Cobalt-zinc alloy catalyst material with adjustable surface microenvironment and preparation method thereof

The cobalt-zinc alloy catalyst was screened through the sulfur competition adsorption factor fsulfur, and the catalyst surface microenvironment was adjusted, which solved the problems of slow sulfur conversion kinetics and catalyst deactivation in lithium-sulfur batteries, achieving high energy density and long cycle stability.

CN118899442APending Publication Date: 2024-11-05TIANJIN UNIV +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410923401.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-10
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The conversion kinetics of sulfur positive electrodes in lithium-sulfur batteries are slow, and the existing catalysts lead to passivation and inactivation of the catalytic surface due to excessive sulfur adsorption, which limits the sulfur conversion rate.

Method used

A sulfur competition adsorption factor fsulfur is proposed to screen suitable cobalt-zinc alloy catalysts. By adjusting the catalyst surface microenvironment, it inhibits sulfurization inactivation and induces lithium sulfide to deposition in three-dimensional mode, thereby increasing battery capacity.

Benefits of technology

The polarization state was maintained during the 1000 cycle, achieving an ultra-high energy density of 464Wh/kg, significantly improving the performance of the lithium-sulfur battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118899442A_ABST
    Figure CN118899442A_ABST
Patent Text Reader

Abstract

The invention relates to a cobalt-zinc alloy catalyst material with an adjustable surface microenvironment. Cobalt-zinc alloy is loaded on a carbon material in a single-phase in-situ manner; under the same system, the fsufu value of the catalyst in which single cobalt metal is loaded on the carbon material in situ is taken as a reference value, and the fsufu value of the cobalt-zinc alloy catalyst material is 40%-90% of the reference value; and in the fsulfurr: # imgabs0 #, Cdl and Cdl and S are electric double layer capacitance values before and after sulfur is added into the electrolyte respectively. The cobalt-zinc alloy catalytic material with an adjustable catalyst surface microenvironment is constructed by utilizing p-d orbital hybridization state difference between transition metal and solvent molecules or sulfur species, and optimal balance of catalytic surface sulfur-solvent adsorption is realized in combination with a sulfur adsorption factor fsulfur.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of battery technology, and in particular to a sulfur competitive adsorption factor and its application in the screening of lithium-sulfur battery catalysts, as well as the screened catalyst and a lithium-sulfur battery using the catalyst and a positive electrode thereof. Background Art

[0002] Lithium-sulfur battery is a type of lithium battery that uses sulfur as the positive electrode and metallic lithium as the negative electrode. Elemental sulfur is abundant in the earth and has the characteristics of low price and environmental friendliness. Lithium-sulfur battery using sulfur as the positive electrode material has a high material theoretical specific capacity and battery theoretical specific energy, reaching 1675mAh / g and 2600Wh / kg respectively, which is much higher than the capacity of lithium cobalt oxide battery widely used in commercial applications (<150mAh / g). Its electrode reaction is easier to control than lithium-air battery, and it is a new battery technology with great practical potential.

[0003] However, in lithium-sulfur batteries, there is a problem of slow conversion kinetics on the sulfur cathode side. The introduction of catalysts has become a major research direction. Catalysis can combine the adsorption process and the catalytic conversion process to more effectively capture LiPSs on the one hand and promote the conversion of sulfur species on the other. Existing catalysts used in lithium-sulfur batteries often cause rapid catalytic surface passivation and deactivation due to excessive sulfur adsorption, which greatly limits the sulfur conversion rate.

[0004] To this end, this application is filed. Summary of the invention

[0005] In view of the above-mentioned problems in the prior art, the present invention starts from the mechanism characteristics of the sulfur species conversion reaction in the lithium-sulfur battery, combines the influence of the competitive adsorption of sulfur and solvent molecules on the catalyst surface on the medium transfer diffusion and mass transfer, and the influence of the difference in orbital hybridization state between catalyst metals on the change of the catalyst surface microenvironment, reveals the relationship between the competitive adsorption of sulfur on the surface of the lithium-sulfur battery and the coordination between the catalyst metals, and proposes a sulfur competitive adsorption factor that can be used in the lithium-sulfur battery. The sulfur competitive adsorption factor can be used for the optimization screening of lithium-sulfur battery catalysts. The screened catalyst is applied to the lithium-sulfur battery to suppress the sulfurization deactivation of the catalyst surface while inducing the deposition of lithium sulfide in a three-dimensional mode, thereby greatly improving the capacity of the lithium-sulfur battery under lean liquid conditions.

[0006] In a first aspect, the present invention provides a sulfur competitive adsorption factor f for describing the sulfur competitive adsorption capacity of the catalyst surface in a lithium-sulfur battery. sulfur :

[0007]

[0008] Among them, C dl and C dl,SThey are the double layer capacitance values ​​before and after adding sulfur into the electrolyte.

[0009] In some embodiments, the C dl and C dl,S It is measured in a lithium-sulfur battery with a salt concentration greater than 0.5 mol / L and a voltage greater than 1 V. It is further preferably measured in a lithium-sulfur battery with a salt concentration of 0.5-2 mol / L and a voltage of 2-3 V.

[0010] In some embodiments, the concentration of sulfur added to the electrolyte is 1-10 mM, preferably 3-5 mM.

[0011] In a second aspect, the present invention provides a method for using the sulfur competitive adsorption factor f sulfur Application in catalyst screening for lithium-sulfur batteries.

[0012] In some embodiments, the specific application method in the screening is to use the metal catalyst with the strongest sulfur adsorption under the same system. sulfur As the benchmark value, filter out f sulfur The value is an alloy catalyst at an atomic ratio of 40% to 90% of the reference value.

