Electrolyte, lithium ion battery and formation method of lithium ion battery
By using specific formula electrolytes in lithium-ion batteries, including vinyl carbonate, vinyl sulfite and antioxidant additives, and using overcharge formation processes, the lithium-ion battery is solved between high cycle life and magnification discharge performance. The contradiction significantly improves the battery's cycle performance and storage capacity.
Patent Information
- Application Number
- CN202411137803.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-01
AI Technical Summary
There is a contradiction between the high cycle life and the magnification discharge performance of existing lithium-ion batteries. The excessive addition of vinylene carbonate will lead to lithium extraction problems, affecting the film-forming structure of the electrolyte on the surface of the electrode material and the battery performance.
Using an electrolyte formulation, including vinyl carbonate, vinyl sulfite and antioxidant additives, the addition of vinyl carbonate is 5-15%, the addition of vinyl sulfite is 1.5-5%, and the antioxidant The additive is added in 0.01-1%, and the battery impedance is reduced by the overcharge process, and a combination of vinyl carbonate and vinyl sulfite are used to reduce the electrolyte impedance.
It significantly reduces the DC internal resistance of lithium-ion batteries, improves the cycling performance and rate discharge performance of the battery, extends the cycle life of the battery, and avoids the electrolyte decomposition problem caused by high vinyl carbonate.
Smart Images

Figure BDA0004999903800000021 
Figure BDA0004999903800000051 
Figure BDA0004999903800000052
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to an electrolyte, a lithium ion battery and a formation method thereof. Background Art
[0002] Compared with other chemical energy storage devices, lithium-ion batteries have advantages such as higher energy density, longer cycle life, and no memory effect. Therefore, they are widely used in mobile phones, laptops, fuel vehicles, new energy vehicles, and industrial energy storage. With the increasing demand for long-life lithium-ion batteries in the energy storage industry, the development of lithium-ion batteries with longer cycle life has become a top priority in battery research and development projects, among which the optimization of electrolyte has become one of the core issues to improve battery cycle life.
[0003] One of the ways to increase the life of energy storage batteries is to continuously increase the amount of additives added. Once the amount of additives added reaches the limit, continuing to add will worsen the cycle due to high impedance lithium precipitation. At present, the most obvious additive to improve the cycle is vinylene carbonate. When the amount of vinylene carbonate added exceeds 4%, it is easy to cause lithium precipitation problems. Therefore, the amount of vinylene carbonate added to the electrolyte does not exceed 5%. From the perspective of electrolyte design, low impedance and long cycle life often have contradictions. Excessive additives will affect the film formation structure and degree of the electrolyte on the surface of the electrode material, which may affect the rate discharge performance of lithium-ion batteries. Therefore, the need to develop electrolytes with high cycle life and rate discharge performance is of great significance to the application and development of lithium-ion batteries. Summary of the invention
[0004] The object of the present invention is to provide an electrolyte with a long cycle life and a good rate discharge performance; another object of the present invention is to provide a lithium ion battery with a long cycle life and a good rate discharge performance; another object of the present invention is to provide a formation method of a lithium ion battery with a long cycle life and a good rate discharge performance.
[0005] The invention discloses an electrolyte, comprising lithium salt, additives and solvents, wherein the additives comprise vinylene carbonate and vinyl sulfite; the amount of vinylene carbonate added accounts for 5-15% of the total mass of the electrolyte, and the amount of vinyl sulfite added accounts for 1.5-5% of the total mass of the electrolyte.
[0006] The lithium salt is selected from one or more of lithium hexafluorophosphate, lithium bis(trifluorosulfonyl imide), lithium bis(oxalatoborate), lithium tetrafluoroborate, lithium difluorooxalatoborate, lithium difluorophosphate, lithium bis(trifluoromethanesulfonyl imide), lithium perchlorate, and lithium hexafluoroarsenate.
[0007] The solvent is selected from one or more of dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, ethylene carbonate, propylene carbonate, methyl acetate, ethyl acetate, ethyl propionate, propyl propionate, methyl propionate, fluorobenzene, xylene, toluene, fluoroethylene carbonate, ethyl methyl carbonate, fluorodimethyl carbonate, fluorodiethyl carbonate, trimethyl phosphate, tetrahydrofuran, acetonitrile, sulfolane, dimethyl sulfoxide, 1,2-dimethoxyethane, and vinyl sulfite.
[0008] Furthermore, the solvent is selected from one or more of ethylene carbonate (EC), propylene carbonate (PC), dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), dipropyl carbonate (DPC), ethyl acetate (EA), methyl acetate (MA), ethyl propionate (EP), and propyl propionate (PP).
