Non-oriented electrical steel sheet and method for producing same
By optimizing the content of Si, Mn and Al and the annealing process, combined with the insulating coating, the challenges of the non-oriented electromagnetic steel plate in terms of high strength and low iron loss are solved, and a non-oriented electromagnetic steel plate with high strength and excellent magnetic characteristics are achieved. Cold rolling fracture and iron damage deterioration are avoided.
Patent Information
- Application Number
- CN202380027701.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-15
- Filing Date
- 2023-03-15
- Publication Date
- 2024-11-01
AI Technical Summary
While the existing non-oriented electromagnetic steel plates pursue high strength and low iron loss, they are prone to problems of reduced toughness and cold rolling fracture, and high alloying will lead to low saturation flux density.
By optimizing the content of Si, Mn and Al, combining batch hot-rolled plate annealing and final annealing process, the nitriding of the steel plate surface is controlled, and an insulating film is used to reduce eddy current loss, and avoid double crystal deformation in the cold rolling process to ensure that the steel plate is guaranteed. toughness and magnetic properties.
The non-oriented electromagnetic steel plate with high strength and excellent magnetic characteristics is suitable for stator and rotor, reducing the yield rate and avoiding breakage and iron damage deterioration during cold rolling.
Smart Images

Figure BDA0005042771310000151 
Figure BDA0005042771310000161
Abstract
Description
Technical Field
[0001] The present invention relates to a non-oriented electrical steel sheet and a method for producing the same. Background Art
[0002] In recent years, global environmental issues have gradually attracted attention, and the demand for energy conservation has further increased. There is also a strong desire for higher efficiency of electrical equipment. Therefore, in non-oriented electromagnetic steel sheets, which are widely used as core materials for motors and generators, the demand for improved magnetic properties has further increased. This trend is particularly evident in drive motors for electric and hybrid vehicles and compressor motors for air conditioners.
[0003] The motor core of the various motors described above is composed of a stator as a fixed part and a rotor as a rotating part. The properties required of the stator and the rotor constituting the motor core are different from each other. The stator is required to have excellent magnetic properties (low iron loss and high magnetic flux density), especially low iron loss and high saturation magnetic flux density, while the rotor is required to have excellent mechanical properties (high strength).
[0004] The properties required for the stator and the rotor are different, so the desired properties can be achieved by separately manufacturing the non-oriented electromagnetic steel sheets for the stator and the non-oriented electromagnetic steel sheets for the rotor. However, preparing two types of non-oriented electromagnetic steel sheets will lead to a decrease in yield. Therefore, in order to achieve the high strength required for the rotor and the low iron loss and high saturation magnetic flux density required for the stator, non-oriented electromagnetic steel sheets with excellent strength and excellent magnetic properties have been studied in the past.
[0005] For example, Patent Documents 1 to 4 attempt to achieve excellent magnetic properties and high strength.
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent Document 1: International Publication No. 2019 / 017426
[0009] Patent Document 2: International Publication No. 2020 / 091039
[0010] Patent Document 3: International Publication No. 2020 / 091043
[0011] Patent Document 4: Japanese Patent Application Publication No. 2010-90474 Summary of the invention
[0012] Technical problem to be solved by the invention
[0013] However, in order to realize non-oriented electrical steel sheets with both high strength and low iron loss, as disclosed in Patent Documents 1 to 4, it is necessary to contain a large amount of alloy elements, which leads to problems such as reduced toughness and easy fracture during cold rolling. In addition, if the alloying is high, the saturation magnetic flux density will also be low.
[0014] The present invention has been made to solve the above-mentioned problems, and an object of the present invention is to stably provide a non-oriented electrical steel sheet having high strength and excellent magnetic properties.
[0015] Technical means for solving technical problems
[0016] The present invention is based on the following non-oriented electrical steel sheet and a method for producing the same.
[0017] (1) A non-oriented electromagnetic steel sheet,
[0018] The chemical composition of the base material is expressed in mass %,
[0019] C: 0.0050% or less,
[0020] Si: more than 3.70% and less than 4.60%,
[0021] Mn: more than 0.20% and less than 0.50%,
[0022] Al: 0.23-0.75%,
[0023] P: 0.030% or less,
[0024] S: 0.0018% or less,
[0025] N: 0.0040% or less,
[0026] Ti: less than 0.0050%,
[0027] Nb: less than 0.0050%,
[0028] Zr: less than 0.0050%,
[0029] V: less than 0.0050%,
[0030] Cu: less than 0.200%,
[0031] Ni: less than 0.500%,
[0032] Sn: 0.005~0.040%,
[0033] Sb: 0~0.040%,
[0034] The rest: Fe and impurities,
[0035] Satisfies the following formula (i),
[0036] The N content [N]s from the surface of the base material to a position of 20 μm in the depth direction is 0.0060% or less,
[0037] The average crystal grain size of the parent material is 50 to 120 μm.
[0038] The saturation flux density is above 1.945T.
[0039] The tensile strength is above 600MPa.
[0040] The plate thickness is 0.10~0.30mm,
[0041] 4.2≦Si+Al+0.5×Mn≦4.9···(i)
[0042] The element symbols in the above formulas represent the content (mass %) of each element.
[0043] (2) The non-oriented electrical steel sheet according to (1) above,
[0044] The base material has an insulating film on its surface.