[0013] In some embodiments, the selected alloy catalyst is f sulfur The value is an alloy catalyst at an atomic ratio of 60% to 80% of the reference value, and further 70% to 75%.

[0014] In a third aspect, the present invention provides a cobalt-zinc alloy catalyst material with adjustable surface microenvironment, wherein the cobalt-zinc alloy is in-situ loaded on a carbon material as a single phase.

[0015] In some embodiments, the catalyst f of a single cobalt metal in situ supported on a carbon material under the same system sulfur The value is a reference value, and the f sulfur The value is 60% to 80% of the standard value, and further 70% to 75%. sulfur It is the sulfur competitive adsorption factor described in the first aspect.

[0016] In some embodiments, in the cobalt-zinc alloy catalyst material, the Zn / Co atomic ratio is 0.5 to 2, preferably 1±0.2.

[0017] In some embodiments, in the cobalt-zinc alloy catalyst material, the carbon material includes one or more of graphene, carbon nanotubes, activated carbon, carbon aerogel, carbon nanofibers, porous carbon spheres, graphitized carbon, carbon nanowires, carbon nanosheets, and carbon composites, wherein the carbon composites include carbon / metal oxides and carbon / sulfides.

[0018] In some embodiments, in the cobalt-zinc alloy catalyst material, the ratio of carbon material to cobalt and zinc is 0.1 to 0.5 mmol in total of cobalt and zinc per 80 mg of graphene oxide, preferably 0.2 to 0.3 mmol in total of cobalt and zinc per 80 mg of graphene oxide.

[0019] In a fourth aspect, the present invention further provides a method for preparing the cobalt-zinc alloy catalyst material described in the third aspect, comprising the following steps: dispersing the carbon material, cobalt salt and zinc salt in a solvent according to a stoichiometric ratio, collecting and drying the product after condensation and reflux, and then heating and reducing it under an inert atmosphere to obtain the catalyst.

[0020] In some embodiments, the concentration of the carbon material in the solvent is 0.5-2 mg / mL.

[0021] In some embodiments, the solvent is isopropanol.

[0022] In some embodiments, the condensation reflux is carried out at a temperature of 70-90°C.

[0023] In some embodiments, the temperature of the heating reduction is 280-320° C., and the heating time is more than 1 hour, preferably 2-48 hours.

[0024] In some embodiments, after the heating reduction, the microwave reaction is further performed at a power of 800-1200 W for 2-10 min.

[0025] In a fifth aspect, the present invention further provides a lithium-sulfur battery positive electrode, comprising the cobalt-zinc alloy catalyst material and a sulfur source as described in the third aspect, wherein the mass ratio of sulfur (S8) that can be provided by the cobalt-zinc alloy catalyst material and the sulfur source is 1:(2 to 2.5).

[0026] In some embodiments, the sulfur source includes elemental sulfur, lithium polysulfide, lithium sulfide, sulfur-containing organic polymers (sulfurized polyacrylonitrile), metal sulfides (such as copper sulfide, zinc sulfide, lead sulfide), selenium / tellurium-sulfur composite materials (such as sulfur selenide and sulfur telluride and their composites), preferably elemental sulfur.

[0027] In some schemes, a conductive agent and a binder are also included, and the mass proportion of the cobalt-zinc alloy catalyst material and the sulfur source in the positive electrode material is 60%-95%, the mass proportion of the conductive agent is 8%-15%, and the mass proportion of the binder is 3%-10%.

[0028] In some embodiments, the positive electrode loading is 1-7 mg / cm 2 , 5~6mg / cm 2 Better.

[0029] In some aspects, the conductive agent includes one or more of CNT, SP, GIN, CMK-3, mesoporous carbon, and carbon fiber.

[0030] In some aspects, the binder includes one or more of PVDF, CMC, SBR, sodium alginate or potassium alginate.

[0031] In some aspects, the current collector includes at least one or more of copper foil, aluminum foil, carbon-containing aluminum foil, stainless steel foil, carbon cloth, and carbon paper.

[0032] In a sixth aspect, the present invention further provides a lithium-sulfur battery, comprising the lithium-sulfur battery positive electrode and separator, a negative electrode, and an electrolyte as described in the fifth aspect.

[0033] In some embodiments, the electrolyte solvent is an ether or an ester; the ether solvent is one or more of 1,3-dioxolane, 1,4-dioxane, ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, and tetraethylene glycol dimethyl ether; the ester solvent is one or more of ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, and ethyl methyl carbonate; the lithium salt dissolved in the electrolyte is at least one of lithium bis(trifluoromethylsulfonyl)imide, lithium hexafluorophosphate, lithium bis(fluorosulfonyl)imide, and lithium nitrate.

[0034] In some embodiments, the ratio of electrolyte to sulfur in the battery is less than 4 μL / mg S , further less than 1.8μL / mg S . That is, it is in a lean state. Further, the ratio of electrolyte to sulfur in the battery is less than 4μL / mg S The initial capacity is not less than 1.5Ah; the ratio of electrolyte to sulfur in the battery is less than 1.8μL / mg S It has an energy density of over 464Wh / kg.

[0035] In some embodiments, the negative electrode is one of lithium metal and silicon-lithium alloy.

[0036] In some embodiments, the membrane is Celgard-2500.

[0037] Compared with the prior art, the present invention has at least the following beneficial effects:

[0038] The present invention draws on the theoretical model of double-layer structure to reveal and propose a quantitative parameter that can be used to describe the competitive adsorption intensity of sulfur species on the catalyst surface - the sulfur adsorption factor f sulfur . This provides a new approach for screening catalyst materials with suitable properties.

