Water electrolysis method, water electrolysis unit, and water electrolysis device
By using a double-layer electrolyte membrane structure in the water electrolysis method, carbon particles are used to suppress side reactions of hydrogen peroxide, the problem of deterioration of polymer electrolyte membrane is solved, and high electrolytic efficiency and durability are improved.
Patent Information
- Application Number
- CN202380027636.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-11-14
- Filing Date
- 2023-03-10
- Publication Date
- 2024-11-01
AI Technical Summary
In the water electrolysis method using polymer electrolyte membrane, it is difficult to maintain high electrolytic efficiency, mainly due to the deterioration of the electrolyte membrane by hydrogen peroxide-based side reactions, the proton conductivity is reduced.
A double-layer electrolyte membrane structure is adopted, in which the first layer contains polymer electrolytes, and the second layer is located on the cathode side and contains carbon particles to inhibit the formation and movement of hydrogen peroxides and prevent the electrolyte membrane from deteriorating.
It effectively suppresses voltage rise, maintains high electrolytic efficiency, and improves the durability and electrolytic efficiency of the electrolyte membrane.
Smart Images

Figure CN118891399A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a water electrolysis method, a water electrolysis unit and a water electrolysis device. Background Art
[0002] Methods for generating oxygen and hydrogen by water electrolysis using a polymer electrolyte membrane are known. These water electrolysis methods supply water to an electrolysis unit divided into an anode and a cathode by a polymer electrolyte membrane, thereby generating oxygen at the anode and hydrogen at the cathode.
[0003] As methods of supplying water to the electrolysis unit, there are known methods of supplying water only to the anode (for example, see Patent Document 1), supplying water only to the cathode (for example, see Patent Document 2), and supplying water to both the anode and the cathode (for example, see Patent Document 3).
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Publication No. 2021-25116
[0007] Patent Document 2: Japanese Patent Application No. 2020-525653
[0008] Patent Document 3: Japanese Patent Application Publication No. 2021-105194 Summary of the invention
[0009] Problems to be solved by the invention
[0010] In order to maintain high electrolysis efficiency in water electrolysis using a polymer electrolyte membrane, it is important to maintain the proton conductivity of the polymer electrolyte membrane. However, in conventional water electrolysis methods using a polymer electrolyte membrane, sufficiently high electrolysis efficiency cannot be maintained.
[0011] Therefore, in view of the above problems, an object of the present invention is to provide a water electrolysis method capable of maintaining high electrolysis efficiency.
[0012] Means for solving problems
[0013] The inventors of the present application have found that the above-mentioned problem is caused by an environment in which hydrogen peroxide and hydrogen peroxide radicals generated by a side reaction at the cathode easily attack the polymer electrolyte membrane, thereby completing the present invention.
[0014] That is, the present invention is a water electrolysis method, in which water is supplied to an electrolysis unit which is divided into an anode and a cathode by an electrolyte membrane and electrolysis is performed, thereby generating oxygen at the anode and hydrogen at the cathode, respectively. The electrolyte membrane has a first layer and a second layer, the first layer contains a polymer electrolyte, and the second layer is located on the cathode side of the first layer and contains carbon particles.
[0015] Effects of the Invention
[0016] According to the present invention, a water electrolysis method capable of maintaining high electrolysis efficiency can be provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] [ Figure 1 ] is a cross-sectional schematic diagram showing an example of an electrolysis unit that can be used in the water electrolysis method involved in an embodiment of the present invention.
[0018] [ Figure 2 ] is a graph showing the relationship between the electrolysis time (evaluation time) and the applied voltage of Examples 1 and 2 and Comparative Examples 1 and 2.
[0019] [ Figure 3 ] is a graph showing the relationship between the electrolysis time (evaluation time) and the applied voltage of Examples 3, 4 and Comparative Examples 3, 4.
[0020] [ Figure 4 ] is a graph showing the relationship between the electrolysis time (evaluation time) and the applied voltage in Examples 1 to 4. DETAILED DESCRIPTION
[0021] Hereinafter, embodiments of the present invention will be described in detail, but the present invention is not limited to the following embodiments and can be implemented with various modifications depending on the purpose and application.
[0022] [Water electrolysis method]
[0023] use Figure 1 A water electrolysis method according to an embodiment of the present invention will be described. Figure 1 This is a schematic cross-sectional view showing an example of an electrolysis unit that can be used in the water electrolysis method according to the embodiment of the present invention.
[0024] The interior of the electrolytic cell 1 is divided into an anode 20 and a cathode 30 by an electrolyte membrane 10. The anode 20 and the cathode 30 are connected to a power source (not shown), respectively. Moreover, the diaphragms 41 and 42 are used to clamp them from both sides. The electrolyte membrane 10 includes a first layer 11 and a second layer 12, and the second layer 12 is arranged on the cathode 30 side. In the present invention, the first layer 11 contains a polymer electrolyte, and the second layer 12 contains carbon particles. The constituent elements of the first layer 11 and the second layer 12 will be described in detail later. In addition, the preferred electrode method will also be described later.
[0025] Water electrolysis occurs by applying voltage to electrodes. If the first layer 11 deteriorates and the membrane resistance increases due to long-term water electrolysis, the applied voltage needs to be increased to maintain a certain current density. Increasing the applied voltage means that the electrolysis efficiency decreases.
[0026] In water electrolysis using a polymer electrolyte membrane, the main reason for the reduction in electrolysis efficiency is the attack of hydrogen peroxides on polymer electrolytes. It should be noted that in this specification, the term "hydrogen peroxides" is used in the general sense of hydrogen peroxide and the free radicals produced by the decomposition of hydrogen peroxide. In water electrolysis, the oxygen generated at the anode sometimes moves to the cathode and reacts with the hydrogen generated at the cathode to generate hydrogen peroxides by side reactions. It is believed that these byproducts deteriorate the electrolyte membrane (reducing proton conductivity).
[0027] In the water electrolysis method according to the embodiment of the present invention, the second layer 12 containing carbon particles is arranged on the cathode 30 side of the first layer 11. It is believed that the second layer 12 suppresses the migration of hydrogen peroxides generated by the side reaction at the cathode 30 to the first layer 11, thereby suppressing the degradation of the first layer. Although the mechanism is not clear, it is speculated that the carbon particles contained in the second layer 12 capture or decompose hydrogen peroxides. In this way, according to the water electrolysis method according to the embodiment of the present invention, the increase in applied voltage can be suppressed, and the effect of being able to maintain high electrolysis efficiency can be achieved.
[0028] In the water electrolysis method involved in the embodiment of the present invention, the method for supplying water to the electrolysis unit is not particularly limited, and a known method can be used. As a method for supplying water to the electrolysis unit, specifically, there are known methods for supplying water to the anode, supplying water to the cathode, and supplying water to the anode and cathode. In the above-mentioned water supply method, it is preferred to supply water from the outside of the electrolysis unit using a pump or the like. The water electrolysis method involved in the embodiment of the present invention can adopt any of the above-mentioned water supply methods. Among them, from the viewpoint of electrolysis efficiency, it is preferred to promote the generation of oxygen and protons caused by the oxidation reaction of water, and therefore, it is preferred to supply water to at least the anode.