[0045] (3) A method for producing a non-oriented electrical steel sheet, which is a method for producing the non-oriented electrical steel sheet according to (1) or (2) above,
[0046] The steel slab is subjected to the following steps: hot rolling; pickling; batch hot-rolled plate annealing at a soaking temperature of 650-780°C and a soaking time of 8-36 hours; cold rolling to a plate thickness of 0.10-0.30 mm; and final annealing at a soaking temperature of 880-1020°C and a soaking time of 1 second to 10 minutes.
[0047] The steel billet has the following chemical composition, in mass %,
[0048] C: 0.0050% or less,
[0049] Si: more than 3.70% and less than 4.60%,
[0050] Mn: more than 0.20% and less than 0.50%,
[0051] Al: 0.23-0.75%,
[0052] P: 0.030% or less,
[0053] S: 0.0018% or less,
[0054] N: 0.0040% or less,
[0055] Ti: less than 0.0050%,
[0056] Nb: less than 0.0050%,
[0057] Zr: less than 0.0050%,
[0058] V: less than 0.0050%,
[0059] Cu: less than 0.200%,
[0060] Ni: less than 0.500%,
[0061] Sn: 0.005~0.040%,
[0062] Sb: 0~0.040%,
[0063] The rest: Fe and impurities,
[0064] Satisfies the following formula (i),
[0065] 4.2≦Si+Al+0.5×Mn≦4.9···(i)
[0066] The element symbols in the above formulas represent the content (mass %) of each element.
[0067] Effects of the Invention
[0068] According to the present invention, a non-oriented electrical steel sheet having high strength and excellent magnetic properties can be obtained. DETAILED DESCRIPTION
[0069] The inventors of the present invention conducted intensive studies to solve the above-mentioned technical problems and finally obtained the following findings.
[0070] In order to achieve high strength, low iron loss, and high saturation magnetic flux density while ensuring toughness during cold rolling, it is necessary to optimize the contents of Si, Mn, and Al, which are main alloying elements.
[0071] Specifically, Si, which has the highest solid solution strengthening ability and the highest contribution to increasing resistance, is contained in an amount of more than 3.70% and less than 4.60%. In addition, in order to obtain good grain growth, Al is contained in an amount of more than 0.23%. On the other hand, in order to suppress the degradation of saturation magnetic flux density, the Al content is set to less than 0.75%. Furthermore, Mn, which has the lowest solid solution strengthening ability among the three elements but has little degradation in toughness and contributes to increasing resistance, is contained in an amount of more than 0.20%.
[0072] Here, the inventors of the present invention have repeatedly studied and found that the iron loss will deteriorate when the surface of the steel plate is nitrided. In addition, although the mechanism is unclear, it is found that Mn has an effect on the nitridation of the surface of the steel plate. In order to suppress the deterioration of the iron loss caused by the nitridation of the surface of the steel plate, the Mn content is set to 0.50% or less. In addition, it is also known that Sn has the effect of suppressing the nitridation of the surface of the steel plate. Therefore, Sn is contained in 0.005-0.040%.
[0073] In the usual continuous hot-rolled sheet annealing, since the hot-rolled sheet with oxide scale is inserted into the annealing furnace, oxide scale is generated which is difficult to remove during pickling after annealing, and mechanical descaling such as shot peening is required before pickling. However, in the high-alloy steel as described above, there is the following problem: twin crystal deformation is caused on the surface of the steel sheet by shot peening, and the twin crystal deformation is used as the starting point, which easily causes problems such as sheet breakage and edge cracking during cold rolling.
[0074] In the present invention, the hot rolled sheet is pickled before annealing, and then the hot rolled sheet is annealed in a batch furnace. The oxide scale of the hot rolled sheet can be easily removed by pickling, so shot peening is not required and twinning deformation does not occur. Therefore, even high alloy steel can ensure good toughness, and the occurrence of problems such as sheet fracture and edge cracking during cold rolling can be suppressed.
[0075] The present invention is obtained based on the above findings. Hereinafter, each element of the present invention will be described in detail.
[0076] 1. Overall composition
[0077] The non-oriented electrical steel sheet according to one embodiment of the present invention has high strength and excellent magnetic properties, and is therefore suitable for both stators and rotors. In addition, the non-oriented electrical steel sheet according to this embodiment preferably has an insulating film on the surface of a base material described below.
[0078] 2. Chemical composition of the base material
[0079] The reasons for limiting the content of each element are as follows. In the following description, "%" for the content means "mass %".
[0080] C: 0.0050% or less
[0081] C (carbon) is an element that causes the iron loss of the non-oriented electrical steel sheet to deteriorate. When the C content exceeds 0.0050%, the iron loss of the non-oriented electrical steel sheet deteriorates and good magnetic properties cannot be obtained. Therefore, the C content is set to 0.0050% or less. The C content is preferably 0.0040% or less, more preferably 0.0035% or less, and even more preferably 0.0030% or less. In addition, C contributes to the high strength of the non-oriented electrical steel sheet. In order to obtain this effect, the C content is preferably 0.0005% or more, and more preferably 0.0010% or more.