[0039] The present invention utilizes the difference in the pd orbital hybridization state between transition metals and solvent molecules or sulfur species to construct a cobalt-zinc alloy catalytic material with adjustable catalyst surface microenvironment, and combines the sulfur adsorption factor f sulfur , achieving an optimized balance of sulfur-solvent adsorption on the catalytic surface.

[0040] The present invention has a moderate f sulfur The moderately solvent-rich environment on the surface of the carbon-supported cobalt-zinc alloy catalyst not only helps to inhibit the poisoning and deactivation of active sites, but also can regulate the deposition behavior of lithium sulfide and induce the deposition of lithium sulfide in a three-dimensional high-capacity mode.

[0041] The lithium-sulfur battery and the positive electrode provided by the present invention, by adding the above-mentioned cobalt-zinc alloy catalyst, can maintain a low polarization state during the cycle of 1000 cycles, and the corresponding Ah-level lithium-sulfur soft-pack battery can maintain a low polarization state at a low concentration of 1.8 μL / mg. S An ultra-high energy density of 464Wh / kg is achieved at an E / S ratio of 1. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0043] Figure 1 Schematic diagram of the double layer structure described by the Gouy-Chapman-Stern model.

[0044] Figure 2 The effect of sulfur-solvent competitive adsorption on the catalytic reaction. A is a schematic diagram of the double-layer structure with appropriate competitive effect, and B is a schematic diagram of the double-layer structure destroyed by excessive sulfur adsorption.

[0045] Figure 3 is the sulfur adsorption factor f sulfur Reliability evaluation diagram. Among them, a is a schematic diagram of the compact layer structure when sulfur is adsorbed on the surface of sulfur-philic and solvent-philic catalysts; b is the f of catalyst materials with different atomic ratios sulfur Value; c is f sulfur and the relationship between Zn / Co atomic ratio.

[0046] Figure 4 HR-TEM photos of the catalysts obtained in Example 1 and Comparative Example 1 and the corresponding element distribution maps.

[0047] Among them, a is the lattice structure of G-Co, b is the TEM photo of G-Co, c is the Co element distribution map of G-Co, d is the C element distribution map of G-Co, e is the lattice structure of G-CoZn, f is the TEM photo of G-CoZn, g is the Co element distribution map of G-CoZn, and h is the Zn element distribution map of G-CoZn.

[0048] Figure 5CV curves and Tafel curves of the embodiments of the present invention and the comparative examples are shown in FIG.

[0049] Figure 6 For the present invention sulfur and reaction kinetics.

[0050] Figure 7 The cycle performance of G-CoZn in the embodiment of the present invention and the comparative examples G-Co and G at different rates. Among them, a is the cycle rate curve, b is the cycle performance at 1.0C, and c is the cycle performance at 2.0C.

[0051] Figure 8 The voltage-activation energy curves (a) of the lithium-sulfur batteries of Example G-CoZn of the present invention and Comparative Examples G-Co and G, and the Co 2p (b) and S2p XPS graphs (c) of the positive electrode after cycling.

[0052] Fig. 9 Dimensionless current-time curves (a) of G-CoZn of the present invention and comparative examples G-Co and G, and SEM photos of Li2S deposition on their surfaces (b).

[0053] Fig.10 The cycle performance of the G-CoZn soft pack battery in the example under the condition of poor electrolyte. Where a is the electrolyte / sulfur (E / S) ratio of 4 μL / mg S The lean solution condition, b is the electrolyte / sulfur (E / S) ratio of 1.8μL / mg S lean solution conditions.

[0054] Fig.11 This is the charge and discharge curve of the G-CoCu lithium-sulfur battery of Comparative Example 3 of the present invention. DETAILED DESCRIPTION

[0055] The embodiments of the present invention are only a part of the embodiments of the present application, rather than all the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present application.

[0056] The chemical raw materials involved in the embodiments of the present invention are all prior art and are commercially available. The experimental devices, test devices, etc. involved in the following embodiments and comparative examples are all conventional devices in the art, without special requirements and limitations.

[0057] The uncontrollable deposition and irreversible transformation of the insulating discharge product lithium sulfide in lithium-sulfur batteries are directly related to the influence of the microenvironment on the catalyst surface. The transformation of sulfur species occurs in the inner tight layer of the double-layer structure and follows the inner-sphere electron transfer mechanism. To this end, we refer to the theoretical model of the double-layer structure to describe the microenvironment on the catalyst surface.

[0058] The Gouy-Chapman-Stern (GCS) model is a theoretical model used to describe the double layer structure of the electrode-electrolyte interface. This model combines the characteristics of the Helmholtz model and the Gouy-Chapman model, and believes that the double layer consists of two parts: a compact layer (Helmholtz layer) close to the electrode surface and a diffusion layer (Gouy-Chapman layer) slightly away from the electrode surface. Figure 1 As shown, the electrode surface has a tight layer (Helmholtz layer) where the electrolyte molecules are tightly adsorbed, and far away from the electrode surface is a solvent environment where the electrolyte is fully solvated and dispersed. Between the tight layer and the solvation environment is a diffusion layer (Diffusion layer) where the electrolyte molecules are gradually dispersed. The GCS model satisfies the following formula:

[0059]

[0060] Among them, C dl is the double layer capacitance of the electrolyte, C Hl is the double layer capacitance of the compact layer, C diff is the double layer capacitance of the diffusion layer.