[0009] Furthermore, the additives also include antioxidant additives, whose chemical structure is as shown in formula (I):
[0010]
[0011] Wherein, R1 is selected from one of hydrogen, halogen, substituted or unsubstituted alkane group, alkene group, alkyne group, aromatic group, phosphate group, sulfonate group, sulfate group, borate group, siloxy group, sulfite group, heterocyclic group and isocyanate group.
[0012] Furthermore, in the chemical structure of the antioxidant additive, R1 is selected from one of acryl, trimethylsilyl and phenyl.
[0013] Furthermore, the amount of the antioxidant additive added is 0.01-1% of the total mass of the electrolyte.
[0014] Furthermore, the amount of vinylene carbonate added is 7-8% of the total mass of the electrolyte, the amount of vinyl sulfite added is 2-3% of the total mass of the electrolyte; and the amount of antioxidant additive added is 0.01-0.5% of the total mass of the electrolyte.
[0015] Furthermore, the amount of vinylene carbonate added is 5-10% of the total mass of the electrolyte, the amount of vinyl sulfite added is 1.5-3.5% of the total mass of the electrolyte; and the amount of the antioxidant additive added is 0.01-0.2% of the total mass of the electrolyte.
[0016] Furthermore, the additives also include vinyl sulfate and / or tris(trimethyl)silyl phosphoric acid; the amount of vinyl sulfate and / or tris(trimethyl)silyl phosphoric acid added accounts for 0.1-1% of the total mass of the electrolyte.
[0017] The present invention also provides a lithium ion battery, comprising a positive electrode, a negative electrode, a separator and the electrolyte as described above.
[0018] The active material of the positive electrode is selected from one or more of lithium iron manganese phosphate and lithium iron manganese phosphate.
[0019] The active material of the negative electrode is selected from one or both of natural graphite and artificial graphite.
[0020] The diaphragm is selected from one of polypropylene diaphragm (PP), polyethylene diaphragm (PE), polyethylene / polypropylene double-layer composite membrane, polyimide electrospinning diaphragm (PI), polypropylene / polyethylene / polypropylene three-layer composite diaphragm (PP / PE / PP), ceramic diaphragm, and PVDF coated diaphragm.
[0021] The present invention also discloses a formation method of a lithium ion battery, comprising the following steps:
[0022] S1: pre-charging the lithium-ion battery as described above for the first time;
[0023] S2: first aging, vacuum pumping;
[0024] S3: Second pre-charge and discharge;
[0025] S4: second aging;
[0026] S5: Overcharge formation, charging the lithium-ion battery to 1.05-1.15 times of the conventional cut-off voltage with a charging current of 1-0.01C.
[0027] The cut-off voltage of a lithium-ion battery with lithium iron phosphate as the positive electrode during the formation process is 3.65V; the cut-off voltage of a lithium-ion battery with lithium manganese iron phosphate as the positive electrode during the formation process is 4.35V.
[0028] Overcharge formation further reduces the impedance of lithium-ion batteries. The principle of overcharge formation to reduce the impedance of lithium-ion batteries is that after the battery cell is charged to a higher voltage, the lithium ion content of the positive electrode material will be further released, the vacancies in the positive electrode material will increase, and the migration resistance of lithium ions in the positive electrode material will be reduced. The polarization degree of the interface is reduced, thereby significantly reducing the impedance of the lithium-ion battery.
[0029] Overcharge formation will have a negative impact on the electrolyte, causing the electrolyte to decompose on the positive electrode surface and deteriorate the electrolyte performance. To solve this problem, the present invention adds an antioxidant additive to the electrolyte. The antioxidant additive is mainly composed of phosphites. Since phosphites are easy to lose electrons, the phosphite ion is first oxidized at the positive electrode interface during overcharge formation, thereby protecting the interface and the electrolyte. By combining the use of vinylene carbonate, vinyl sulfite, antioxidant additives and a new process of overcharge formation, the DC internal resistance of lithium-ion batteries is significantly reduced and the cycle performance of lithium-ion batteries is improved.
[0030] Furthermore, the first pre-charging operation is to first charge to 10% SOC with a constant current of 0.01C, and then charge to 30% SOC with a constant current of 0.02C.
[0031] Furthermore, the first aging operation is aging at 45° C. for 48 hours and vacuum pumping.
[0032] Furthermore, the second pre-charging operation is to charge to 100% SOC at a constant current of 0.1C.
[0033] Furthermore, the overcharge operation is to charge with a current of 0.5C to 1.06-1.12 times of the cut-off current; then charge with a current of 0.1C to 1.06-1.12 times of the cut-off current; and then charge with a current of 0.02C to 1.06-1.12 times of the cut-off current.