[0082] Si: more than 3.70% and less than 4.60%
[0083] Si (silicon) is an element that increases the electrical resistance of steel, reduces eddy current loss, and improves the high-frequency iron loss of non-oriented electromagnetic steel sheets. In addition, Si is also an effective element for increasing the strength of non-oriented electromagnetic steel sheets due to its large solid solution strengthening energy. In order to obtain these effects, the Si content is set to more than 3.70%. The Si content is preferably 3.80% or more, more preferably 3.90% or more, and even more preferably 4.00% or more. On the other hand, when the Si content is excessive, the workability deteriorates significantly and cold rolling is difficult to implement. Therefore, the Si content is set to less than 4.60%. The Si content is preferably less than 4.50%, more preferably less than 4.40%.
[0084] Mn: more than 0.20% and less than 0.50%
[0085] Mn (manganese) is an element effective in increasing the resistance of steel and reducing eddy current loss, thereby improving the high-frequency iron loss of non-oriented electromagnetic steel sheets. In addition, when the Mn content is too low, the effect of increasing the resistance is small, and fine sulfides (MnS) are precipitated in the steel, so the iron loss deteriorates. Therefore, the Mn content is set to more than 0.20%. The Mn content is preferably 0.25% or more, and more preferably 0.30% or more. On the other hand, if the Mn content is excessive, the nitridation of the surface layer of the steel plate becomes excessive, and the iron loss deteriorates. Therefore, the Mn content is set to less than 0.50%. The Mn content is preferably 0.45% or less, and more preferably 0.40% or less.
[0086] Al: 0.23~0.75%
[0087] Al (aluminum) is an element that has the effect of improving the high-frequency iron loss of non-oriented electromagnetic steel sheets by increasing the resistance of steel to reduce eddy current loss. In addition, Al also has the effect of improving iron loss by improving texture. In addition, although Al is not as good as Si, it is also an element that contributes to the high strength of non-oriented electromagnetic steel sheets through solid solution strengthening. In addition, adding an appropriate amount of Al suppresses the refinement of AlN generated by combining with N in steel, has the effect of improving grain growth during final annealing and suppressing the degradation of iron loss caused by fine AlN itself.
[0088] In order to obtain these effects, the Al content is set to be greater than 0.23%. The Al content is preferably greater than 0.25%, more preferably greater than 0.27%. In addition, the aforementioned nitridation of the surface layer of the steel plate occurs more easily when the Al content is higher. As a result, the iron loss deteriorates. However, in the present invention, by controlling the contents of Mn and Sn, the nitridation of the surface layer of the steel plate can be controlled even when the Al content is high. Therefore, the effect of the present invention is significantly exerted when the Al content is high. That is, when the Al content exceeds 0.45%, or is greater than 0.47%, the effect of the present invention is more significantly exerted. On the other hand, when the Al content is excessive, the toughness deteriorates and the risk of fracture during cold rolling increases. Therefore, the Al content is set to be less than 0.75%. The Al content is preferably less than 0.70%, more preferably less than 0.65%.
[0089] In this embodiment, the electrical resistance of the steel is ensured by properly controlling the contents of Si, Al and Mn. In addition, from the viewpoint of ensuring strength, it is necessary to properly control the contents of Si, Al and Mn. On the other hand, from the viewpoint of ensuring saturation magnetic flux density and toughness, an upper limit is also necessary. Therefore, in addition to the contents of Si, Al and Mn being within the above ranges, the following formula (i) must also be satisfied. The intermediate value of the following formula (i) is preferably greater than 4.3, more preferably greater than 4.4, preferably less than 4.8, and more preferably less than 4.7.
[0090] 4.2≦Si+Al+0.5×Mn≦4.9···(i)
[0091] The element symbols in the above formulas represent the content (mass %) of each element.
[0092] P: 0.030% or less
[0093] P (phosphorus) is contained in steel as an impurity. When its content is excessive, the toughness of the non-oriented electrical steel sheet is significantly reduced. Therefore, the P content is set to 0.030% or less. The P content is preferably 0.025% or less, and more preferably 0.020% or less. In addition, an extreme reduction in the P content sometimes causes an increase in manufacturing costs, so the P content is preferably 0.003% or more, and more preferably 0.005% or more.
[0094] S: 0.0018% or less
[0095] S (sulfur) is an element that increases iron loss by forming fine precipitates of MnS, thereby deteriorating the magnetic properties of the non-oriented electrical steel sheet. Therefore, the S content is set to 0.0018% or less. The S content is preferably 0.0016% or less, and more preferably 0.0014% or less. In addition, an extreme reduction in the S content sometimes causes an increase in manufacturing costs, so the S content is preferably 0.0001% or more, more preferably 0.0003% or more, and even more preferably 0.0005% or more.
[0096] N: 0.0040% or less
[0097] N (nitrogen) is an element that is inevitably mixed into steel. It is an element that forms nitrides, increases iron loss, and deteriorates the magnetic properties of non-oriented electrical steel sheets. Therefore, the N content is set to 0.0040% or less. The N content is preferably 0.0030% or less, and more preferably 0.0020% or less. In addition, an extreme reduction in the N content sometimes causes an increase in manufacturing costs, so the N content is preferably 0.0005% or more.
[0098] Ti: less than 0.0050%
[0099] Ti (titanium) is an element inevitably mixed into steel, and can combine with carbon or nitrogen to form precipitates (carbides, nitrides). When carbides or nitrides are formed, these precipitates themselves deteriorate the magnetic properties of the non-oriented electrical steel sheet. Furthermore, they hinder the grain growth in the final annealing, deteriorating the magnetic properties of the non-oriented electrical steel sheet. Therefore, the Ti content is set to less than 0.0050%. The Ti content is preferably 0.0040% or less, more preferably 0.0030% or less, and further preferably 0.0020% or less. In addition, an extreme reduction in the Ti content sometimes leads to an increase in manufacturing costs, so the Ti content is preferably 0.0005% or more.