[0029] In the water electrolysis method according to the embodiment of the present invention, water (H2O) is supplied to the anode 20 and the cathode 30 and electrolysis is performed, thereby generating oxygen (O2) at the anode 20 and hydrogen (H2) at the cathode 30. By directly supplying water to the anode that requires water in the electrolysis reaction, high electrolysis efficiency can be expected.
[0030] Water may or may not be supplied to the cathode 30. It is expected that the supply of water to the cathode 30 promotes the separation of hydrogen generated by the cathode 30. On the other hand, if water is supplied to the cathode 30, the dissolved oxygen contained in the supplied water may react with the hydrogen generated by the cathode 30 to generate hydrogen peroxides as a side reaction. Therefore, from the viewpoint of suppressing the generation of hydrogen peroxides as a side reaction, it is preferable that water is not supplied to the cathode 30 in the water electrolysis method according to the embodiment of the present invention. That is, it is preferable that water is supplied only to the anode 20 in the water electrolysis method according to the embodiment of the present invention.
[0031] When water is supplied to the cathode 30, deaerated water is preferably used in consideration of the above. For the deaeration treatment, a known method such as gas bubbling, reduced pressure treatment, membrane separation, chemical removal using a deoxidizer, etc. can be used.
[0032] In addition, the water electrolysis method according to the embodiment of the present invention may adopt a method in which water is not supplied to the anode but only to the cathode. In this case, the water supplied to the cathode is transported to the anode through the electrolyte membrane. In this case, it is also preferred to use degassed water.
[0033] The water electrolysis method according to the embodiment of the present invention is preferably a proton exchange membrane type water electrolysis method using a proton exchange membrane as an electrolyte membrane, and may be an anion exchange membrane type water electrolysis method using an anion exchange membrane.
[0034] [Layer 1]
[0035] The electrolyte membrane used in the water electrolysis method of the present invention has two layers, and the layer on the anode side in the positional relationship with the second layer described later is called the first layer, and the first layer contains a polymer electrolyte. That is, the first layer functions as a polymer electrolyte layer. As the polymer electrolyte, a known polymer electrolyte such as a fluorine-based polymer electrolyte and a hydrocarbon-based polymer electrolyte can be used.
[0036] Examples of fluorine-based polymer electrolytes include fluorine-based polymers having ionic groups. The fluorine-based polymers are polymers in which most or all of the hydrogen atoms in the alkyl and / or alkylene groups in the molecule are replaced by fluorine atoms.
[0037] Examples of fluorine-based polymer electrolytes include perfluorocarbon sulfonic acid polymers, perfluorocarbon phosphonic acid polymers, trifluorostyrene sulfonic acid polymers, trifluorostyrene phosphonic acid polymers, ethylene tetrafluoroethylene-g-styrene sulfonic acid polymers, ethylene-tetrafluoroethylene copolymers, and polyvinylidene fluoride-perfluorocarbon sulfonic acid polymers.
[0038] Among them, perfluorocarbon sulfonic acid polymers are preferred from the viewpoints of heat resistance, chemical stability, etc. Examples of such polymers include commercially available products such as “NAFION” (registered trademark) (manufactured by Chemizer Co., Ltd.), “FREMINION” (registered trademark) (manufactured by AGC Corporation), and “ASHIPREX” (registered trademark) (manufactured by Asahi Kasei Corporation).
[0039] Examples of hydrocarbon-based polymer electrolytes include hydrocarbon-based polymers having ionic groups. A hydrocarbon-based polymer is a polymer having a main chain with hydrocarbon as a main structural unit.
[0040] As the hydrocarbon-based polymer electrolyte, an aromatic hydrocarbon-based polymer having an aromatic ring in the main chain is preferred. The aromatic ring includes not only hydrocarbon-based aromatic rings but also heterocyclic rings. In addition, a portion of aliphatic units may be included together with the aromatic ring unit.
[0041] Specific examples of aromatic hydrocarbon polymers include those having, together with an aromatic ring in the main chain, a polysulfone, polyethersulfone, polyphenylene ether, polyarylene ether, polyphenylene sulfide, polyphenylene sulfide sulfone, polyparaphenylene, polyarylene polymers, polyarylene ketone, polyether ketone, polyarylene phosphine oxide, polyether phosphine oxide, polyphenylene Polymers with structures such as polyazole, polybenzothiazole, polybenzimidazole, polyamide, polyimide, polyetherimide, and polyimide sulfone.
[0042] It should be noted that the above-mentioned polysulfone is a general term for structures having a sulfone bond in the molecular chain, the above-mentioned polyethersulfone is a general term for structures having an ether bond and a sulfone bond in the molecular chain, and the above-mentioned polyetherketone is a general term for structures having an ether bond and a ketone bond in the molecular chain. The aromatic hydrocarbon-based polymer may have a plurality of these structures.
[0043] As the aromatic hydrocarbon polymer, a polyetherketone polymer is particularly preferred. Examples of the polyetherketone polymer include polyetherketone, polyetherketoneketone, polyetheretherketone, polyetheretherketoneketone, and polyetherketoneetherketoneketone.
[0044] The above-mentioned ionic group is an ionic group having any one of cation exchange capacity or anion exchange capacity. In the water electrolysis method of the present invention, it is preferred to use a proton exchangeable ionic group. As such a functional group, sulfonic acid group, sulfonimide group, sulfate group, phosphonic acid group, phosphoric acid group, carboxylic acid group, ammonium group, phosphonium group, amino group can be cited. Two or more ionic groups can be included in the polymer. Among them, from the aspect of excellent water electrolysis performance, preferably sulfonic acid group, sulfonimide group, sulfate group, from the aspect of raw material cost, more preferably sulfonic acid group.
[0045] From the balance of proton conductivity and water resistance, the ion exchange capacity (IEC) of the polymer electrolyte is preferably 0.1meq / g or more and 5.0meq / g or less. The IEC of the hydrocarbon polymer with an ionic group is more preferably 1.0meq / g or more, and more preferably 1.4meq / g or more. In addition, the IEC of the hydrocarbon polymer with an ionic group is more preferably 3.5meq / g or less, and more preferably 3.0meq / g or less. The IEC of the fluorine-based polymer with an ionic group is more preferably 0.5meq / g or more, and more preferably 0.7meq / g or more. In addition, the IEC of the fluorine-based polymer with an ionic group is more preferably 1.8meq / g or less, and more preferably 1.5meq / g or less. When IEC is 0.1meq / g or more and 5.0meq / g or less, excellent proton conductivity and water resistance can be achieved simultaneously.
[0046] Here, IEC is the molar amount of ionic groups introduced into the polymer electrolyte per unit dry weight, and a larger value indicates a larger amount of ionic groups introduced. In the present invention, IEC is defined as a value obtained by neutralization titration.
[0047] As the polymer electrolyte used in the first layer, hydrocarbon polymers are preferred, aromatic hydrocarbon block copolymers are more preferred, and polyetherketone block copolymers are particularly preferred, from the perspective of relatively high water electrolysis performance and relatively low oxygen permeability. Here, the so-called block copolymer refers to a block copolymer formed by a segment containing a structural unit containing an ionic group and a segment containing a structural unit not containing an ionic group.