[0061] In lithium-sulfur batteries, the surface of the sulfur catalyst also has a double-layer structure that conforms to the GCS model through the competitive adsorption state of sulfur and solvent molecules, such as Figure 2 As shown. Under good competitive adsorption, the catalyst surface forms an inner tight layer by tightly adsorbing sulfur and solvent molecules. Away from the catalyst surface is a solvent environment where lithium polysulfide and salt anions are fully dispersed in the solvent. The middle is a diffusion layer (outer tight layer), as shown Figure 2 As shown in A. When there is too strong sulfur adsorption on the catalyst surface, excessive sulfur deposition on the catalyst surface will hinder the adsorption of solvent molecules as the mass transfer medium, affect the diffusion of polysulfides to the surface and the desorption and mass transfer of lithium sulfide, thereby changing the deposition behavior of lithium sulfide, destroying the double layer structure, and causing the catalyst surface to be passivated and deactivated. Therefore, the double layer capacitance value of the compact layer (C Hl ) is directly related to the competitive adsorption state of sulfur and solvent on the catalyst surface.

[0062] Considering the feasibility of measuring the double-layer capacitance, the GCS model is used in the microenvironment of lithium-sulfur batteries. When the salt concentration is greater than 0.5 mol / L and the voltage is greater than 1 V, the thickness of the diffusion layer in the double layer is greatly compressed. At this time, the double-layer capacitance of the diffusion layer (C diff ) can be ignored, and C dl ≈C Hl In lithium-sulfur batteries, the salt concentration is generally greater than 0.5 mol / L, and the voltage of lithium-sulfur batteries is generally above 2 V. The double-layer capacitance value (C dl ) and the double layer capacitance of the compact layer (C Hl ), the double-layer capacitance of the electrolyte (C dl ) can be used to quantitatively reveal the competitive adsorption of sulfur and solvent on the catalyst surface. Based on this law, we propose an experimental parameter that can be used to describe the competitive adsorption capacity of sulfur on the catalyst surface - the sulfur adsorption factor (f sulfur ):

[0063]

[0064] Among them, C dl and C dl,S These are the double layer capacitance values ​​before and after adding sulfur (S8) to the electrolyte.

[0065] This parameter can quantitatively describe and evaluate the changes in the microenvironment regulation of the catalyst surface, which is conducive to the selection of lithium-sulfur battery catalyst materials with an optimized balance of sulfur-solvent adsorption.

[0066] There are differences in the hybridization states of pd orbitals between transition metals and solvent molecules or sulfur species. Usually, the d orbitals of transition metal atoms and the p orbitals of ligands (such as solvent molecules or sulfur species) interact in energy and space. This interaction can lead to the redistribution of electron density, thereby affecting the stability, electronic structure and chemical properties of the compound. Different transition metals show different coordination numbers, symmetries, orbital directions and ligand field splitting energies, and their effects on sulfur-solvent competitive adsorption are also quite different. Through a large number of research and screening, it was found that cobalt-zinc alloy materials, through zinc (Zn) alloying, changed the electronic structure of cobalt (Co) metal, while enhancing the catalyst's adsorption capacity for solvent molecules, weakened its adsorption of sulfur species, and were able to construct a moderately solvent-rich inner compact layer structure. On the one hand, this structure effectively inhibits the catalytic surface passivation and deactivation caused by strong sulfur adsorption. On the other hand, the solvent-rich surface microenvironment also strengthens the diffusion and mass transfer of sulfur species, thereby inducing lithium sulfide to deposit in a high-capacity three-dimensional mode.

[0067] To this end, we also proposed a cobalt-zinc alloy catalyst material with adjustable surface microenvironment, in which the cobalt-zinc alloy is in situ supported on a carbon material as a single phase. The preparation method includes the following steps: dispersing the carbon material, cobalt salt and zinc salt in a solvent, collecting and drying the product after condensation and reflux, and then heating and reducing it under an inert atmosphere to obtain a carbon-supported cobalt-zinc alloy catalyst, i.e., the target product. During the preparation process, products with different alloy ratios can be obtained by adjusting the addition amount of cobalt salt and zinc salt.

[0068] The above catalyst material is used to prepare a lithium-sulfur battery, and a lithium-sulfur battery can be further provided. The preparation method includes: mixing the above cobalt-zinc alloy catalyst material with sulfur powder, melting sulfur under an inert atmosphere to obtain a sulfur-carbon composite positive electrode active material, and then mixing the sulfur-carbon composite positive electrode active material with a conductive agent and a binder to prepare a positive electrode slurry, coating the positive electrode slurry on a current collector to prepare a lithium-sulfur battery positive electrode sheet, and finally assembling the lithium-sulfur battery positive electrode sheet with a diaphragm, a negative electrode and an electrolyte to obtain a lithium-sulfur battery. The preparation process of the lithium-sulfur battery can follow the general lithium-sulfur battery preparation process and means.