[0100] Nb: less than 0.0050%
[0101] Nb (niobium) is an element that combines with carbon or nitrogen to form precipitates (carbides, nitrides) and thus contributes to high strength, but these precipitates themselves deteriorate the magnetic properties of the non-oriented electrical steel sheet. Therefore, the Nb content is set to less than 0.0050%. The Nb content is preferably 0.0040% or less, more preferably 0.0030% or less, and even more preferably 0.0020% or less. In addition, an extreme reduction in the Nb content sometimes causes an increase in manufacturing costs, so the Nb content is preferably 0.0001% or more.
[0102] Zr: less than 0.0050%
[0103] Zr (zirconium) is an element that combines with carbon or nitrogen to form precipitates (carbides, nitrides) and thus contributes to high strength. These precipitates themselves deteriorate the magnetic properties of the non-oriented electrical steel sheet. Therefore, the Zr content is set to less than 0.0050%. The Zr content is preferably 0.0040% or less, more preferably 0.0030% or less, and even more preferably 0.0020% or less. In addition, an extreme reduction in the Zr content sometimes leads to an increase in manufacturing costs, so the Zr content is preferably 0.0001% or more.
[0104] V: less than 0.0050%
[0105] V (vanadium) is an element that combines with carbon or nitrogen to form precipitates (carbides, nitrides) and thus contributes to high strength, but these precipitates themselves deteriorate the magnetic properties of the non-oriented electrical steel sheet. Therefore, the V content is set to less than 0.0050%. The V content is preferably 0.0040% or less, more preferably 0.0030% or less, and even more preferably 0.0020% or less. In addition, an extreme reduction in the V content sometimes leads to an increase in manufacturing costs, so the V content is preferably 0.0001% or more.
[0106] Cu: less than 0.200%
[0107] Cu (copper) is an element inevitably mixed into steel. If Cu is contained purposefully, the manufacturing cost of the non-oriented electrical steel sheet will increase. Therefore, in the present embodiment, Cu does not need to be actively contained, and the impurity level is sufficient. The Cu content is set to be less than the maximum value of 0.200% that is inevitably mixed in the manufacturing process. The Cu content is preferably less than 0.150%, more preferably less than 0.100%. In addition, the lower limit of the Cu content is not particularly limited, but an extreme reduction in the Cu content sometimes causes an increase in manufacturing costs. Therefore, the Cu content is preferably greater than 0.001%, more preferably greater than 0.003%, and even more preferably greater than 0.005%.
[0108] Ni: less than 0.500%
[0109] Ni (nickel) is an element that is inevitably mixed into steel. However, Ni is also an element that improves the strength of non-oriented electromagnetic steel sheets, so it can also be contained purposefully. Among them, due to the high price of Ni, the Ni content is set to less than 0.500%. The Ni content is preferably less than 0.400%, and more preferably less than 0.300%. In addition, the lower limit of the Ni content is not particularly limited, but an extreme reduction in the Ni content sometimes causes an increase in manufacturing costs. Therefore, the Ni content is preferably greater than 0.001%, more preferably greater than 0.003%, and even more preferably greater than 0.005%. In addition, when contained purposefully, the Ni content is preferably set to greater than 0.200%.
[0110] Sn: 0.005~0.040%
[0111] Sn (tin) is an element that segregates to the surface of the base material, inhibits oxidation and nitridation during annealing, and is useful for ensuring low iron loss in non-oriented electromagnetic steel sheets. In addition, Sn also has the effect of segregating to grain boundaries, improving texture, and increasing the magnetic flux density of non-oriented electromagnetic steel sheets. In order to obtain these effects, the Sn content is set to 0.005% or more. The Sn content is preferably 0.010% or more, more preferably 0.015% or more. On the other hand, when the Sn content is excessive, the toughness of the steel decreases and cold rolling is difficult. Therefore, the Sn content is set to 0.040% or less. The Sn content is preferably less than 0.040%, more preferably less than 0.035%, and more preferably less than 0.030%.
[0112] Sb: 0~0.040%
[0113] Sb (antimony), like Sn, is an element that segregates to the surface of the base material to inhibit oxidation and nitridation during annealing, thereby being useful for ensuring low iron loss in non-oriented electromagnetic steel sheets. In addition, Sb also has the effect of segregating to the grain boundaries, improving the texture, and increasing the magnetic flux density of the non-oriented electromagnetic steel sheet. Therefore, Sb may also be contained as needed. However, if the Sb content is excessive, the toughness of the steel decreases, and cold rolling sometimes becomes difficult. Therefore, the Sb content is set to less than 0.040%. The Sb content is preferably less than 0.030%. In addition, in the case where the above-mentioned effect is to be reliably obtained, the Sb content is preferably set to more than 0.005%, and more preferably to more than 0.010%.
[0114] In the chemical composition of the base material of the non-oriented electrical steel sheet of the present invention, the remainder is Fe and impurities. Here, the so-called "impurities" are components mixed in the industrial steel production due to various factors such as raw materials such as ore and scrap and the production process, and are allowed within the range that does not adversely affect the present invention.