[0048] The first layer preferably contains a hydrocarbon-based polymer electrolyte as the polymer electrolyte. Relative to the total mass of the polymer electrolyte of the first layer, it is preferred that 60% by mass or more of the hydrocarbon-based polymer electrolyte be contained, more preferably 75% by mass or more of the hydrocarbon-based polymer electrolyte be contained, further preferably 90% by mass of the hydrocarbon-based polymer electrolyte be contained, and particularly preferably 100% by mass of the hydrocarbon-based polymer electrolyte be contained.
[0049] In order to improve its strength, the first layer preferably contains a porous substrate. As the form in which the first layer contains a porous substrate, it is preferably, for example, the following form: having a layered portion (composite portion) containing a porous substrate and a polymer electrolyte, and having a layered portion (non-composite portion) containing a polymer electrolyte but not containing a porous substrate on one or both sides of the composite portion. The composite portion is preferably filled or impregnated with a hydrocarbon-based polymer electrolyte in the pores of the porous substrate.
[0050] In the first layer, the thickness of the first layer is recorded as 100%, and the thickness ratio of the composite part in the case of layered state is preferably 10 to 90%, more preferably 20 to 80%, and particularly preferably 30 to 70%. Here, the thickness of the composite part is calculated as the thickness of the porous substrate. As the specific thickness of the composite part, it is preferably in the range of 22 to 47 μm, more preferably in the range of 25 to 45 μm, and particularly preferably in the range of 30 to 43 μm. In addition, when the non-composite part is layered, the thickness of each layer is preferably 3 μm or more, more preferably 5 μm or more, and particularly preferably 10 μm or more. In addition, the thickness of each layer of the non-composite part is preferably 45 μm or less, more preferably 40 μm or less, and particularly preferably 35 μm or less.
[0051] As the form of the porous substrate, there can be mentioned woven fabrics, nonwoven fabrics, porous films, mesh fabrics, etc. As the porous substrate, there can be mentioned, for example, hydrocarbon porous substrates with hydrocarbon polymer compounds as main components, fluorine porous substrates with fluorine polymer compounds as main components, etc.
[0052] Examples of hydrocarbon polymer compounds include polyethylene (PE), polypropylene (PP), polystyrene (PS), polyacrylate, polymethacrylate, polyvinyl chloride (PVC), polyvinylidene chloride (PVdC), polyester, polycarbonate (PC), polysulfone (PSU), polyethersulfone (PES), polyphenylene ether (PPO), polyarylene ether polymers, polyphenylene sulfide (PPS), polyphenylene sulfide sulfone, polyparaphenylene (PPP), polyarylene polymers, polyarylene ketone, polyether ketone (PEK), polyarylene phosphine oxide, polyether phosphine oxide, polyphenylene ... Polyimide (PI), polyetherimide (PEI), polyimide sulfone (PIS), etc.
[0053] Examples of fluorine-based polymer compounds include polytetrafluoroethylene (PTFE), polyhexafluoropropylene, tetrafluoroethylene-hexafluoropropylene copolymer (FEP), ethylene-tetrafluoroethylene copolymer (ETFE), polyvinylidene fluoride (PVdF), polychlorotrifluoroethylene (PCTFE), perfluoroalkoxy fluororesin (PFA), and ethylene-chlorotrifluoroethylene copolymer (ECTFE).
[0054] As the form of the porous substrate, for example, from the viewpoint of reinforcing the first layer which is relatively thick and has a thickness of 40 μm or more, a porous substrate with relatively high strength is preferred, and from this viewpoint, a mesh fabric is preferred. Compared with the porous substrates commonly used in the past in this field, the fiber diameter of the mesh fabric is relatively large and has high strength. As the material of the fiber constituting the mesh fabric, polyester, liquid crystal polyester, polyphenylene sulfide, polyether ketone, polyether ether ketone, and polyether ketone ketone are preferred. Among them, liquid crystal polyester is particularly preferred from the viewpoint of strength.
[0055] The thickness of the first layer is preferably 40 μm or more and 250 μm or less. From the viewpoint of improved durability, the thickness of the first layer is more preferably 50 μm or more, further preferably 60 μm or more, and particularly preferably 70 μm or more. On the other hand, if the thickness of the first layer is greater than 250 μm, the water electrolysis performance is reduced, and in addition, it becomes disadvantageous from the viewpoints of material cost, productivity, and processability. From the above viewpoints, the thickness of the first layer is more preferably 200 μm or less, further preferably 180 μm or less, and particularly preferably 150 μm or less.
[0056] The first layer may contain various additives such as antioxidants, surfactants, radical scavengers, hydrogen peroxide decomposers, non-electrolyte polymers, elastomers, fillers, etc., within a range that does not inhibit the effects of the present invention.
[0057] When the first layer includes a polymer electrolyte and a porous substrate, the total mass of the polymer electrolyte and the porous substrate is preferably 80% by mass or more, more preferably 90% by mass or more, and particularly preferably 95% by mass or more relative to the total mass of the first layer. In addition, when the first layer does not include a porous substrate, the mass of the polymer electrolyte is preferably 80% by mass or more, more preferably 90% by mass or more, and particularly preferably 95% by mass or more relative to the total mass of the first layer.
[0058] When the first layer contains components other than the polymer electrolyte and the porous substrate, the total mass of the other components is preferably less than 20 mass %, more preferably less than 10 mass %, and particularly preferably less than 5 mass % relative to the total mass of the first layer.
[0059] As described above, the polymer electrolyte used in the first layer is preferably a proton-exchange polymer electrolyte, but may also be an anion-exchange polymer electrolyte.
[0060] [Layer 2]
[0061] The electrolyte membrane used in the water electrolysis method of the present invention has two layers, and the layer on the cathode side in terms of positional relationship with the above-mentioned first layer is called the second layer, and the second layer contains at least carbon particles. As carbon particles, there are no particular restrictions, and known carbon particles can be used. For example, carbon black, activated carbon, carbon nanotubes, carbon nanofibers, fullerenes, etc. can be mentioned. Among them, carbon black is preferred. As carbon black, for example, furnace black, acetylene black, thermal cracking carbon black, channel black, lamp black, gas black, petroleum carbon black, Ketjen black can be mentioned.
[0062] The specific surface area of the carbon particles is preferably 30 to 2,000 m 2 The carbon particles having such a specific surface area can be expected to effectively contribute to the capture and decomposition of hydrogen peroxides.
[0063] In addition, the carbon particles preferably have acidic groups such as phenolic hydroxyl groups, carboxyl groups, quinone groups, lactone groups, etc. as surface functional groups. Carbon particles having such surface functional groups are expected to effectively contribute to the capture and decomposition of hydrogen peroxides.
[0064] In addition, the carbon particles are preferably carbon particles that do not carry a catalyst metal. For example, carbon particles (carbon) carrying a catalyst metal such as platinum are generally used in the catalyst layer, but such carbon particles carrying a catalyst metal sometimes cannot fully exhibit the function of capturing or decomposing hydrogen peroxide.