[0069] To verify the sulfur adsorption factor (f sulfur ) can be used as a representative to prepare carbon-supported cobalt-zinc alloy catalysts with different alloy atomic ratios and their lithium-sulfur batteries, and observe f sulfur The results show that f sulfur The correlation between the Zn / Co atomic ratio and the catalyst was confirmed. sulfur The reliability and applicability of the sulfur competitive adsorption intensity descriptor. Figure 3 As shown, G-Co, G-CoZn-0.5, G-CoZn, G-CoZn-2 and G-CoZn-5 represent cobalt-zinc alloy catalyst materials containing no Zn and having Zn / Co atomic ratios of 0.5, 1, 2 and 5, respectively. The specific preparation method is shown in the examples. Figure 3 a shows the difference in the compact layer structure of sulfur adsorbed on the surface of sulfur-philic catalysts (such as G-Co) and solvent-philic catalysts (such as G-CoZn-n, n = 0.5, 1, 2, 5). By cyclic voltammetry, the curves of different scan rates were measured in the potential range of 3V to 3.05V, and the current density and scan rate at 3V potential were plotted to obtain the following: Figure 3 b, the slope of the straight line is the double-layer capacitance value. By comparing the double-layer capacitance values ​​before and after adding 4 mM S8 to the electrolyte, the f of the carbon-supported cobalt-zinc alloy catalyst can be evaluated. sulfur Values, such as Figure 3 b and Table 1. f sulfur The relationship between the value and the Zn / Co atomic ratio is as follows Figure 3 As shown in c.

[0070] Table 1

[0071] <![CDATA[C dl,S ]]> <![CDATA[C dl ]]> <![CDATA[f sulfur ]]> G-Co 8.39 13.06 0.358 G-CoZn-0.5 9.19 13.44 0.316 G-CoZn 9.81 13.23 0.259 G-CoZn-2 11.41 13.57 0.159 G-CoZn-5 11.65 12.88 0.096

[0072] The above results show that with moderate f sulfur The moderately solvent-rich environment on the surface of the catalyst (carbon-supported cobalt-zinc alloy catalyst) helps to inhibit the poisoning and deactivation of active sites, which is conducive to regulating the deposition behavior of lithium sulfide and inducing the deposition of lithium sulfide in a three-dimensional high-capacity mode. This effect greatly improves the active material utilization, rate performance and long-cycle stability of lithium-sulfur batteries.

[0073] In different systems, f sulfur The value of may change, but due to f sulfur It reflects the solvent-rich state of the catalyst surface and the competitive adsorption relationship between the solvent and sulfur. sulfur The trend of change is basically the same in different systems, and can be further screened by f sulfur The value of is used to optimize the suitable catalyst and its atomic ratio.

[0074] Considering that as a specific means to further screen catalyst materials with suitable performance, the f of metal catalysts (such as G-Co) with the strongest sulfur adsorption under the same system sulfur As the benchmark value, filter out f sulfur The alloy catalyst (such as G-CoZn-0.5, G-CoZn, G-CoZn-2) with an atomic ratio of 40% to 90% of the reference value can obtain an optimized catalyst material with moderate surface enrichment of solvent. sulfur The alloy catalyst (such as G-CoZn) with an atomic ratio of 60% to 80% of the baseline value and further 70% to 75% has a better surface solvent enrichment degree and can better balance the competitive adsorption state of sulfur-solvent and the kinetic reaction capacity.

[0075] As some exemplary preferred schemes, in the above-mentioned cobalt-zinc alloy catalyst material, the Zn / Co atomic ratio is 0.5 to 2, preferably 1±0.2.

[0076] As some exemplary preferred solutions, in the above-mentioned cobalt-zinc alloy catalyst material, the carbon material includes one or more of graphene, carbon nanotubes, activated carbon, carbon aerogel, carbon nanofiber, porous carbon sphere, graphitized carbon, carbon nanowire, carbon nanosheet, and carbon composite material, wherein the carbon composite material includes carbon / metal oxide, carbon / sulfide, etc., which can improve the electrochemical performance. In this case, graphene oxide is preferably used.

[0077] As some exemplary preferred schemes, the ratio of graphene oxide to cobalt and zinc is 0.1-0.5 mmol of cobalt and zinc per 80 mg of graphene oxide, preferably 0.2-0.3 mmol of cobalt and zinc per 80 mg of graphene oxide, so as to achieve a moderate loading amount and catalytic activity, while balancing the effect of the introduction of carbon materials on the conductivity of the system.

[0078] As some exemplary preferred solutions, during the preparation of the above cobalt-zinc alloy catalyst material, the concentration of the carbon material in the solvent is 0.5-2 mg / mL to promote full dispersion.

[0079] As some exemplary preferred schemes, in the preparation process of the above-mentioned cobalt-zinc alloy catalyst material, the choice of solvent is not particularly limited, as long as it is conducive to dissolving the carbon material and the metal salt and facilitating condensation and reflux, and isopropanol is preferred.

[0080] As some exemplary preferred solutions, during the preparation of the cobalt-zinc alloy catalyst material, condensation reflux can be performed under oil bath conditions, and the oil bath temperature is 70-90° C. Condensation reflux promotes the full combination of cobalt salt and zinc salt on the carbon material.

[0081] As some exemplary preferred schemes, during the preparation of the above-mentioned cobalt-zinc alloy catalyst material, the inert atmosphere may include one or more of argon and nitrogen.

[0082] As some exemplary preferred schemes, during the preparation of the above cobalt-zinc alloy catalyst material, the heating reduction temperature is 280-320° C., and the heating time is more than 1 hour, preferably 2-48 hours.

[0083] As some exemplary preferred schemes, in the preparation process of the above cobalt-zinc alloy catalyst material, microwave-assisted heating reduction is used to promote the reduction of cobalt salt and zinc salt on the surface of the carbon material. After heating reduction, a microwave reaction with a power of 800-1200W is used for 2-10min. Microwave-assisted heating reduction is conducive to promoting the rapid formation of cobalt-zinc alloy, is convenient and fast, and the yield can reach 40-50%.

[0084] As some exemplary preferred schemes, in the above-mentioned lithium-sulfur battery or its positive electrode sheet, the mass ratio of the cobalt-zinc alloy catalyst material to the sulfur powder is 1:(2-2.5), which is conducive to the reasonable performance of the catalytic effect.