[0115] In addition, as impurity elements, the contents of Cr and Mo are not particularly specified. In the non-oriented electrical steel sheet of the present embodiment, these elements are contained in the range of 0.5% or less, respectively, which has no effect on the characteristics of the non-oriented electrical steel sheet of the present embodiment. In addition, Ca and Mg are contained in the range of 0.002% or less, respectively, which has no particular effect on the characteristics of the non-oriented electrical steel sheet of the present embodiment. Even if rare earth elements (REM) are contained in the range of 0.004% or less, there is no particular effect on the characteristics of the non-oriented electrical steel sheet of the present embodiment. In addition, in the present embodiment, REM refers to a total of 17 elements consisting of Sc, Y and lanthanide elements, and the above-mentioned REM content refers to the total content of these elements.
[0116] O is also an impurity element, but if it is contained in the range of 0.035% or less, it has no effect on the characteristics of the non-oriented electrical steel sheet of the present embodiment. O is also mixed into the steel during the annealing process, so it is contained in the range of 0.010% or less in the content at the billet stage (i.e., ladle value), and has no particular effect on the characteristics of the non-oriented electrical steel sheet of the present embodiment.
[0117] Furthermore, in addition to the above-mentioned elements, elements such as Pb, Bi, As, B, and Se may be contained as impurity elements. However, if the content of each is within the range of 0.0050% or less, the characteristics of the non-oriented electrical steel sheet of the present embodiment are not impaired.
[0118] The chemical composition of the base material of the non-oriented electrical steel sheet of the present embodiment can be measured by various known measurement methods. For example, it can be measured by ICP emission analysis, gravimetric analysis or spark discharge emission analysis. In addition, C and S can be measured by combustion-infrared absorption method, N can be measured by inert gas combustion-heat conduction method, and O can be measured by inert gas melting-non-dispersive infrared absorption method.
[0119] Furthermore, in the present embodiment, from the viewpoint of suppressing nitridation in the surface layer of the steel plate, the N content [N]s from the surface of the base material to the position of 20 μm in the depth direction is set to 0.0060% or less. If [N]s is 0.0060% or less, iron loss degradation can be suppressed. [N]s is preferably 0.0055% or less, and more preferably 0.0050% or less.
[0120] In addition, the N content [N]s from the surface of the base material to the position of 20 μm in the depth direction is measured according to the following procedure. First, the N content [N]1 of the non-oriented electrical steel sheet after the insulating film is removed by a heated alkaline solution is measured. Next, both surfaces of the non-oriented electrical steel sheet are removed by chemical polishing at a rate of 20 μm, and the N content [N]2 of the sample after removal is measured. Then, [N]s is calculated by the following formula based on the measured [N]1, [N]2, and the sheet thickness t (μm) of the non-oriented electrical steel sheet.
[0121] [N]s=(t×[N]1-(t-40)×[N]2) / 40
[0122] 3. Crystal size
[0123] In the present embodiment, the average crystal grain size of the base material is set to 50 to 120 μm. By setting the average crystal grain size of the base material to be greater than 50 μm, the deterioration of hysteresis loss can be suppressed and the magnetic properties can be improved. On the other hand, by setting the average crystal grain size to be less than 120 μm, the strength of the steel can be improved, and the deterioration of iron loss caused by the increase in eddy current loss can be suppressed. The average crystal grain size is preferably greater than 60 μm, more preferably greater than 70 μm. In addition, the average crystal grain size is preferably less than 110 μm, more preferably less than 100 μm.
[0124] In the present invention, the average crystal grain size of the base material is determined in accordance with JIS G 0551:2013 "Steel - Microscopic testing method for crystal grain size".
[0125] 4.Magnetic properties
[0126] In the non-oriented electrical steel sheet of the present embodiment, the excellent magnetic properties mean that the iron loss W 10 / 400 Low, saturation flux density Bs is high.
[0127] Here, the iron loss W 10 / 400 It represents the iron loss generated under the conditions of maximum magnetic flux density of 1.0T and frequency of 400Hz, and is measured according to the Epstein method specified in JIS C 2550-1:2011. In the present invention, the iron loss W 10 / 400 Low means that it is 14.5 W / kg or less when the plate thickness is 0.26 mm or more, 12.5 W / kg or less when the plate thickness is 0.21-0.25 mm, and 11.0 W / kg or less when the plate thickness is 0.20 mm or less.
[0128] The saturation magnetic flux density Bs is measured by a vibrating sample magnetometer (VSM). In the non-oriented electrical steel sheet of the present embodiment, the magnetic flux density Bs is 1.945 T or more regardless of the sheet thickness.
[0129] 5. Mechanical properties
[0130] The non-oriented electrical steel sheet of the present embodiment has high strength, specifically, a tensile strength of 600 MPa or more. The tensile strength is preferably 605 MPa or more, more preferably 610 MPa or more. Here, the tensile strength is measured by performing a tensile test based on JIS Z 2241:2011.
[0131] 6.Plate thickness
[0132] In the non-oriented electrical steel sheet of the present embodiment, the sheet thickness is set to 0.10 mm or more from the viewpoint of the manufacturing cost of cold rolling and final annealing. On the other hand, from the viewpoint of reducing iron loss, the sheet thickness is set to 0.30 mm or less. Therefore, the sheet thickness of the non-oriented electrical steel sheet of the present embodiment is 0.10 to 0.30 mm.