[0065] As described above, the carbon particles are preferably carbon particles that do not carry a catalyst metal, but may contain a small amount of carbon particles that carry a catalyst metal within a range that does not hinder the effect of the present invention. In this case, the content is preferably 20% by mass or less, more preferably 10% by mass or less, and particularly preferably 5% by mass or less, when the total amount of the carbon particles is 100% by mass.
[0066] The carbon particles not only contribute to the capture and decomposition of hydrogen peroxide, but also can be expected to have an effect of bonding the second layer to the first layer by an anchoring effect.
[0067] From the viewpoint of the function of capturing / decomposing hydrogen peroxides, dispersibility, film-forming property and adhesiveness, the average primary particle size of the carbon particles is preferably 5 nm or more, more preferably 10 nm or more, particularly preferably 20 nm or more, and is preferably 500 nm or less, more preferably 200 nm or less, particularly preferably 100 nm or less.
[0068] The second layer may or may not contain a binder. When the second layer does not contain a binder, for example, the second layer can be formed by blowing carbon particles onto the first layer. Details will be described later.
[0069] From the viewpoint of film strength and productivity, the second layer preferably contains a binder. As the binder, an organic binder and an inorganic binder can be cited. As the organic binder, various polymers can be used, and as the inorganic binder, a known inorganic binder that can be modulated by a sol-gel method can be used.
[0070] The second layer preferably contains a polymer as a binder. Examples of the polymer include nonionic polymers and ionic polymers, which can be used alone or in combination. Examples of the nonionic polymer include fluorine-based polymers and hydrocarbon-based polymers.
[0071] Examples of the nonionic fluorine-based polymer include polytetrafluoroethylene, polyvinylidene fluoride, a copolymer of vinylidene fluoride and hexafluoropropylene, a copolymer of vinylidene fluoride and trifluoroethylene, a copolymer of vinylidene fluoride and tetrafluoroethylene, and polyvinylidene fluoride.
[0072] Examples of the nonionic hydrocarbon polymer include polysulfone, polyethersulfone, polyphenylene ether, polyarylene ether, polyphenylene sulfide, polyphenylene sulfide sulfone, polyparaphenylene, polyarylene polymers, polyarylene ketone, polyether ketone, polyarylene phosphine oxide, polyether phosphine oxide, polyphenylene sulfide, polyphenylene sulfide sulfone ... Polyimide, polyimide sulfone, polyvinyl alcohol, etc.
[0073] Examples of the ionic polymer include the above-mentioned fluorine-based polymer electrolytes and hydrocarbon-based polymer electrolytes.
[0074] As the polymer contained in the second layer, from the viewpoint of electrolysis efficiency, a polymer electrolyte is preferably used. In addition, from the viewpoint that degradation caused by hydrogen peroxides is less likely to occur and the adhesion between the catalyst layer sometimes provided by the cathode and the second layer is improved, a fluorine-based polymer electrolyte is particularly preferably used.
[0075] When the second layer contains a polymer, from the viewpoint of the durability of the first layer (inhibiting degradation), the electrolysis efficiency, and the adhesion between the first layer and the second layer, the ratio (I / C) of the mass of the polymer (I) to the mass of the carbon particles (C) is preferably 0.4 or more, more preferably 0.5 or more, particularly preferably 0.6 or more, and is preferably 2.0 or less, more preferably 1.6 or less, and particularly preferably 1.4 or less.
[0076] When the second layer contains an adhesive, it preferably contains 60% by mass or more of a fluorine-based polymer electrolyte relative to the total mass of the adhesive, more preferably contains 75% by mass or more of a fluorine-based polymer electrolyte, further preferably contains 90% by mass or more of a fluorine-based polymer electrolyte, and particularly preferably contains 100% by mass of a fluorine-based polymer electrolyte.
[0077] The second layer may further contain a known hydrogen peroxide decomposition agent and a free radical scavenger. As the hydrogen peroxide decomposition agent, for example, phosphorus compounds such as polyphosphoric acid, trimethylphosphine, and alkyl phosphites can be cited. As the free radical scavenger, for example, phenol derivatives such as 2,6-di-tert-butyl-methylphenol, 2,4-dimethyl-6-methylphenol, 2,4-di-tert-butyl-6-methylphenol, aromatic amine derivatives such as N,N'-diphenyl-p-phenylenediamine, phenyl-β-naphthylamine, and metal compounds such as Ce, Ru, Mn, Co, and Fe can be cited. Among them, Ce compounds are preferred, and Ce oxides are particularly preferred.
[0078] The second layer may contain various additives such as a surfactant, a non-electrolyte polymer, an elastomer, etc., within a range not inhibiting the effects of the present invention.
[0079] The carbon particles in the second layer preferably contain a mass of 25% or more, more preferably 30% or more, and particularly preferably 40% or more relative to the total mass of the second layer. In addition, the above ratio is preferably 90% or less, more preferably 80% or less, and particularly preferably 70% or less.
[0080] From the viewpoint of suppressing the migration of hydrogen peroxides, the thickness of the second layer is preferably 3 μm or more, more preferably 5 μm or more, and particularly preferably 7 μm or more. On the other hand, from the viewpoint of ensuring good water electrolysis performance, the thickness is preferably 30 μm or less, more preferably 25 μm or less, further preferably 20 μm or less, and particularly preferably 15 μm or less.
[0081] In addition, from the viewpoint of ensuring good water electrolysis performance, the ratio (T2 / T1) of the thickness (T2) of the second layer to the thickness (T1) of the first layer is preferably 0.30 or less, more preferably 0.25 or less, further preferably 0.20 or less, and particularly preferably 0.15 or less. On the other hand, from the viewpoint of inhibiting the migration of hydrogen peroxides and improving durability, the above ratio (T2 / T1) is preferably 0.03 or more, more preferably 0.05 or more, further preferably 0.06 or more, and particularly preferably 0.07 or more.
[0082] In the electrolyte membrane of the present invention, the membrane electrode assembly (MEA) and the catalyst layer-carrying electrolyte membrane (CCM) using the same, the second layer of the electrolyte membrane is preferably arranged in contact with the catalyst layer of the cathode described later from the viewpoint of electrolysis efficiency and durability.
[0083] [Method for producing electrolyte membrane]
[0084] The following is an example of a method for producing an electrolyte membrane. As the polymer electrolyte used in the first layer, a commercially available product such as "NAFION" (registered trademark) (manufactured by Kemaz Co., Ltd.) can be used, or a film obtained by coating a polymer electrolyte solution on a film-forming substrate such as a PET film, drying it, and then forming a film can also be used.
[0085] The first layer may also be in the form of a layered portion (non-composite portion) containing a porous substrate and a polymer electrolyte on one or both sides of a layered portion (composite portion) containing a porous substrate and a polymer electrolyte. As a method for manufacturing the above-mentioned form, for example, the following method can be cited: a method of laminating a porous substrate on a polymer electrolyte solution coated on a film-forming substrate and impregnating the porous substrate; and a method of further coating a polymer electrolyte solution on a porous substrate impregnated with the polymer electrolyte solution by the above method and drying the porous substrate.