[0034] Furthermore, the overcharge operation is to charge with a current of 0.1C to 1.08-1.1 times of the cut-off current; then charge with a current of 0.02C to 1.06-1.12 times of the cut-off current; then charge with a current of 0.02C to 1.06-1.12 times of the cut-off current.
[0035] The electrolyte disclosed in the present invention combines vinyl carbonate and vinyl sulfite, which can significantly reduce the problem of excessive electrolyte impedance caused by high concentration of vinyl carbonate. This is because vinyl sulfite obtains an electron during the formation process and is converted into vinyl sulfite radical anion, which then undergoes nucleophilic attack with multiple vinyl carbonates to generate polyvinyl carbonate-based vinyl sulfite compounds. The compound has a sulfite group, which has a weaker ability to bind to lithium ions than carbonate functional groups. Lithium ions with weaker binding force to organic matter in the SEI membrane are more likely to bind to vinyl carbonate in the solvation shell, thereby making the solvation shell of the lithium ions easier to peel off, reducing the migration resistance of lithium ions in the SEI membrane, thereby reducing the impedance of the electrolyte. DETAILED DESCRIPTION
[0036] In order to make the technical solution of the present invention clearer, the present invention is further described in detail below in conjunction with specific embodiments.
[0037] The positive electrode sheets of the lithium-ion batteries in the embodiments of the present invention and the comparative examples all use lithium iron phosphate as the positive electrode active material, and the positive electrode active material, conductive carbon black and binder polyvinylidene fluoride (PVDF) are mixed in a mass ratio of 95.5:2:2.5. Specifically, lithium iron phosphate, conductive carbon black and PVDF are first dispersed in an appropriate amount of N-methylpyrrolidone, and then stirred thoroughly according to the homogenization process. The uniformly dispersed positive electrode slurry is evenly coated on aluminum foil, and the positive electrode sheet is obtained by baking, rolling, slitting and punching.
[0038] The specific production process of the negative electrode sheet is to select artificial graphite as the negative electrode active material, put it into a slurry tank with a mass ratio of 96:1:2:1 with conductive carbon black, styrene-butadiene rubber (SBR), and sodium carboxymethyl cellulose (CMC), and make a uniformly dispersed negative electrode slurry according to the slurry making process. Then the negative electrode slurry is evenly coated on the copper foil, and after baking, rolling, slitting, and punching, the negative electrode sheet is obtained.
[0039] After the positive and negative electrodes are punched, the positive electrode is placed in an oven at 110-140°C and the negative electrode is placed in an oven at 90-100°C for 20-30 hours. Using polyethylene diaphragm (PE) as the diaphragm, when the moisture content of the electrode meets the requirements, the positive electrode, negative electrode and diaphragm are placed in a laminating machine to form a bare cell, and then the bare cell is encapsulated in a stamped aluminum-plastic film bag.
[0040] After the packaged dry cell is dried at 80-95°C for 8-15h, the electrolyte prepared in the embodiments of the present invention and the comparative examples is injected into the dry cell, and the cells are placed aside, formed, and divided. The present invention mainly divides the cells by charging to 3.65V at 0.1C constant current and constant voltage, and discharging to 2.5V at 0.1C constant current and constant voltage.
[0041] The antioxidant additive is synthesized from R1-OH, m-diphenol, phenol and phosphorus trichloride, wherein R1 is one of propenyl, trimethylsilyl and phenyl. The specific synthesis steps are as follows:
[0042]
[0043] The obtained product structure is as follows:
[0044]
[0045]
[0046] Example 1
[0047] Preparation of electrolyte: Control the moisture content in the glove box to be less than 10ppm, and control the moisture content of the solvent to be less than 10ppm. Use a percentile balance to accurately weigh 60g of ethylene carbonate and 140g of ethyl methyl carbonate, and pour them into an aluminum bottle. After fully stirring, put it in a 0℃ constant temperature box and freeze it for 1h. Then add 30g of lithium hexafluorophosphate while stirring. Finally, add 12.4g of vinylene carbonate, 3.72g of vinyl sulfite, 1.24g of vinyl sulfate, and 0.74g of tris(trimethyl)silyl phosphate, respectively, and stir evenly. Control the content of vinylene carbonate to 5% and the content of vinyl sulfite to 1.5%.
[0048] Inject the electrolyte into the packaged dry cell, and then soak it in a 25°C environment for 48 hours. After the electrolyte fully soaks the dry cell, start pre-charging, formation and capacity division. The pre-charging step is to charge to 10% SOC at a constant current of 0.01C, and then change to a constant current of 0.02C to charge to 30% SOC. After pre-charging, age at 45°C for 48 hours, and then vacuum evacuate. After aging, charge to 100% SOC at a constant current of 0.1C, stand for 10 minutes, and then discharge to 2.5V to determine the first charge and discharge efficiency. Next, continue aging at 45°C for 24 hours. After aging, perform capacity division.
