ALA-T can achieve higher corrosion inhibition efficiency.

[0050] Figure 2 The results of seven cycles of gas phase identification experiment of carbon steel samples are shown in Figure 1. A, B, and C are respectively without adding VCI, adding the corresponding ternary composite VCI of Example 1 (m BCAU :m 硫脲 :m SDBS =2:3:0.5), add the corresponding quaternary composite VCI (m BCAU :m 硫脲 :m SDBS :m ALA-T =2:3:0.5:0.2) of carbon steel samples. It can be seen that: compared with the blank group, the metal samples protected by the ternary compound VCI without ALA-T have significantly less rust, but there is still a problem of insufficient protection in the early stage. However, after adding a small amount of ALA-T, the metal samples of the quaternary compound VCI containing ALA-T are almost free of rust and can provide effective protection in the early stage of corrosion.

[0051] Embodiment 3:

[0052] This example uses the ternary composite VCI (m BCAU :m 硫脲:m SDBS =2:3:0.5) made of rust-proof paper, the quaternary composite VCI (m BCAU :m 硫脲 :m SDBS :m ALA-T =2:3:0.5:0.2) and carbon steel metal samples protected by blank base paper were used as experimental objects for contact angle test and vapor phase corrosion inhibition test. Vapor phase anti-rust paper containing / not containing ALA-T was prepared by impregnation method. The mass concentration of total vapor phase rust inhibitor in the impregnation solution was 40g / L, and the mass ratio of corrosion inhibitor containing ALA-T group in the same solvent was as follows: m BCAU :m 硫脲 :m SDBS :m ALA-T =2:3:0.5:0.2, excluding ALA-T group m BCAU :m 硫脲 :m SDBS =2:3:0.5.

[0053] 1) Contact angle test

[0054] Experimental method: Vapor-phase anti-rust paper containing / not containing ALA-T was prepared by the impregnation method. This example determines the corrosion inhibition performance of the above composite vapor-phase corrosion-inhibiting paper, which is described in detail as follows. First, the metal sample is polished to 2000# with sandpaper step by step, then washed with deionized water, degreased with alcohol, and dried with cold air. In a closed environment at 50°C, the samples were wrapped with base paper, ternary composite vapor-phase anti-rust paper without ALA-T, and quaternary composite vapor-phase anti-rust paper containing ALA-T for 72 hours. The contact angle was measured using a contact angle tester to study the difference in contact angles.

[0055] Table 5 Contact angle test results of metal surfaces of metal samples pre-coated with vapor phase anti-rust paper

[0056]

[0057] Figure 3 The base paper and the ternary composite VCI (m BCAU :m 硫脲 :m SDBS =2:3:0.5) made of rust-proof paper, the quaternary composite VCI (m BCAU :m 硫脲 :m SDBS :m ALA-T=2:3:0.5:0.2) after the steel contact angle test results after the anti-rust paper made. It can be seen that the contact angle of the metal sample in contact with the base paper is 83.6°, the contact angle of the metal sample protected by the ternary composite VCI anti-rust paper without ALA-T increases to 97.1°, and the contact angle of the metal sample protected by the quaternary composite VCI anti-rust paper containing ALA-T increases to 102.0°. The relevant data are listed in Table 5. The contact angle results show that: the VCI components of each component successfully volatilize to the metal surface to form a protective film. The introduction of ALA-T enhances the synergistic effect of the composite VCI and improves the uniform adhesion of each component on the metal surface, thereby improving the hydrophobicity of the VCI composite film, presenting a larger contact angle, making it difficult to form an electrolyte film on its surface, hindering the erosion and diffusion of corrosive ions, and reducing the ability of the metal electrochemical reaction and the risk of electrochemical corrosion.

[0058] 2) Long-term gas phase identification experiment

[0059] Experimental method: Same as the gas phase identification experiment in Example 1

[0060] Table 6 Evaluation results of gas phase corrosion inhibition ability of ternary / quaternary composite gas phase anti-rust paper without / with ALA-T (15 cycles)

[0061]

[0062] Note: ○ indicates no corrosion and the surface is bright and shiny; ◎ indicates slight corrosion and rust can be observed on the metal surface; ● indicates severe corrosion and a large amount of corrosion products on the surface

[0063] It can be seen from Table 6 that the carbon steel metal protected by the base paper corroded on the second day, and corrosion products were visible on the surface. A large amount of rust appeared on the surface on the sixth day, and the rust was serious. The carbon steel sample protected by the anti-rust paper prepared by the ternary composite VCI without ALA-T was observed to be slightly corroded on the 10th day. The carbon steel sample protected by the anti-rust paper prepared by the quaternary composite VCI containing ALA-T was not observed to have trace corrosion products until the 15th day.