[0086] In addition, as a polymer electrolyte, a polymer electrolyte in which an ionic group and a cation of an alkali metal or an alkaline earth metal form a salt state can also be used. In this case, it is preferred that after forming the first layer on the film-forming substrate, an acid treatment is implemented to exchange the cation of the alkali metal or the alkaline earth metal with a proton. Here, the acid treatment can be performed by a known method.
[0087] The electrolyte membrane of the present invention can be conveniently produced by laminating the second layer on the first layer. As a lamination method, a spraying method, a coating method or a transfer method can be adopted.
[0088] The blowing method is a method of blowing carbon particles onto the first layer using a nozzle or the like to form and stack the second layer. After the second layer is formed on the first layer, hot pressing is preferably performed to improve adhesion. In addition, by blowing carbon particles onto the first layer before the first layer is completely dried during the manufacturing process of the first layer, the adhesion between the first layer and the second layer can be improved.
[0089] The coating method is a method of coating a coating liquid for forming a second layer on a first layer formed on a film-forming substrate and drying the coating liquid to form a second layer. The transfer method is a method of transferring the second layer onto the first layer by heating and pressing a transfer sheet obtained by laminating the second layer on a transfer substrate and the first layer formed on a film-forming substrate. In the case of the coating method or the transfer method, the second layer preferably contains the above-mentioned binder.
[0090] [electrode]
[0091] The anode and cathode are each composed of components that can be used to form electrodes. The components that can be used to form electrodes are not particularly limited, and materials and structures known in the art can be used. For example, a layered structure obtained by stacking a catalyst layer on an electrode substrate composed of a conductive material, and an electrode substrate loaded with a catalyst can be cited. It should be noted that a more specific mode of the catalyst layer and the electrode substrate is described later. In addition, as a catalyst when loaded on an electrode substrate, catalyst particles used in the catalyst layer described later can be used. Among them, a layered structure of an electrode substrate and a catalyst layer is preferably formed. When the electrode adopts this layered structure, in the water electrolysis unit, when viewed from the electrode substrate, the catalyst layer can be arranged on the side opposite to the electrolyte membrane side, or it can be arranged on the electrolyte membrane side, but the catalyst layer is preferably configured on the electrolyte membrane side.
[0092] It should be noted that the catalyst layer may also be provided on the electrolyte membrane. Hereinafter, an electrode provided with a catalyst layer is sometimes referred to as an "electrode with a catalyst layer", and an electrolyte membrane provided with a catalyst layer is sometimes referred to as an "electrolyte membrane with a catalyst layer (CCM)". The catalyst layer may be laminated on an electrode substrate or an electrolyte membrane by a known coating method or transfer method.
[0093] [Electrode substrate]
[0094] The electrode substrate (which sometimes also serves as a gas diffusion layer) is mainly used for the application of voltage and is made of a conductive material. For example, a porous substrate such as metal or carbon can be used. Examples of the metal porous substrate include metal nonwoven fabrics, metal fiber sintered bodies, metal powder sintered bodies, and metal foam sintered bodies. Examples of the carbon porous substrate include carbon felt, carbon paper, carbon cloth, and graphite particle sintered bodies.
[0095] As the electrode substrate constituting the anode, a metal porous substrate is preferably used, which has a high potential and excellent corrosion resistance in the presence of oxygen, strong acidity, etc. As the metal constituting the metal porous substrate, from the above viewpoints, titanium, aluminum, nickel, stainless steel and alloys with at least one metal therein as the main component are preferred, and titanium and alloys with titanium as the main component are particularly preferred.
[0096] As the electrode substrate constituting the cathode, a carbon porous substrate is preferred, and carbon paper is particularly preferred, from the viewpoint of material cost and conductivity.
[0097] [Catalyst layer]
[0098] Catalyst layer is generally a layer comprising catalyst particles and polymer electrolyte. As catalyst particles, metals such as platinum group elements (platinum, ruthenium, rhodium, palladium, osmium, iridium), iron, lead, gold, silver, copper, chromium, cobalt, nickel, manganese, vanadium, molybdenum, gallium, aluminum or their alloys or oxides, composite oxides etc. can be usually used, in addition, carbon particles (carbon particles carrying catalyst metals) loaded with the above-mentioned catalyst metals can also be used. As the above-mentioned carbon particles, as long as it is particulate and has electrical conductivity, will not be corroded, degraded carbon particles due to the reaction with the catalyst, then it is not particularly limited, but carbon black, graphite, activated carbon, carbon fiber, carbon nanotubes and fullerene particles can be preferably used.
[0099] Examples of the polymer electrolyte include the fluorine-based polymer electrolytes and hydrocarbon-based polymer electrolytes described above. From the viewpoint of gas diffusibility and chemical durability, the polymer electrolyte of the catalyst layer is preferably a fluorine-based polymer electrolyte, and more preferably a perfluorocarbon sulfonic acid-based polymer.
[0100] The mass ratio of the content of the catalyst particles to the content of the polymer electrolyte in the catalyst layer (catalyst particles / polymer electrolyte) is usually in the range of 1-15, and preferably in the range of 1.5-13.
[0101] The catalyst layer provided in the cathode (sometimes referred to as a “cathode catalyst layer”) and the catalyst layer provided in the anode (sometimes referred to as an “anode catalyst layer”) may be composed of the same material or different materials.
[0102] The cathode catalyst layer may be any catalyst as long as it is a catalyst particle that generates hydrogen gas using protons as a raw material, and preferably contains a platinum catalyst, and particularly preferably uses carbon particles carrying platinum.
[0103] The anode catalyst layer can be any catalyst that generates oxygen from water as a raw material as catalyst particles, preferably using noble metals such as iridium, ruthenium, rhodium, palladium or their oxides, and particularly preferably iridium oxide. At this time, the catalyst particles can be independent particles or can be supported on titanium oxide or the like.
[0104] [Membrane Electrode Assembly (MEA)]
[0105] The electrodes constituting the anode and cathode can be integrated with the electrolyte membrane. The object obtained by integrating the electrode and the electrolyte membrane is called a "membrane electrode assembly (MEA)". As the form of the membrane electrode assembly, there can be cited a membrane electrode assembly obtained by stacking an electrode substrate on an electrolyte membrane with a catalyst layer (CCM) and a membrane electrode assembly obtained by stacking an electrode with a catalyst layer on an electrolyte membrane.
[0106] The membrane electrode assembly may be one in which the electrolyte membrane and the electrode are pre-bonded, or one in which the electrolyte membrane and the electrode are arranged one by one in the cell and then bonded by a fastening process.
[0107] The membrane electrode assembly suitable for use in the present invention is preferably a structure of "anode electrode substrate / anode catalyst layer / electrolyte membrane / cathode catalyst layer / cathode electrode substrate". In the above structure, it is more preferable to use an electrolyte membrane with a catalyst layer in which the anode catalyst layer and the cathode catalyst layer are each stacked on the electrolyte membrane. In addition, in the above structure, the cathode catalyst layer is arranged on the second layer side of the electrolyte membrane, but it is preferred that the second layer and the cathode catalyst layer are arranged in abutting manner.