[0085] As some exemplary preferred schemes, in the above-mentioned lithium-sulfur battery or its positive electrode sheet, in the mixture of sulfur-carbon composite positive electrode active material, conductive agent and binder, the mass proportion of sulfur-carbon composite positive electrode active material is 60%-95%, the mass proportion of conductive agent is 8%-15%, and the mass proportion of binder is 3%-10%.

[0086] As some exemplary preferred schemes, in the above-mentioned lithium-sulfur battery or its positive electrode sheet, the material of the conductive agent is not limited, and generally includes one or more of CNT, SP, GIN, CMK-3, mesoporous carbon and carbon fiber.

[0087] As some exemplary preferred schemes, in the above-mentioned lithium-sulfur battery or its positive electrode sheet, the material of the binder is not limited, and generally includes one or more of PVDF, CMC, SBR, sodium alginate or potassium alginate.

[0088] As some exemplary preferred schemes, in the above-mentioned lithium-sulfur battery or its positive electrode sheet, the material of the current collector is not limited, and generally includes at least one or more of copper foil, aluminum foil, carbon-containing aluminum foil, stainless steel foil, carbon cloth and carbon paper.

[0089] As some exemplary preferred schemes, in the above-mentioned lithium-sulfur battery, the electrolyte is an ether or an ester. The ether solvent is one or more of 1,3-dioxolane, 1,4-dioxane, ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, and tetraethylene glycol dimethyl ether. It is preferably a mixed solution of 1,3-dioxolane and ethylene glycol dimethyl ether, wherein the volume ratio of 1,3-dioxolane and ethylene glycol dimethyl ether is 1:1. The ester solvent is one or more of ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, and ethyl methyl carbonate. It is preferably a mixed solution of ethylene carbonate and diethyl carbonate, wherein the volume ratio of ethylene carbonate and diethyl carbonate is 1:1. The lithium salt dissolved in the electrolyte is at least one of lithium bis(trifluoromethylsulfonyl)imide, lithium hexafluorophosphate, lithium bis(fluorosulfonyl)imide and lithium nitrate, preferably lithium hexafluorophosphate and lithium nitrate, wherein the concentration of lithium hexafluorophosphate is preferably 0.5-2 mol / L, and the concentration of lithium nitrate is preferably 0.1-1 mol / L.

[0090] As some exemplary preferred schemes, in the above-mentioned lithium-sulfur battery, the negative electrode active material is one of lithium metal and silicon-lithium alloy, and the lithium metal can be in the form of lithium sheet, preferably with a thickness of 40 to 50 μm and a diameter of 14 to 18 mm.

[0091] As some exemplary preferred solutions, in the above lithium-sulfur battery, the separator is not limited, and Celgard-2500 is taken as a preferred example.

[0092] Example 1 Preparation of Carbon-Supported Cobalt-Zinc Alloy Catalyst

[0093] Carbon oxide graphene was dispersed in isopropanol at a concentration of 1 mg: 1 mL, and after ultrasonic dispersion, a total amount of 0.24 mmol of cobalt acetate and zinc acetate was added per 80 mg of graphite oxide powder. The mixture was condensed and refluxed in an 80 ° C oil bath for 1.5 h, and the resulting product was washed several times with ethanol, collected by centrifugation and dried. The obtained dry solid powder was placed in a tube furnace, heated at 300 ° C for 2 h under an argon atmosphere for preliminary reduction, and after cooling to room temperature, the solid products were placed in a microwave reactor, and the carbon-supported cobalt-zinc alloy catalyst was obtained by reacting at 1000 W full power for 3 min under argon atmosphere protection. In this embodiment, according to the Zn / Co atomic ratio of the feed, G-CoZn-0.5, G-CoZn, G-CoZn-2 and G-CoZn-5 were obtained.

[0094] Example 2 Preparation of button lithium-sulfur battery

[0095] The carbon-supported cobalt-zinc alloy catalyst obtained in Example 1 and sulfur powder were mixed in a mass ratio of 3:7, and sulfur was melted in a tube furnace under an argon atmosphere to obtain a sulfur-carbon composite positive electrode active material. The sulfur-carbon composite positive electrode active material was mixed with a conductive agent and a binder in a mass ratio of 8:1:1 to prepare a positive electrode slurry with a solid content of 20%. The positive electrode slurry was coated on a carbon-coated aluminum foil with a loading of 5.5 mg / cm 2 , and dried to obtain the positive electrode of the lithium-sulfur battery. Celgard-2500 diaphragm and lithium metal negative electrode were selected. The solvent of the electrolyte was 1,3-dioxolane and ethylene glycol dimethyl ether in a volume ratio of 1:1. The lithium salt was 1 mol / L lithium bistrifluoromethylsulfonyl imide and 2% lithium nitrate by mass. Lithium-sulfur CR2032 button batteries were assembled.

[0096] Example 3 Preparation of lithium-sulfur soft pack battery

[0097] The negative electrode in Example 2 was replaced with carbon felt to assemble a lithium-sulfur soft pack battery with an electrolyte / sulfur (E / S) ratio of 4 μL / mg. S and 1.8 μL / mg S .

[0098] Comparative Example 1

[0099] The same method as in Examples 1 and 2 was used to prepare a carbon-supported cobalt metal catalyst (G-Co), and a corresponding lithium-sulfur battery was assembled.

[0100] Comparative Example 2

[0101] Graphene (G) obtained by high-temperature thermal reduction of graphene oxide was used as a catalyst to replace the cobalt-zinc alloy catalyst material, and a lithium-sulfur battery was assembled accordingly.