[0133] In addition, the influence of nitridation on the surface of the steel plate becomes more significant when the plate thickness is thinner. That is, when the nitridation on the surface of the steel plate cannot be suppressed, the iron loss deteriorates more significantly as the plate thickness is thinner. However, in the present invention, since the nitridation on the surface of the steel plate is suppressed, the degradation of the iron loss can be suppressed even when the plate thickness is thin. Therefore, when the plate thickness is, for example, less than 0.25 mm or less than 0.20 mm, the effect of the present invention is more significantly exerted.
[0134] 7. Insulation film
[0135] In the non-oriented electromagnetic steel sheet of the present embodiment, it is preferred that an insulating coating is provided on the surface of the base material. The non-oriented electromagnetic steel sheet is used after the core material blank is punched out and stacked. By providing an insulating coating on the surface of the base material, the eddy current between the plates can be reduced, and the eddy current loss can be reduced as an iron core.
[0136] There is no particular limitation on the type of insulating coating, and a known insulating coating used as an insulating coating for non-oriented electromagnetic steel sheets can be used. As such an insulating coating, for example, a composite insulating coating mainly composed of an inorganic substance and further containing an organic substance can be cited. Here, the so-called composite insulating coating is, for example, an insulating coating mainly composed of at least one of inorganic substances such as metal chromate, metal phosphate, or colloidal silica, Zr compound, Ti compound, etc., and dispersed with fine organic resin particles. In particular, from the perspective of reducing the environmental load during manufacturing, which has been in increasing demand in recent years, it is preferred to use an insulating coating using metal phosphate, a coupling agent of Zr or Ti, or their carbonates or ammonium salts as starting materials.
[0137] The amount of the insulating film applied is not particularly limited, but is preferably 200 to 1500 mg / m2 per side, for example. 2 It is more preferably 300 to 1200 mg / m per side. 2 By forming the insulating film in such a manner that the adhesion amount is within the above range, it is possible to maintain excellent uniformity. In addition, when measuring the adhesion amount of the insulating film afterwards, various known measurement methods can be used, for example, a method of appropriately measuring the mass difference before and after immersion in a sodium hydroxide aqueous solution, or a fluorescent X-ray method using a calibration curve method, etc.
[0138] 8. Manufacturing method
[0139] The non-oriented electrical steel sheet of the present embodiment can be manufactured by sequentially performing a hot rolling process, a pickling process, a batch hot rolled sheet annealing process, a cold rolling process and a final annealing process on a steel ingot having the above-mentioned chemical composition under the conditions shown below. In addition, when an insulating film is formed on the surface of the base material, the insulating film forming process is performed after the above-mentioned final annealing process. Each process is described in detail below.
[0140] <Hot rolling process>
[0141] The steel ingot (steel billet) having the above chemical composition is heated, and the heated steel ingot is hot-rolled to obtain a hot-rolled plate. Here, the heating temperature of the steel ingot during hot rolling is not particularly specified, and is preferably set to 1050 to 1250° C., for example. In addition, the plate thickness of the hot-rolled plate after hot rolling is not particularly specified, but is preferably set to about 1.5 to 3.0 mm, for example, in consideration of the final plate thickness of the base material.
[0142] <Pickling process>
[0143] The hot rolled sheet is pickled to remove the oxide scale layer formed on the surface of the base material. The pickling conditions such as the concentration of the acid used in the pickling, the concentration of the accelerator used in the pickling, and the temperature of the pickling solution are not particularly limited and can be set to known pickling conditions.
[0144] <Batch hot-rolled sheet annealing process>
[0145] Afterwards, hot-rolled plate annealing is performed for the purpose of reducing the iron loss of the steel plate. Hot-rolled plate annealing is performed using a batch annealing furnace, with the soaking temperature set to 650-780°C and the soaking time set to 8-36 hours. By setting the soaking time to more than 8 hours, the metal texture is fully homogenized, the coarsening of the precipitates is also developed, and the effect of improving the iron loss can be fully obtained. On the other hand, when the soaking temperature exceeds 780°C, or the soaking time exceeds 36 hours, the crystal grain size is excessively coarsened, the toughness is reduced, and it breaks during cold rolling.
[0146] In addition, the batch annealing furnace is a non-oxidizing atmosphere, which can be set to a mixed atmosphere of H2 and N2 with a ratio of H2 of 1 to 100 volume % (i.e., H2+N2=100 volume %). Even if it is an atmosphere containing N2, if the content of Mn and Sn is appropriate, the nitridation of the surface layer of the base material can be suppressed. However, from the viewpoint of more reliably suppressing nitridation, it is preferably set to an atmosphere of H2: 100 volume %.
[0147] <Cold rolling process>
[0148] The steel sheet after the hot-rolled sheet annealing is subjected to cold rolling. In the cold rolling, the steel sheet is rolled at a reduction ratio such that the final sheet thickness of the base material becomes 0.10 to 0.30 mm.
[0149] <Final annealing process>
[0150] After the above-mentioned cold rolling, final annealing is performed. In the method for manufacturing a non-oriented electrical steel sheet of the present embodiment, a continuous annealing furnace is preferably used for final annealing. Final annealing is performed under the conditions of a soaking temperature of 880 to 1020°C and a soaking time of 1 second to 10 minutes. It is preferred that the atmosphere be a mixed atmosphere of H2 and N2 with a H2 ratio of 1 to 100% by volume (i.e., H2+N2=100% by volume), and the dew point of the atmosphere be set to -50 to +10°C.