[0049] Example 2
[0050] Preparation of electrolyte: Control the moisture content in the glove box to be less than 10ppm, and control the moisture content of the solvent to be less than 10ppm. Use a percentile balance to accurately weigh 60 grams of ethylene carbonate and 140 grams of ethyl methyl carbonate, and pour them into an aluminum bottle. After fully stirring, put it in a 0℃ constant temperature box and freeze it for 1 hour. Then add 30 grams of lithium hexafluorophosphate while stirring. Finally, add 17.98 grams of vinyl carbonate, 6.41 grams of vinyl sulfite, 1.28 grams of vinyl sulfate, and 0.77 grams of tris(trimethyl)silyl phosphate, respectively, and stir evenly. Control the content of vinyl carbonate to 7% and the content of vinyl sulfite to 2.5%.
[0051] The electrolyte is injected into the lithium-ion dry battery for energy storage, and then immersed in an environment of 25°C for 48 hours. After the electrolyte fully infiltrates the battery, pre-charging, formation and capacity division are started. The pre-charging process is to charge to 10% SOC at a constant current of 0.01C, and then change to a constant current of 0.02C to charge to 30% SOC. After pre-charging, age for 48 hours at 45°C, and then vacuum evacuate. After aging, charge to 100% SOC at a constant current of 0.1C, stand for 10 minutes, and then discharge to 2.5V to determine the first charge and discharge efficiency. Next, continue aging at 45°C for 24 hours. After aging is completed, capacity division is performed.
[0052] Example 3
[0053] Preparation of electrolyte: Control the moisture content in the glove box to be less than 10ppm, and control the moisture content of the solvent to be less than 10ppm. Use a percentile balance to accurately weigh 60 grams of ethylene carbonate and 140 grams of ethyl methyl carbonate, and pour them into an aluminum bottle. After fully stirring, put it in a constant temperature box at 0℃ and freeze it for 1h. Then add 30 grams of lithium hexafluorophosphate while stirring. Finally, add 23.88 grams of vinyl carbonate, 9.28 grams of vinyl sulfite, 1.33 grams of vinyl sulfate, and 0.80 grams of tris(trimethyl)silyl phosphate, respectively, and stir evenly. Control the content of vinyl carbonate to 9% and the content of vinyl sulfite to 3.5%.
[0054] The electrolyte is injected into the lithium-ion dry battery for energy storage, and then immersed in an environment of 25°C for 48 hours. After the electrolyte fully infiltrates the battery, pre-charging, formation and capacity division are started. The pre-charging process is to charge to 10% SOC at a constant current of 0.01C, and then change to a constant current of 0.02C to charge to 30% SOC. After pre-charging, age for 48 hours at 45°C, and then vacuum evacuate. After aging, charge to 100% SOC at a constant current of 0.1C, stand for 10 minutes, and then discharge to 2.5V to determine the first charge and discharge efficiency. Next, continue aging at 45°C for 24 hours. After aging is completed, capacity division is performed.
[0055] Example 4
[0056] Preparation of electrolyte: Control the moisture content in the glove box to be less than 10ppm, and control the moisture content of the solvent to be less than 10ppm. Use a percentile balance to accurately weigh 60 grams of ethylene carbonate and 140 grams of ethyl methyl carbonate, and pour them into an aluminum bottle. After fully stirring, put it in a 0℃ constant temperature box and freeze it for 1 hour. Then add 30 grams of lithium hexafluorophosphate while stirring. Finally, add 17.98 grams of vinyl carbonate, 6.41 grams of vinyl sulfite, 1.28 grams of vinyl sulfate, and 0.77 grams of tris(trimethyl)silyl phosphate, respectively, and stir evenly. Control the content of vinyl carbonate to 7% and the content of vinyl sulfite to 2.5%.
[0057] The electrolyte is injected into the lithium-ion dry battery for energy storage, and then placed in an environment of 25°C for 48 hours. After the electrolyte fully infiltrates the battery, pre-charge formation and capacity division are started. The pre-charge process is to charge to 10% SOC at a constant current of 0.01C, and then change to 0.02C constant current to charge to 30% SOC. After pre-charge, age for 48 hours at 45°C, and then vacuum evacuate. After aging, charge to 100% SOC at a constant current of 0.1C, stand for 10 minutes, and then discharge to 2.5V to determine the first charge and discharge efficiency. Next, continue aging at 45°C for 24 hours. After aging, start overcharge formation. The steps of overcharge formation are to first charge to 3.8V at a constant current of 0.5C, then charge to 3.8V at a constant current of 0.1C, and finally charge to 3.8V at a constant current of 0.02C. After completing overcharge formation, finally perform capacity division.