[0102] Comparative Example 3

[0103] A cobalt-copper alloy catalyst material (G-CoCu) was prepared by the same method as in Examples 1 and 2, and a lithium-sulfur battery was assembled accordingly. The reduction temperature during the preparation process was 700° C. and the heat treatment time was 2 h.

[0104] Figure 4 The HR-TEM images of the catalysts obtained in Example 1 and Comparative Example 1 and the corresponding element distribution are shown. By comparison, it can be seen that the carbon-supported cobalt-zinc alloy catalyst prepared by the present invention is composed of Zn atoms partially replacing Co atoms, and the introduction of Zn atoms causes a certain degree of lattice distortion. The Co element and the Zn element are evenly distributed in the particle area without obvious separation, and the obtained nanoparticles are single-phase Co-Zn alloys.

[0105] Figure 5 The CV curves and Tafel curves of the embodiments and comparative examples are shown. As can be seen from the figure, the introduction of metal nanoparticles (relative to G-Comparative Example 2) effectively improves the redox peak current, proving that it has a significant catalytic promotion effect on sulfur conversion kinetics, but the catalytic effects of Co metal (G-Co) and cobalt-zinc alloys of different proportions are different. Further, the Tafel slope of the rate-controlling step is fitted and calculated, and the catalytic effect of G-CoZn is the best, and its Tafel slope is only 23.2mV / dec.

[0106] Will Figure 5 Test results and f sulfur Associated Figure 6 The volcano-shaped curve shown. Figure 6 The relationship between sulfur-solvent competitive adsorption and sulfur conversion kinetics is more intuitively demonstrated. sulfur The reaction kinetics changes with the decrease of Zn addition. sulfur The catalytic performance is limited by the number of active sites. In this region, the strong adsorption of the solvent will hinder the direct contact between the catalyst and the sulfur species. As the competitive adsorption of sulfur increases, the contact opportunities between the catalyst and the sulfur species will increase, which will directly lead to an improvement in the catalytic effect. sulfur After exceeding a certain threshold, the catalytic performance of the material will decrease as the amount of Zn added decreases. This is because the competitive adsorption of sulfur is too strong at this time, destroying the double layer structure, hindering product desorption and diffusion mass transfer, and causing the reaction kinetics to deteriorate. This result further verifies the sulfur adsorption factor (f sulfur ) The reliability of the evaluation of catalyst surface enrichment and the rationality of using optimized screening of catalysts and their atomic ratios. The G-CoZn material at the top of the volcano curve has the best f sulfur (relative to G-Co f sulfurThe competitive adsorption of solvent and sulfur on the catalyst surface was effectively balanced, showing the best catalytic performance.

[0107] Figure 7 The cycling performance of Example G-CoZn and Comparative Examples G-Co and G at different rates are demonstrated. The lithium-sulfur battery of Example G-CoZn can still exhibit a reversible specific capacity of about 657 mAh / g at a high rate of 4.0C, which is much higher than the other two samples (G: 478 mAh / g; G-Co: 558 mAh / g). In addition, the battery of Example G-CoZn can also maintain a reversible specific capacity of more than 672 mAh / g after 300 cycles at a current density of 1.0C, with a retention rate of 75%; when the current density is increased to 2.0C, the lithium-sulfur battery of Example G-CoZn still has a high initial capacity of up to 784 mAh / g, and can be stably cycled for more than 1,000 cycles, with a single-cycle attenuation rate of only 0.042%. Much higher than the other two samples.

[0108] Figure 8 The voltage-activation energy curves of the lithium-sulfur batteries of Example G-CoZn and Comparative Examples G-Co and G, as well as the Co 2p and S2p XPS graphs of the positive electrode after cycling are shown. Although G-Co effectively reduces the sulfur conversion barrier in the high potential region, it has no significant effect on the low potential region; while G-CoZn can show significant catalytic effects at both high and low potentials. Co-S bonds were detected on the surface of the positive electrode with G-Co as the catalyst, proving that G-Co was poisoned by sulfidation; while the Co-S signal was basically undetectable on the positive electrode with G-CoZn as the catalyst, which is due to the protective effect of moderate solvent enrichment on the catalytic surface.

[0109] Fig. 9 The dimensionless current-time curves of Example G-CoZn and Comparative Examples G-Co and G, as well as SEM photos of Li2S deposition on their surfaces are shown. Li2S follows a 2DP growth mode on the G surface, and the growth mode on the G-Co surface is converted to 2DI. However, due to the strong adsorption of sulfur by the Co site, the outward diffusion of the product is suppressed, resulting in Li2S still being in a two-dimensional deposition mode on the G-Co surface, which will cause the catalytic site to be quickly covered by an insulating Li2S thin layer, thereby limiting its subsequent conversion and seriously affecting the sulfur utilization rate. For G-CoZn, the presence of the surface solvent enhances the diffusion and mass transfer of Li2S, enabling it to grow in a three-dimensional mode, which not only improves the Li2S deposition capacity, but also ensures the long-term stability of the catalytic site.

[0110] Fig.10 The cycling performance of the Example G-CoZn soft pack battery is shown. The stacked soft pack battery with a high sulfur loading of 1.06 g has an electrolyte / sulfur (E / S) ratio of 4 μL / mgS A high initial capacity of 1.51Ah was achieved under lean solution conditions, and it could be stably cycled for more than 50 cycles at a current density of 0.1C; when the E / S ratio was reduced to 1.8μL / mgS, an ultra-high energy density of more than 464Wh / kg was achieved.