[0151] When the soaking temperature is less than 880°C, the crystal grain size becomes fine and the iron loss becomes poor, which is not preferred. When the soaking temperature exceeds 1020°C, not only the strength is insufficient, but also nitridation of the surface layer occurs, resulting in poor iron loss, which is not preferred. In addition, if the soaking time is less than 1 second, the grains cannot grow sufficiently. On the other hand, when the soaking time exceeds 10 minutes, the manufacturing cost increases.
[0152] <Insulation film forming process>
[0153] After the above-mentioned final annealing, an insulating film forming step is performed as needed. Here, the method for forming the insulating film is not particularly limited, and the processing liquid for forming a known insulating film as shown below can be used, and the processing liquid can be applied and dried by a known method. As a known insulating film, for example, a composite insulating film mainly composed of inorganic substances and further containing organic substances can be cited.
[0154] The so-called composite insulating film is, for example, an insulating film mainly composed of at least one of metal salts such as metal chromate and metal phosphate, or inorganic substances such as colloidal silica, Zr compounds, and Ti compounds, and dispersed with fine organic resin particles. In particular, from the viewpoint of reducing the environmental load during production, which has been in increasing demand in recent years, it is preferred to use an insulating film using a metal phosphate, a coupling agent of Zr or Ti as a starting material, or an insulating film using a metal phosphate, a carbonate or an ammonium salt of a coupling agent of Zr or Ti as a starting material.
[0155] The surface of the base material on which the insulating film is formed may be subjected to any pretreatment such as degreasing treatment with alkali or pickling treatment with hydrochloric acid, sulfuric acid, phosphoric acid, etc. before the treatment liquid is applied. Alternatively, the treatment liquid may be applied to the surface of the base material in the final annealed state without performing these pretreatments.
[0156] The non-oriented electrical steel sheet of the present invention obtained as described above has excellent properties such as high saturation magnetic flux density, low iron loss, and high strength, and is therefore suitable as a material for either a rotor core or a stator.
[0157] Hereinafter, the present invention will be described in more detail with reference to Examples, but the present invention is not limited to these Examples.
[0158] Example
[0159] After heating the steel billet having the chemical composition shown in Table 1 to 1150°C, hot rolling was carried out at a final rolling temperature of 850°C and a final rolling thickness of 2.0 mm, and coiling was carried out at 600°C to produce a hot-rolled steel sheet. The obtained hot-rolled steel sheet was pickled to remove the oxide scale, and then annealed in a batch annealing furnace at the soaking temperature and soaking time shown in Table 2. The steel sheet obtained in this way was cold-rolled to produce a cold-rolled steel sheet with a thickness of 0.20 mm. In addition, a final annealing was carried out at a soaking temperature shown in Table 2 for a soaking time of 20 seconds in a mixed atmosphere of H2: 20%, N2: 80%, and a dew point of -30°C. The steel sheet after the final annealing was coated with an insulating film composed of aluminum phosphate and an alkali-styrene copolymer resin emulsion with a particle size of 0.2μm, and sintered at 350°C in the atmosphere.
[0160] [Table 1]
[0161]
[0162] [Table 2]
[0163] Table 2
[0164]
[0165] The underline indicates outside the scope of the present invention.
[0166] For each test material obtained, the average grain size was measured in a cross section parallel to the rolling direction of the base material in accordance with JIS G 0551:2013 "Steel - Microscopic test method for grain size". In addition, Epstein test pieces were taken from the rolling direction and width direction of each test material, and the iron loss W was evaluated by the Epstein test based on JIS C 2550-1:2011. 10 / 400 The saturation magnetic flux density was measured by a vibrating sample magnetometer (VSM).
[0167] Next, JIS No. 5 tensile test pieces were taken from each test material in accordance with JIS Z 2241: 2011 so that the longitudinal direction coincided with the rolling direction of the steel plate. Then, the tensile test was performed using the test pieces in accordance with JIS Z 2241: 2011 to measure the tensile strength.
[0168] Furthermore, the N content [N]s from the surface of the base material to the position of 20 μm in the depth direction was measured according to the following procedure. First, the N content [N]1 of the non-oriented electrical steel sheet after the insulating film was removed by a heated alkaline solution was measured. Next, both surfaces of the non-oriented electrical steel sheet were removed by chemical polishing at a rate of 20 μm, and the N content [N]2 of the sample after removal was measured. Then, [N]s was calculated by the following formula based on the measured [N]1, [N]2 and the sheet thickness t (μm) of the non-oriented electrical steel sheet.
[0169] [N]s=(t×[N]1-(t-40)×[N]2) / 40
[0170] The above results are shown together in Table 2.
[0171] In Test Nos. 2, 3, 6, 7, 9, 11, 15 to 17, 20, 21, 26, 27, 29 and 30 which satisfy the requirements of the present invention, it is found that the iron loss is low, the saturation magnetic flux density is high, and the tensile strength is high at 600 MPa or more.
[0172] On the other hand, in the comparative examples Test Nos. 1, 4, 5, 8, 10, 12 to 14, 18, 19, 22 to 25, 28, and 31 to 33, the iron loss W 10 / 400 Deterioration, or saturation magnetic flux density deterioration, or toughness deterioration significantly, making manufacturing difficult.