[0058] Example 5
[0059] The electrolyte in this embodiment is prepared by the following steps: control the moisture content in the glove box to be less than 10ppm, and control the moisture content of the solvent to be less than 10ppm. Use a percentile balance to accurately weigh 60 grams of ethylene carbonate and 140 grams of ethyl methyl carbonate, and pour them into an aluminum bottle. After fully stirring, put it in a constant temperature box at 0°C and freeze for 1 hour. Then add 30 grams of lithium hexafluorophosphate while stirring. Finally, add 17.98 grams of vinylene carbonate, 6.41 grams of vinyl sulfite, 1.28 grams of vinyl sulfate, and 0.77 grams of tris(trimethyl)silyl phosphate, respectively, and stir evenly. Control the content of vinylene carbonate at 7% and the content of vinyl sulfite at 2.5%.
[0060] The electrolyte is injected into the lithium-ion dry battery for energy storage, and then placed in an environment of 25°C for 48 hours. After the electrolyte fully infiltrates the battery, pre-charge formation and capacity division are started. The pre-charge process is to charge to 10% SOC at a constant current of 0.01C, and then change to 0.02C constant current to charge to 30% SOC. After pre-charge, age for 48 hours at 45°C, and then vacuum evacuate. After aging, charge to 100% SOC at a constant current of 0.1C, stand for 10 minutes, and then discharge to 2.5V to determine the first charge and discharge efficiency. Next, continue aging at 45°C for 24 hours. After aging, start overcharge formation. The steps of overcharge formation are to first charge to 3.8V at a constant current of 0.1C, then charge to 3.8V at a constant current of 0.02C, and finally charge to 3.8V at a constant current of 0.01C. After completing overcharge formation, finally perform capacity division.
[0061] Example 6
[0062] Preparation of electrolyte: Control the moisture content in the glove box to be less than 10ppm, and control the moisture content of the solvent to be less than 10ppm. Use a percentile balance to accurately weigh 60 grams of ethylene carbonate and 140 grams of ethyl methyl carbonate, and pour them into an aluminum bottle. After fully stirring, put it in a 0℃ constant temperature box and freeze it for 1 hour. Then add 30 grams of lithium hexafluorophosphate while stirring. Finally, add 17.98 grams of vinyl carbonate, 6.41 grams of vinyl sulfite, 1.28 grams of vinyl sulfate, and 0.77 grams of tris(trimethyl)silyl phosphate, respectively, and stir evenly. Control the content of vinyl carbonate to 7% and the content of vinyl sulfite to 2.5%.
[0063] The electrolyte is injected into the lithium-ion dry battery for energy storage, and then placed in an environment of 25°C for 48 hours. After the electrolyte fully infiltrates the battery, pre-charge formation and capacity division are started. The pre-charge process is to charge to 10% SOC at a constant current of 0.01C, and then change to 0.02C constant current to charge to 30% SOC. After pre-charge, age for 48 hours at 45°C, and then vacuum. After aging, charge to 100% SOC at a constant current of 0.1C, stand for 10 minutes, and then discharge to 2.5V to determine the first charge and discharge efficiency. Next, continue aging at 45°C for 24 hours. After aging, start overcharge formation. The steps of overcharge formation are to first charge to 4.1V at a constant current of 0.1C, then charge to 4.1V at a constant current of 0.02C, and finally charge to 4.1V at a constant current of 0.01C. After completing overcharge formation, finally perform capacity division.
[0064] Example 7
[0065] Preparation of electrolyte: Control the moisture content in the glove box to be less than 10ppm, and control the moisture content of the solvent to be less than 10ppm. Use a percentile balance to accurately weigh 60g of ethylene carbonate and 140g of ethyl methyl carbonate, and pour them into an aluminum bottle. After fully stirring, put it in a constant temperature box at 0℃ and freeze for 1h. Then add 30g of lithium hexafluorophosphate while stirring. Finally, add 17.98g of vinyl carbonate, 6.41g of vinyl sulfite, 1.28g of vinyl sulfate, 0.77g of tris(trimethyl)silyl phosphate, and 0.077g of antioxidant additive (T1) respectively, and stir evenly. Control the content of vinyl carbonate at 7%, the content of vinyl sulfite at 2.5%, and the content of T1 at 0.03%.