[0108] [Catalyst layer electrolyte membrane (CCM)]
[0109] As described above, the catalyst layer-carrying electrolyte membrane is obtained by laminating the anode catalyst layer on the first layer side of the electrolyte membrane and laminating the cathode catalyst layer on the second layer side of the electrolyte membrane.
[0110] Examples of a method for stacking the catalyst layer on the electrolyte membrane include a coating method, a transfer method, or a method using both a coating method and a transfer method. These methods are not particularly limited, and a known method can be used.
[0111] As a coating method, a known coating method can be used to apply a coating liquid for a catalyst layer on the electrolyte membrane. Specifically, the following method can be cited: a coating liquid for a cathode catalyst layer is applied on the second layer side of the electrolyte membrane, and dried to form a cathode catalyst layer, and an anode catalyst layer is applied on the first layer side of the electrolyte membrane. The anode catalyst layer is dried to form an anode catalyst layer. The stacking order of the cathode catalyst layer and the anode catalyst layer can also be opposite to the above order. In the case of adopting a coating method, it is preferred to pre-stack a membrane substrate or a support on the surface of the electrolyte membrane opposite to the surface coated with the catalyst layer coating liquid.
[0112] As a transfer method, the following method can be cited: prepare a cathode catalyst layer transfer sheet obtained by stacking a cathode catalyst layer on a transfer substrate, and an anode catalyst layer transfer sheet obtained by stacking an anode catalyst layer on a transfer substrate, respectively, adhere the cathode catalyst layer transfer sheet to the second layer side of the electrolyte membrane, and adhere the anode catalyst layer transfer sheet to the first layer side of the electrolyte membrane, and heat and pressurize them.
[0113] The combination of the coating method and the transfer method may be as follows: first, a cathode catalyst layer coating liquid is coated on the second layer side of the electrolyte membrane, and dried to form the cathode catalyst layer, and an anode catalyst layer transfer sheet is attached to the opposite side of the electrolyte membrane, and heated and pressed to transfer the anode catalyst layer. Conversely to the above, a method of coating the anode catalyst layer coating liquid and then transferring the cathode catalyst layer may be used.
[0114] In addition, in the manufacturing process of the electrolyte membrane with a catalyst layer, a method of laminating the second layer of the electrolyte membrane and the cathode catalyst layer together on the first layer of the electrolyte membrane may be adopted. As such a method, for example, the following method may be mentioned: the first layer formed on the film-forming substrate and the transfer sheet obtained by laminating the cathode catalyst layer and the second layer in sequence on the transfer substrate are heated and pressurized, and the second layer and the cathode catalyst layer are simultaneously laminated on the first layer.
[0115] [Water electrolysis unit and water electrolysis device]
[0116] The water electrolysis unit of the present invention is a water electrolysis unit whose interior is divided into an anode and a cathode by an electrolyte membrane, that is, a water electrolysis unit in which an electrode as an anode and an electrode as a cathode are separated by an electrolyte membrane, and the electrolyte membrane has a first layer containing a polymer electrolyte and a second layer containing carbon particles, and the second layer is arranged on the cathode side. It should be noted that the details of the first layer and the second layer are as described above. In addition, the anode and the cathode can also preferably adopt the structure described in detail above.
[0117] A typical example of the water electrolysis unit of the present invention adopts the above Figure 1 The electrolytic cells shown are constructed in the same manner. Figure 1 The "electrolysis unit" described in is synonymous with the "water electrolysis unit", and therefore, it is described here as the "water electrolysis unit".
[0118] That is, in the water electrolysis unit of the present invention, the electrolyte membrane 10 is arranged between the anode 20 and the cathode 30, and the inside thereof is divided. Figure 1 In the example, the structure is such that they are clamped from both sides by diaphragms 41 and 42. The electrolyte membrane 10 includes a first layer 11 and a second layer 12, and the second layer 12 is arranged on the cathode 30 side of the first layer 11. In addition, in the water electrolysis device of the present invention, a power supply (not shown) is connected to the anode 20 and the cathode 30, and a voltage is applied. In addition, the generally known water electrolysis device includes a water supply part that supplies water to the water electrolysis unit, a power supply part that supplies power to the water electrolysis unit, an oxygen discharge part that discharges the generated oxygen, a hydrogen discharge part that discharges the generated hydrogen, and a water discharge part that discharges the excess water after electrolysis as basic components. The water electrolysis device involved in the embodiment of the present invention may also have the above-mentioned basic components.
[0119] Example
[0120] Hereinafter, the present invention will be described in more detail using examples, but the present invention is not limited thereto. It should be noted that various measurement conditions are as follows.
[0121] [Example 1]
[0122] [Synthesis of polyetherketone-based block copolymer b1]
[0123] [Synthesis example 1]
[0124] (Synthesis of 2,2-bis(4-hydroxyphenyl)-1,3-dioxolane (K-DHBP) represented by the following chemical formula (G1))
[0125] Into a 500 mL flask equipped with a stirrer, a thermometer and a distillation tube, 49.5 g of 4,4'-dihydroxybenzophenone, 134 g of ethylene glycol, 96.9 g of trimethyl orthoformate and 0.50 g of p-toluenesulfonic acid monohydrate were added and dissolved. Then, the mixture was stirred at 78-82°C for 2 hours. The internal temperature was further slowly raised to 120°C, and the distillation of methyl formate, methanol and trimethyl orthoformate was completely stopped. After the reaction solution was cooled to room temperature, the reaction solution was diluted with ethyl acetate, the organic layer was washed with 100 mL of 5% potassium carbonate aqueous solution, and the solvent was distilled off after separation. 80 mL of dichloromethane was added to the residue to precipitate crystals, which were filtered and dried to obtain 52.0 g of 2,2-bis(4-hydroxyphenyl)-1,3-dioxolane represented by the following chemical formula (G1). The crystals were subjected to GC analysis, and the results showed 99.9% of 2,2-bis(4-hydroxyphenyl)-1,3-dioxolane and 0.1% of 4,4'-dihydroxybenzophenone. The purity was 99.9%.
[0126]
[0127] [Synthesis example 2]
[0128] (Synthesis of 3,3'-sodium disulfonate-4,4'-difluorobenzophenone represented by the following chemical formula (G2))
[0129] 109.1 g of 4,4'-difluorobenzophenone (Sigmar Drizzle Japan reagent) was reacted in 150 mL of fuming sulfuric acid (50% SO3) (Fuji Film Wako Pure Chemical Industries, Ltd. reagent) at 100°C for 10 hours. Then, a large amount of water was added little by little, and after neutralization with sodium hydroxide, 200 g of salt (NaCl) was added to precipitate the synthetic product. The obtained precipitate was filtered out and recrystallized with an ethanol aqueous solution to obtain 3,3'-sodium disulfonate-4,4'-difluorobenzophenone represented by the following chemical formula (G2). The purity was 99.3%.