[0173] Specifically, in Test No. 1, the Mn content was lower than the prescribed range, so as a result, the amount of fine MnS precipitation increased and the iron loss deteriorated. In Test No. 4, the S content was higher than the prescribed range, so as a result, the amount of MnS precipitation increased and the iron loss deteriorated. In Test No. 5, the Sn content was lower than the prescribed range, and as a result, [N]s increased and the iron loss deteriorated. In Test No. 8, the Sn content was higher than the prescribed range, so the toughness deteriorated, the steel broke during cold rolling, and the tensile strength and magnetic properties could not be measured.
[0174] In Test No. 10, the Mn content was higher than the specified range, resulting in an increase in [N]s and a deterioration in iron loss. In Test No. 12, Si+Al+0.5×Mn was higher than the specified range, resulting in a deterioration in saturation magnetic flux density. In Test No. 13, the Si content and Si+Al+0.5×Mn were higher than the specified range, resulting in deterioration in toughness, fracture during cold rolling, and inability to measure tensile strength and magnetic properties.
[0175] In Test No. 14, the annealing temperature of the hot-rolled sheet was higher than the prescribed range, so the toughness deteriorated, and it broke during cold rolling, and the tensile strength and magnetic properties could not be measured. In Test No. 18, the annealing temperature of the hot-rolled sheet was lower than the prescribed range, so the average crystal grain size after the final annealing was smaller than the prescribed range, resulting in poor iron loss. In Test No. 19, the final annealing temperature was lower than the prescribed range, and the average crystal grain size was smaller than the prescribed range, resulting in poor iron loss. In Test No. 22, the final annealing temperature was higher than the prescribed range, the average crystal grain size was larger than the prescribed range, and [N]s was higher than the prescribed range, resulting in poor iron loss and poor strength.
[0176] In Test No. 23, the Si content was lower than the prescribed range, resulting in poor tensile strength. In addition, in Test No. 24, Si + Al + 0.5 × Mn was lower than the prescribed range, resulting in poor iron loss. Furthermore, in Test No. 25, the Al content was lower than the prescribed range, resulting in a smaller average grain size after final annealing than the prescribed range, resulting in poor iron loss. And, in Test No. 28, the Al content was higher than the prescribed range, resulting in poor toughness, fracture during cold rolling, and the measurement of tensile strength and magnetic properties could not be performed.
[0177] In Test No. 31, the soaking time of hot-rolled sheet annealing was longer than the specified range, so the coarsening of the crystal grain size led to poor toughness, and the sheet broke during cold rolling, making it impossible to measure the tensile strength and magnetic properties. In Test No. 32, the soaking temperature of hot-rolled sheet annealing was higher than the specified range, so the coarsening of the crystal grain size led to poor toughness, and the sheet broke during cold rolling, making it impossible to measure the tensile strength and magnetic properties. In addition, in Test No. 33, the Al content was lower than the specified range, so as a result, the texture deteriorated and fine AlN precipitated, and the iron loss deteriorated.
[0178] Industrial Applicability
[0179] As described above, according to the present invention, a non-oriented electrical steel sheet having high strength and excellent magnetic properties can be obtained at low cost.
Claims
1. A non-oriented electromagnetic steel sheet, The chemical composition of the base material is expressed in mass %, C: 0.0050% or less, Si: more than 3.70% and less than 4.60%, Mn: more than 0.20% and less than 0.50%, Al:0.23~0.75%、 P: 0.030% or less, S: 0.0018% or less, N: 0.0040% or less, Ti: less than 0.0050%, Nb: less than 0.0050%, Zr: less than 0.0050%, V: less than 0.0050%, Cu: less than 0.200%, Ni: less than 0.500%, Sn: 0.005~0.040%, Sb: 0~0.040%, The rest: Fe and impurities, And satisfy the following formula (i), 4.2≦Si+Al+0.5×Mn≦4.9···(i) in, The element symbols in the above formula are the content of each element in mass %. The N content [N]s from the surface of the base material to a position of 20 μm in the depth direction is 0.0060% or less, The average crystal grain size of the parent material is 50 to 120 μm. The saturation flux density is above 1.945T. The tensile strength is above 600MPa. The plate thickness is 0.10~0.30mm.
2. The non-oriented electrical steel sheet according to claim 1, The base material has an insulating film on its surface.
3. A method for producing a non-oriented electrical steel sheet, the method comprising producing the non-oriented electrical steel sheet according to claim 1 or claim 2, The steel ingot is subjected to the following steps: hot rolling; pickling; batch hot rolled sheet annealing at a soaking temperature of 650-780°C and a soaking time of 8-36 hours; cold rolling to a sheet thickness of 0.10-0.30 mm; and final annealing at a soaking temperature of 880-1020°C and a soaking time of 1 second to 10 minutes. The steel ingot has the following chemical composition, In terms of mass%, C: 0.0050% or less, Si: more than 3.70% and less than 4.60%, Mn: more than 0.20% and less than 0.50%, Al:0.23~0.75%、 P: 0.030% or less, S: 0.0018% or less, N: 0.0040% or less, Ti: less than 0.0050%, Nb: less than 0.0050%, Zr: less than 0.0050%, V: less than 0.0050%, Cu: less than 0.200%, Ni: less than 0.500%, Sn: 0.005~0.040%, Sb: 0~0.040%, The rest: Fe and impurities, And satisfy the following formula (i), 4.2≦Si+Al+0.5×Mn≦4.9···(i) in, The element symbols in the above formulas represent the content of each element in mass %.