[0064] Figure 4 The results of the 75-cycle gas phase identification experiment of carbon steel samples are shown in Figure 1. A, B, and C are respectively the results of the gas phase identification experiment of carbon steel samples without adding VCI and adding the ternary composite VCI corresponding to Example 1 (m BCAU :m 硫脲 :m SDBS =2:3:0.5), add the corresponding quaternary composite VCI (m BCAU :m 硫脲 :m SDBS :m ALA-T=2:3:0.5:0.2) corresponding to the optical photograph of the carbon steel sample. It can be seen that after the 75th cycle of the gas phase identification experiment, the surface of the carbon steel protected by the anti-rust paper prepared by the quaternary composite VCI containing ALA-T is still full of luster, and there is almost no rust, while the surface of the carbon steel protected by the anti-rust paper prepared by the ternary composite VCI without ALA-T has obvious small rust spots. The experimental results show that the addition of the fourth VCI component ALA-T effectively inhibits the early corrosion of the metal and greatly reduces the entire corrosion process of the metal.

[0065] Figure 5 The SEM images of the carbon steel surface protected by base paper (A), ternary VCI paper (B) and quaternary VCI paper (C) are shown in Figure 1. As can be seen from the figure, the surface of 45# steel protected by base paper has crisscross cracks, a large number of corrosion pits, and obvious gullies and cracks; although there are no corrosion pits on the surface of 45# steel protected by ternary VCI paper, there are still obvious gullies and cracks, indicating that ternary VCI paper has a certain degree of VCI effect; while the surface of 45# steel protected by quaternary VCI paper can only see the sandpaper texture during grinding, without obvious cracks or rust accumulation, and the corrosion resistance is significantly improved, indicating that the addition of ALA-T greatly improves the VCI performance of quaternary VCI paper.

Claims

1. An amino acid-based composite vapor phase corrosion inhibitor, characterized in that: The method is prepared by preparing a mixed aqueous solution of dicyclohexylamine methyl urea, thiourea, sodium dodecylbenzene sulfonate and alanine ternary complex, wherein the mass ratio of dicyclohexylamine methyl urea: thiourea: sodium dodecylbenzene sulfonate: alanine ternary complex is 10-30: 20-40: 3-10: 1-3; wherein dicyclohexylamine methyl urea is denoted as BCAU, sodium dodecylbenzene sulfonate is denoted as SDBS, and alanine ternary complex is denoted as ALA-T; The preparation method of the composite gas phase corrosion inhibitor comprises the following steps: Step 1, preparation of ALA-T by solvent-free method: 2-8 g of L-alanine and 4-10 mL of phosphoric acid were added to a reaction bottle, and magnetic stirring was performed at room temperature for 10 minutes until the product was a viscous liquid, and dibutylamine was added dropwise under stirring, and the reaction process was observed until the product changed from a viscous liquid to a granular solid, and vacuum dried for 3 hours. The obtained white powder was ALA-T, and the yield was 74.23% to 92.65%; Step 2, weighing four vapor phase corrosion inhibitor components of BCAU, thiourea, SDBS and ALA-T respectively in a mass ratio of 10-30:20-40:3-10:1-3; Step 3, dissolving the BCAU, thiourea, SDBS and ALA-T weighed in step 2 with 1 / 4 volume of distilled water respectively, stirring evenly, to obtain the desired BCAU solution, thiourea solution, SDBS solution and ALA-T solution respectively; Step 4: The BCAU solution, thiourea solution, SDBS solution and ALA-T solution obtained in step 3 are allowed to stand for 10 minutes respectively, and then the four solutions are mixed and stirred evenly. The stirring time of BCAU, thiourea, SDBS and ALA-T solutions in step 1 is 5 to 10 minutes; the mixing temperature of BCAU solution in step 2 is 50° C., and the concentrations of BCAU solution, thiourea solution, SDBS solution and ALA-T solution are preferably 8 g / L, 12 g / L, 2 g / L and 0.8 g / L; the temperature of the four solutions in step 3 for mixing and stirring evenly is 50° C.

2. The use of the amino acid-based composite vapor phase corrosion inhibitor according to claim 1, characterized in that The application comprises the following steps: placing neutral base paper in the mixed aqueous solution of the composite vapor phase corrosion inhibitor according to claim 1, immersing for 1-10 minutes at 55-120°C, and then taking out and drying; the loading amount of the vapor phase anti-rust paper surface corrosion inhibitor is 15-30g / m 2 .