[0130]
[0131] [Synthesis example 3]
[0132] (Synthesis of nonionic oligomer a1 represented by the following general formula (G3))
[0133] In a 2,000 mL SUS polymerization apparatus equipped with a stirrer, a nitrogen inlet tube, and a Dean-Stark water separator, 16.59 g of potassium carbonate (Aldrich reagent, 120 mmol), 25.83 g (100 mmol) of K-DHBP obtained in Synthesis Example 1, and 20.3 g of 4,4'-difluorobenzophenone (Aldrich reagent, 93 mmol) were placed. After nitrogen substitution, 300 mL of N-methylpyrrolidone (NMP) and 100 mL of toluene were added, and after dehydration at 150°C, the temperature was raised to remove toluene, and polymerization was carried out at 170°C for 3 hours. Reprecipitation and purification were carried out using a large amount of methanol to obtain a terminal hydroxyl body of nonionic oligomer a1. The number average molecular weight of the terminal hydroxyl body of the nonionic oligomer a1 is 10,000.
[0134] In a 500 mL three-necked flask equipped with a stirrer, a nitrogen inlet tube, and a Dean-Stark water trap, 1.1 g of potassium carbonate (Sigma Aldrich Japan (same) reagent, 8 mmol) and 20.0 g (2 mmol) of the terminal hydroxyl body of the above nonionic oligomer a1 were placed. After nitrogen substitution in the apparatus, 100 mL of NMP and 30 mL of toluene were added, and after dehydration at 100°C, the temperature was raised to remove the toluene. Further, 2.2 g of hexafluorobenzene (Sigma Aldrich Japan (same) reagent, 12 mmol) was added, and the reaction was carried out at 105°C for 12 hours. Reprecipitation and purification were carried out using a large amount of isopropanol to obtain the nonionic oligomer a1 (terminal: fluorine group) represented by the following general formula (G3). The number average molecular weight was 11,000.
[0135]
[0136] [Synthesis Example 4]
[0137] (Synthesis of Ionic Oligomer a2 Represented by the Following General Formula (G4))
[0138] In a 2,000 mL SUS polymerization apparatus equipped with a stirrer, a nitrogen inlet tube, and a Dean-Stark water trap, 27.6 g of potassium carbonate (Sigma Aldrich Japan (the same) reagent, 200 mmol), 12.9 g (50 mmol) of K-DHBP obtained in Synthesis Example 1, 9.3 g (Sigma Aldrich Japan (the same) reagent, 50 mmol), 39.3 g (93 mmol) of 3,3'-sodium disulfonate-4,4'-difluorobenzophenone obtained in Synthesis Example 2, and 17.9 g of 18-crown ether-6 (Fuji Fluum Wako Pure Chemical Industries, Ltd., 82 mmol) were charged, and after nitrogen substitution, NMP was added. 300mL and 100mL toluene were added, dehydrated at 150°C, heated to remove toluene, and polymerized at 170°C for 6 hours. Reprecipitation and purification were performed using a large amount of isopropanol to obtain an ionic oligomer a2 (terminal: hydroxyl group) represented by the following general formula (G4). The number average molecular weight is 16,000. It should be noted that in the general formula (G4), M represents a hydrogen atom, Na or K.
[0139]
[0140] (Synthesis of polyetherketone-based block copolymer b1)
[0141] In a 2,000 mL SUS polymerization apparatus equipped with a stirrer, a nitrogen inlet tube, and a Dean-Stark water separator, 16 g of ionic oligomer a2 and 11 g of nonionic oligomer a1 were charged, NMP was added so that the total amount of oligomers charged was 7 wt%, and the reaction was carried out at 105°C for 24 hours.
[0142] Reprecipitation was performed in a large amount of isopropanol / NMP mixed solution (mass ratio 2 / 1), the obtained precipitate was recovered by filtration, and washed with a large amount of isopropanol blocking agent (block) to obtain block copolymer C1. The weight average molecular weight of the polyetherketone-based block copolymer b1 was 340,000, and the ion exchange capacity (IEC) was 2.1 meq / g.
[0143] [Production of Electrolyte Membrane]
[0144] [Creation of the first layer]
[0145] The PET film "LumiLa" (registered trademark) 125T60 manufactured by Toray Co., Ltd. was attached to a SUS plate and fixed using "Kaputon" (registered trademark) tape. The polyetherketone block copolymer b1 synthesized above was dissolved in NMP, filtered under pressure using a 1 μm polypropylene filter, and the prepared solution (solution P1, concentration of 13% by mass) was cast on the above PET film and dried to obtain a film-like polymer film. It was further immersed in a 10% by mass sulfuric acid aqueous solution at 80°C for 24 hours, subjected to proton substitution and deprotection reactions, and then immersed in a large excess of pure water for 24 hours, and washed thoroughly to obtain the first layer. The thickness of the first layer was 90 μm.
[0146] [Layer 2 stacking]
[0147] The coating liquid for the second layer described below was cast on the first layer and dried to laminate the second layer on the first layer. The thickness of the second layer was 10 μm.
[0148] [Preparation of coating liquid for the second layer]
[0149] Carbon particles: 10 parts by mass of carbon black (VULCAN (registered trademark) XC72 manufactured by Cabot Corporation)
[0150] Binder: 9 parts by mass of a fluorine-based polymer electrolyte ("Nafion" (registered trademark) manufactured by Chemours Co., Ltd., product number D2020) in terms of solid content
[0151] Solvent: A mixed solvent of water and 1-propanol with a mass ratio of 4:6
[0152] The carbon particles and polymer electrolyte were dispersed in a solvent using a bead mill to prepare a coating solution having a solid content concentration of 10% by mass. The ratio (I / C) of the mass of the polymer electrolyte (I) to the mass of the carbon particles (C) in the coating solution was 0.9.
[0153] [Fabrication of Electrolyte Membrane with Catalyst Layer]
[0154] The cathode catalyst layer described below was stacked on the second layer side of the electrolyte membrane prepared above, and the anode catalyst layer described below was stacked on the first layer side to prepare an electrolyte membrane with catalyst layers. The dry thickness of the cathode catalyst layer and the anode catalyst layer was 11 μm each.
[0155] <Cathode Catalyst Layer>
[0156] As the total solid components, a catalyst layer comprising 10 parts by mass of catalyst particles (carbon particles TEC10E50E (platinum loading rate 50% by mass) manufactured by Tanaka Kikinzoku Kogyo Co., Ltd. loaded with a platinum catalyst) and 5 parts by mass of a fluorine-based polymer electrolyte ("Nafion" (registered trademark) manufactured by Chemizer Co., Ltd., product number D2020).
[0157] <Anode Catalyst Layer>
[0158] As the total solid content, the catalyst layer includes 10 parts by mass of catalyst particles (IrO2 Catalyst Elyst Ir750480 (Ir content: 75%) manufactured by Umicore Co., Ltd.) and 1.3 parts by mass of a fluorine-based polymer electrolyte ("Nafion" (registered trademark) product number D2020 manufactured by Chemizer Co., Ltd.).
[0159] [Fabrication of membrane electrode assembly]
[0160] On the cathode catalyst layer side of the electrolyte membrane with a catalyst layer produced above, a commercially available gas diffusion electrode 24BCH manufactured by SGL is stacked as a cathode also serving as a gas diffusion layer, and a commercially available porous titanium sintered body plate is stacked as an anode also serving as a gas diffusion layer, thereby producing a membrane electrode assembly.