[0066] The electrolyte is injected into the lithium-ion dry battery for energy storage, and then placed in an environment of 25°C for 48 hours. After the electrolyte fully infiltrates the battery, pre-charge formation and capacity division are started. The pre-charge process is to charge to 10% SOC at a constant current of 0.01C, and then change to 0.02C constant current to charge to 30% SOC. After pre-charge, age for 48 hours at 45°C, and then vacuum. After aging, charge to 100% SOC at a constant current of 0.1C, stand for 10 minutes, and then discharge to 2.5V to determine the first charge and discharge efficiency. Next, continue aging at 45°C for 24 hours. After aging, start overcharge formation. The steps of overcharge formation are to first charge to 4.1V at a constant current of 0.1C, then charge to 4.1V at a constant current of 0.02C, and finally charge to 4.1V at a constant current of 0.01C. After completing overcharge formation, finally perform capacity division.
[0067] Example 8
[0068] Preparation of electrolyte: Control the moisture content in the glove box to be less than 10ppm, and control the moisture content of the solvent to be less than 10ppm. Use a percentile balance to accurately weigh 60g of ethylene carbonate and 140g of ethyl methyl carbonate, and pour them into an aluminum bottle. After fully stirring, put it in a constant temperature box at 0℃ and freeze for 1h. Then add 30g of lithium hexafluorophosphate while stirring. Finally, add 17.98g of vinyl carbonate, 6.41g of vinyl sulfite, 1.28g of vinyl sulfate, 0.77g of tris(trimethyl)silyl phosphate, and 0.077g of antioxidant additive (T2) respectively, and stir evenly. Control the content of vinyl carbonate at 7%, the content of vinyl sulfite at 2.5%, and the content of T2 at 0.03%.
[0069] The electrolyte is injected into the lithium-ion dry battery for energy storage, and then placed in an environment of 25°C for 48 hours. After the electrolyte fully infiltrates the battery, pre-charge formation and capacity division are started. The pre-charge process is to charge to 10% SOC at a constant current of 0.01C, and then change to 0.02C constant current to charge to 30% SOC. After pre-charge, age for 48 hours at 45°C, and then vacuum. After aging, charge to 100% SOC at a constant current of 0.1C, stand for 10 minutes, and then discharge to 2.5V to determine the first charge and discharge efficiency. Next, continue aging at 45°C for 24 hours. After aging, start overcharge formation. The steps of overcharge formation are to first charge to 4.1V at a constant current of 0.1C, then charge to 4.1V at a constant current of 0.02C, and finally charge to 4.1V at a constant current of 0.01C. After completing overcharge formation, finally perform capacity division.
[0070] Example 9
[0071] Preparation of electrolyte: Control the moisture content in the glove box to be less than 10ppm, and control the moisture content of the solvent to be less than 10ppm. Use a percentile balance to accurately weigh 60g of ethylene carbonate and 140g of ethyl methyl carbonate, and pour them into an aluminum bottle. After fully stirring, put it in a constant temperature box at 0℃ and freeze it for 1h. Then add 30g of lithium hexafluorophosphate while stirring. Finally, add 17.98g of vinyl carbonate, 6.41g of vinyl sulfite, 1.28g of vinyl sulfate, 0.77g of tris(trimethyl)silyl phosphate, and 0.077g of antioxidant additive (T3) respectively, and stir evenly. Control the content of vinyl carbonate at 7%, the content of vinyl sulfite at 2.5%, and the content of T3 at 0.03%.
[0072] The electrolyte is injected into the lithium-ion dry battery for energy storage, and then placed in an environment of 25°C for 48 hours. After the electrolyte fully infiltrates the battery, pre-charge formation and capacity division are started. The pre-charge process is to charge to 10% SOC at a constant current of 0.01C, and then change to 0.02C constant current to charge to 30% SOC. After pre-charge, age for 48 hours at 45°C, and then vacuum. After aging, charge to 100% SOC at a constant current of 0.1C, stand for 10 minutes, and then discharge to 2.5V to determine the first charge and discharge efficiency. Next, continue aging at 45°C for 24 hours. After aging, start overcharge formation. The steps of overcharge formation are to first charge to 4.1V at a constant current of 0.1C, then charge to 4.1V at a constant current of 0.02C, and finally charge to 4.1V at a constant current of 0.01C. After completing overcharge formation, finally perform capacity division.
[0073] Comparative Example
[0074] Preparation of electrolyte: Control the moisture content in the glove box to be less than 10ppm, and control the moisture content of the solvent to be less than 10ppm. Use a percentile balance to accurately weigh 60g of ethylene carbonate and 140g of ethyl methyl carbonate, and pour them into an aluminum bottle. After fully stirring, put it in a 0℃ constant temperature box and freeze it for 1h. Then add 30g of lithium hexafluorophosphate while stirring. Finally, add 7.17g of vinyl carbonate, 1.20g of vinyl sulfate, and 0.72g of tris(trimethyl)silyl phosphate respectively, and stir evenly. Control the content of vinyl carbonate to 3%.