[0111] Fig.11 The charge and discharge behavior of the G-CoCu lithium-sulfur battery of Comparative Example 3 is shown in comparison. It can be seen that Comparative Example 3 exhibits abnormal charging behavior, which is because Cu is too active in the working range of the lithium-sulfur battery (1.7V-2.8V vsLi+ / Li), and severe oxidation occurs at high potential, resulting in the inability of the corresponding positive electrode to be charged normally, and metal Cu cannot be used as an alloy material for the positive electrode catalyst of the lithium-sulfur battery.

[0112] The technical features of the above-described embodiments can be combined arbitrarily. In order to make the description concise, all possible combinations of the technical features in the above-described embodiments are not described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification. Although the embodiments of the present invention have been shown and described above, it can be understood that the above-described embodiments are exemplary and cannot be understood as limitations of the present invention. Those of ordinary skill in the art can change, modify, replace and deform the above-described embodiments within the scope of the present invention. In addition, those of ordinary skill in the art can combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples without contradiction.

Claims

1. A cobalt-zinc alloy catalyst material with adjustable surface microenvironment, wherein the cobalt-zinc alloy is in-situ loaded on a carbon material in a single phase.

2. The cobalt-zinc alloy catalyst material with adjustable surface microenvironment according to claim 1, characterized in that: The f of the catalyst with single cobalt metal in situ supported on carbon material under the same system sulfur The value is a reference value, and the f sulfur The value is 40% to 90% of the reference value, further 60% to 80%, and further 70% to 75%; The f sulfur : Among them, C dl and C dl,S They are the double layer capacitance values ​​before and after adding sulfur into the electrolyte.

3. The cobalt-zinc alloy catalyst material with adjustable surface microenvironment according to claim 2, characterized in that: The C dl and C dl,S It is measured in a lithium-sulfur battery with a salt concentration greater than 0.5 mol / L and a voltage greater than 1 V; preferably, it is measured in a lithium-sulfur battery with a salt concentration of 0.5-2 mol / L and a voltage of 2-3 V.

4. The cobalt-zinc alloy catalyst material with adjustable surface microenvironment according to claim 2, characterized in that: The concentration of sulfur added to the electrolyte is 1 to 10 mM, preferably 3 to 5 mM.

5. The cobalt-zinc alloy catalyst material with adjustable surface microenvironment according to claim 1, characterized in that: In the cobalt-zinc alloy catalyst material, the Zn / Co atomic ratio is 0.5 to 2, preferably 1±0.

2.

6. The cobalt-zinc alloy catalyst material with adjustable surface microenvironment according to claim 1, characterized in that: In the cobalt-zinc alloy catalyst material, the carbon material includes one or more of graphene, carbon nanotubes, activated carbon, carbon aerogel, carbon nanofiber, porous carbon sphere, graphitized carbon, carbon nanowire, carbon nanosheet, and carbon composite material, wherein the carbon composite material includes carbon / metal oxide and carbon / sulfide; Preferably, in the cobalt-zinc alloy catalyst material, the ratio of carbon material to cobalt and zinc is 0.1 to 0.5 mmol in total of cobalt and zinc per 80 mg of graphene oxide, and more preferably 0.2 to 0.3 mmol in total of cobalt and zinc per 80 mg of carbon material.

7. A method for preparing the cobalt-zinc alloy catalyst material according to any one of claims 1 to 6, comprising the steps of dispersing a carbon material, a cobalt salt and a zinc salt in a solvent according to a stoichiometric ratio, collecting and drying the product after condensation and reflux, and then heating and reducing it under an inert atmosphere to obtain the catalyst.

8. The method for preparing the cobalt-zinc alloy catalyst material according to claim 7, characterized in that: The concentration of the carbon material in the solvent is 0.5 to 2 mg / mL; Preferably, the solvent is isopropanol; Preferably, the condensation reflux is carried out at a temperature of 70-90°C; Preferably, the temperature of heating reduction is 280-320°C, and the heating time is more than 1 hour, more preferably 2-48 hours; Preferably, after the heating reduction, a microwave reaction is further performed at a power of 800-1200 W for 2-10 min.

9. A lithium-sulfur battery positive electrode comprising the cobalt-zinc alloy catalyst material according to any one of claims 1 to 6.

10. The lithium-sulfur battery positive electrode according to claim 9, characterized in that: The positive electrode active material comprises the cobalt-zinc alloy catalyst material and a sulfur source, and the mass ratio of sulfur S8 that can be provided by the cobalt-zinc alloy catalyst material and the sulfur source is 1:(2-2.5); Preferably, the sulfur source includes elemental sulfur, lithium polysulfide, lithium sulfide, sulfur-containing organic polymer, metal sulfide, selenium / tellurium-sulfur composite material; Preferably, it also includes a conductive agent and a binder, the mass proportion of the cobalt-zinc alloy catalyst material and the sulfur source in the positive electrode material is 60%-95%, the mass proportion of the conductive agent is 8%-15%, and the mass proportion of the binder is 3%-10%; Preferably, the positive electrode loading is 1 to 7 mg / cm 2 , 5~6mg / cm 2 is better; Preferably, the conductive agent includes one or more of CNT, SP, GIN, CMK-3, mesoporous carbon and carbon fiber; Preferably, the binder includes one or more of PVDF, CMC, SBR, sodium alginate or potassium alginate; Preferably, the current collector includes at least one or more of copper foil, aluminum foil, carbon-containing aluminum foil, stainless steel foil, carbon cloth and carbon paper.