[0161] [Water electrolysis method]
[0162] The membrane electrode assembly prepared above was placed in a JARI standard unit "Ex-1" (electrode area 25 cm 2 ) and the cell temperature was set to 50°C. Deionized water with a conductivity of 1 μS / cm or less was supplied to both the anode and cathode at a flow rate of 0.2 L / min under atmospheric pressure and a current density of 1.0 A / cm 2 A voltage was applied in a manner of , and water electrolysis was performed for 2,000 hours (in Table 1, water electrolysis method 1).
[0163] [Comparative Example 1]
[0164] In Example 1, except that the second layer was not laminated, the electrolyte membrane, the electrolyte membrane with a catalyst layer, and the membrane electrode assembly were produced in the same manner as in Example 1, and water electrolysis was carried out in the same manner as in Example 1.
[0165] [Example 2 and Comparative Example 2]
[0166] In the water electrolysis methods of Example 1 and Comparative Example 1, water electrolysis was performed by supplying only deionized water to the anode (water electrolysis method 2 in Table 1), and water electrolysis was performed in the same manner. Example 2 corresponds to Example 1, and Comparative Example 2 corresponds to Comparative Example 1.
[0167] [Example 3]
[0168] In Example 1, the first layer was changed to a fluorine-based polymer electrolyte layer ("Nafion" (registered trademark) Nafion115 manufactured by Chemours Co., Ltd.: thickness of 125 μm). Otherwise, the same operations were performed as in Example 1 to prepare an electrolyte membrane, an electrolyte membrane with a catalyst layer, and a membrane electrode assembly, and water electrolysis was carried out in the same manner as in Example 1 (water electrolysis method 1 in Table 2).
[0169] [Comparative Example 3]
[0170] In Example 3, except that the second layer was not laminated, the electrolyte membrane, the electrolyte membrane with a catalyst layer, and the membrane electrode assembly were produced in the same manner as in Example 3, and water electrolysis was carried out in the same manner as in Example 1.
[0171] [Example 4 and Comparative Example 4]
[0172] In the water electrolysis methods of Example 3 and Comparative Example 3, only deionized water was supplied to the anode to perform water electrolysis (water electrolysis method 2 in Table 2), and water electrolysis was performed in the same manner. Example 4 corresponds to Example 3, and Comparative Example 4 corresponds to Comparative Example 3, respectively.
[0173] [evaluate]
[0174] For the above-mentioned Examples and Comparative Examples, the applied voltage and the average voltage at electrolysis times of 0 hours, 500 hours, 1,000 hours, and 2,000 hours are shown in Tables 1 and 2. In addition, the relationship between the electrolysis time and the applied voltage is shown in Figure 2 and Figure 3 In the table, water electrolysis method 1 is a method of supplying water to both the anode and the cathode, water electrolysis method 2 is a method of water electrolysis in which water is supplied only to the anode, the applied voltage at the electrolysis time "0 hours" indicates the initial applied voltage, the average applied voltage indicates the average value of the applied voltage every 25 hours from 0 hours to 2000 hours, and the voltage rise rate indicates the voltage rise rate after 2,000 hours calculated by the following formula 1.
[0175] Voltage rise rate (%) = (V1-V0) / V0×100···Formula 1
[0176] In the formula, V1 represents the applied voltage after 2,000 hours, and V0 represents the initial applied voltage.
[0177] The lower the average applied voltage is, the higher the electrolysis efficiency is, and the lower the voltage increase rate is, the better the durability is (the electrolysis efficiency can be maintained).
[0178] [Table 1]
[0179]
[0180] [Table 2]
[0181]
[0182] From Table 1, Table 2 and Figure 2 , Figure 3 It is found that the water electrolysis method of the present invention using the electrolyte membrane in which the second layer is stacked on the first layer has a smaller voltage increase rate and is superior in durability compared to the water electrolysis method of the comparative example using the electrolyte membrane in which the second layer is not stacked.
[0183] It is also found that the water electrolysis method 2 (supplying water only to the anode) has a smaller voltage increase rate and is superior in durability compared to the water electrolysis method 1 (supplying water to both the anode and the cathode).
[0184] In addition, Figure 4 The relationship between the electrolysis time and the applied voltage of Examples 1 to 4 is shown in FIG. Compared with Examples 3 and 4 (Nafion 115), Examples 1 and 2 (block copolymer b1) can maintain high electrolysis efficiency by applying a low voltage for 2,000 hours. That is, Figure 4 It was shown that the membrane using a hydrocarbon-based polymer electrolyte as the first layer can maintain high electrolysis efficiency for a long period of time compared to the membrane using a fluorine-based polymer electrolyte as the first layer.
[0185] Description of Reference Numerals
[0186] 1 electrolysis unit
[0187] 10Electrolyte membrane
[0188] 11 Layer 1
[0189] 12 Layer 2
[0190] 20 Anode
[0191] 30 cathode
[0192] 41, 42 diaphragm
Claims
1. A water electrolysis method, wherein water is supplied to an electrolysis unit which is internally divided into an anode and a cathode by an electrolyte membrane and electrolyzed, thereby generating oxygen at the anode and hydrogen at the cathode, respectively, wherein the electrolyte membrane comprises a first layer and a second layer, wherein the first layer contains a polymer electrolyte, and the second layer is located on the cathode side of the first layer and contains carbon particles. 2 . The water electrolysis method according to claim 1 , wherein all or part of the carbon particles contained in the second layer are carbon particles that do not support a catalyst metal. The water electrolysis method according to claim 1 or 2, wherein the second layer contains a binder. 4 . The water electrolysis method according to claim 3 , wherein all or part of the binder contained in the second layer is a fluorine-based polymer electrolyte. 5 . The water electrolysis method according to claim 1 , wherein the first layer has a thickness of 40 μm or more and 250 μm or less. 6 . The water electrolysis method according to claim 1 , wherein a ratio of a thickness T2 of the second layer to a thickness T1 of the first layer (ie, T2 / T1 ) is 0.03 to 0.
30. 7 . The water electrolysis method according to claim 1 , wherein all or part of the polymer electrolyte contained in the first layer is a hydrocarbon-based polymer electrolyte. 8 . The water electrolysis method according to claim 1 , wherein each of the anode and the cathode comprises a catalyst layer and an electrode substrate in this order from the electrolyte membrane side. 9 . The water electrolysis method according to claim 8 , wherein the catalyst layer constituting the cathode contains a platinum catalyst. 10 . The water electrolysis method according to claim 8 , wherein the second layer of the electrolyte membrane is arranged in contact with the catalyst layer of the cathode. 11 . The water electrolysis method according to claim 1 , wherein water is supplied to the electrolysis unit at least to the anode.
12. A water electrolysis unit, which is a water electrolysis unit whose interior is divided into an anode and a cathode by an electrolyte membrane, wherein the electrolyte membrane has a first layer and a second layer, the first layer contains a polymer electrolyte, and the second layer is located on the cathode side of the first layer and contains carbon particles.
13. A water electrolysis device comprising the water electrolysis unit according to claim 12.