[0075] The electrolyte is injected into the lithium-ion dry battery for energy storage, and then immersed in an environment of 25°C for 48 hours. After the electrolyte fully infiltrates the battery, pre-charging, formation and capacity division are started. The pre-charging process is to charge to 10% SOC at a constant current of 0.01C, and then change to a constant current of 0.02C to charge to 30% SOC. After pre-charging, age for 48 hours at 45°C, and then vacuum evacuate. After aging, charge to 100% SOC at a constant current of 0.1C, stand for 10 minutes, and then discharge to 2.5V to determine the first charge and discharge efficiency. Next, continue aging at 45°C for 24 hours. After aging is completed, capacity division is performed.
[0076] Performance Testing:
[0077] The electrolytes and lithium-ion batteries of the embodiments and comparative examples were tested and their performance differences were compared using the following methods:
[0078] (1) Lithium-ion battery 45°C cycle test
[0079] The embodiments and comparative examples of the present invention carry out a 45°C cycle test on lithium-ion batteries according to the following steps. The detailed steps are: take a lithium-ion battery that has been fixed in capacity, put it into a 45°C constant temperature box, and let it stand for more than 1 hour to ensure that the internal temperature of the battery is close to 45°C. Then charge it at a constant current and constant voltage of 1C, with a cut-off voltage of 3.65V and a cut-off current of 0.05C. Then discharge it to 2.5V at a constant current of 1C. Perform charge and discharge cycles on the battery according to the above steps, and record the discharge capacity retention rate after 2000 cycles. The discharge capacity retention rate of the battery after 2000 cycles is calculated as the discharge capacity after the cycle divided by the discharge capacity of the first cycle. See Table 1 for specific test data.
[0080] (2) Lithium-ion battery storage test at 60°C
[0081] The steps of the high temperature storage performance test of the lithium-ion battery in the embodiments and comparative examples of the present invention are as follows: the fixed capacity battery is discharged to 2.5V at a constant current of 1C, left for 5 minutes, and then charged to 3.65V at a constant current and constant voltage of 1C, with a cut-off current of 0.05C. The battery is placed in a constant temperature box at 60°C and stored for 30 days, 60 days, 90 days, and 120 days respectively. After the battery is stored to the specified date, the battery is taken out. The battery is connected to the test cabinet, discharged to 2.5V at a constant current of 1C, and then charged at a constant current and constant voltage of 1C. The process of 1C constant current discharge is repeated 3 times. Finally, the discharge capacity recovery rate of the battery is obtained, and the relevant test results are shown in Table 2.
[0082] (3) Lithium-ion battery 25℃ rate test
[0083] The batteries in the embodiments of the present invention and the comparative examples are tested for rate performance at 25°C according to the following steps. The battery is placed in a constant temperature cabinet at 25°C and allowed to stand for 6 hours before charging and discharging. First, charge at 0.1C constant current and constant voltage, and discharge at 0.1C constant current, i.e., the battery is constant capacity. Then the discharge rate is changed, and the battery is discharged to 2.5V at 0.3C, 0.5C, and 1C, respectively, to obtain the discharge capacity at different rates. The discharge capacity at different rates is divided by the discharge capacity at 0.1C to obtain the capacity retention rate at different rates. The test results of the 25°C rate are shown in Table 3.
[0084] Table 1
[0085]
[0086] As shown in Table 1, this is the capacity retention rate of different lithium-ion batteries after 2000 cycles in a high temperature environment of 45°C. When 5% vinyl carbonate and 1.5% vinyl sulfite are added to the electrolyte, the capacity retention rate of the battery after 2000 cycles is 2.5% higher than that of the battery with only 3% vinyl carbonate. This is because the high content of vinyl carbonate improves the thermal stability of the interface film and reduces the occurrence of interface side reactions, while vinyl sulfite reduces the interface impedance and prevents the lithium precipitation problem caused by high vinyl carbonate. With the increase of the content of vinyl carbonate and vinyl sulfite, the capacity retention first increases and then decreases. With the use of the overcharge formation method in Example 4, the impedance of the lithium-ion battery is further reduced, the risk of lithium insertion due to excessive impedance is reduced, and the capacity retention rate of the battery cycle is improved, especially for batteries with higher vinyl carbonate. Since the overcharge formation method easily causes the oxidative decomposition of vinyl carbonate and vinyl sulfite, the content of vinyl carbonate and vinyl sulfite is reduced. Examples 7-9 inhibited the consumption of vinylene carbonate and vinyl sulfite by using antioxidant additives, and improved the cycle performance. Compared with the examples and comparative examples, Example 9 has the best high-temperature cycle performance.
[0087] Table 2
[0088]
[0089]
[0090] Table 2 shows the capacity recovery rate of batteries injected with different electrolytes and different formation methods at different storage times. Compared with the comparative examples, the capacity recovery rates of all batteries in Examples 1-9 are better, especially Example 9. Example 9 has a moderate content of vinyl carbonate and vinyl sulfite. At the same time, the overcharge formation step of Example 9 is most conducive to reducing the impedance of the battery. The new antioxidant additive T3 has the best antioxidant performance and reduces the oxidation consumption of vinyl carbonate and vinyl sulfite in the overcharge formation. The combination of vinyl carbonate, vinyl sulfite, overcharge formation and antioxidant additive (T3) makes Example 9 have the best high-temperature storage performance.
[0091] Table 3
[0092]
[0093] Table 3 shows the rate data of the embodiments and comparative examples at 25°C. Compared with the comparative examples, the rate performance of all embodiments is slightly worse, which is mainly caused by the thickening of the interface film caused by high vinyl carbonate. Comparing Example 2 with Examples 4, 5, and 6, the rate performance of the battery is significantly improved by the overcharge formation method, mainly because the overcharge method can reduce the polarization degree of the positive electrode interface, thereby reducing the positive electrode interface impedance. Comparing Example 6 with Examples 7, 8, and 9, the addition of antioxidant additives reduces the rate performance, mainly because the antioxidant additives reduce the oxidative decomposition of vinyl carbonate, indirectly increase the content of vinyl carbonate, and thus reduce the rate performance. Compared with T1 and T2, antioxidant T3 has the least deteriorating effect on the rate performance.
[0094] Combining the 45°C cycling, 60°C storage and room temperature rate data, Example 9 has the most balanced performance in cycling, storage and rate, that is, the best solution is 7% vinylene carbonate, 2.5% vinyl sulfite, 0.1C / 0.02C / 0.01C charging to 4.1V, T3.
[0095] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the patent of the present invention. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. An electrolyte comprising a lithium salt, an additive and a solvent, It is characterized in that The additives include vinylene carbonate and vinyl sulfite; the amount of vinylene carbonate added accounts for 5-15% of the total mass of the electrolyte, and the amount of vinyl sulfite added accounts for 1.5-5% of the total mass of the electrolyte.
2. An electrolyte according to claim 1, It is characterized in that The additives also include antioxidant additives, whose chemical structure is as shown in formula (I): Wherein, R1 is selected from one of hydrogen, halogen, substituted or unsubstituted alkane group, alkene group, alkyne group, aromatic group, phosphate group, sulfonate group, sulfate group, borate group, siloxy group, sulfite group, heterocyclic group and isocyanate group.
3. An electrolyte according to claim 2, It is characterized in that In the chemical structural formula of the antioxidant additive, the R1 is selected from one of acryl, trimethylsilyl and phenyl.
4. An electrolyte according to claim 3, It is characterized in that The amount of the antioxidant additive added is 0.01-1% of the total mass of the electrolyte.
5. An electrolyte according to claim 4, It is characterized in that The amount of vinylene carbonate added is 5-10% of the total mass of the electrolyte, the amount of vinyl sulfite added is 1.5-3.5% of the total mass of the electrolyte; and the amount of antioxidant additive added is 0.01-0.5% of the total mass of the electrolyte.
6. An electrolyte according to claim 1, It is characterized in that The additives also include vinyl sulfate and / or tris(trimethyl)silyl phosphoric acid; the amount of vinyl sulfate and / or tris(trimethyl)silyl phosphoric acid added accounts for 0.1-1% of the total mass of the electrolyte.
7. A lithium ion battery, It is characterized in that It comprises a positive electrode, a negative electrode, a separator and an electrolyte as described in any one of claims 1-6.
8. A method for forming a lithium ion battery, It is characterized in that The following steps are involved: S1: pre-charging the lithium-ion battery as claimed in claim 7 for the first time; S2: first aging, vacuum pumping; S3: Second pre-charge and discharge; S4: second aging; S5: Overcharge formation, charging the lithium-ion battery to 1.05-1.15 times of the conventional cut-off voltage with a charging current of 1-0.01C.
9. A lithium ion battery formation method according to claim 8, It is characterized in that The overcharge formation operation is to charge with a current of 0.5C to 1.06-1.12 times of the cut-off current; then charge with a current of 0.1C to 1.06-1.12 times of the cut-off current; and then charge with a current of 0.02C to 1.06-1.12 times of the cut-off current.
10. A lithium ion battery formation method according to claim 8, It is characterized in that The overcharge formation operation is to charge with a current of 0.1C to 1.08-1.1 times of the cut-off current; then charge with a current of 0.02C to 1.06-1.12 times of the cut-off current; and then charge with a current of 0.02C to 1.06-1.12 times of the cut-off current.