Electrode testing method, reference electrode, electrode assembly, battery and electric device

By constructing a test circuit and utilizing the principle that the internal resistance of the voltmeter is greater than the internal resistance of the electrode, the voltage change caused by the change in electrode area in the electrolyte is measured, and the polarization index is calculated. This solves the problem of inaccurate polarization performance testing of the reference electrode and improves the accuracy and precision of the test.

CN118914870APending Publication Date: 2024-11-08CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310504683.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-06
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing technologies make it difficult to accurately test the polarization performance of the reference electrode, which affects the measurement results of the potential of the positive and negative electrodes.

Method used

A test circuit was constructed. By adjusting the immersion area of ​​the second electrode in the electrolyte, and taking advantage of the fact that the internal resistance of the voltmeter is much greater than the internal resistance of the electrode, the voltage change was measured based on the voltage division principle of the series circuit to reflect the polarization performance. The polarization index was calculated by normalizing the voltage difference and the internal resistance.

Benefits of technology

This improves the accuracy and precision of the reference electrode polarization performance test, reduces interference with the potential measurement of the positive and negative electrodes, and ensures the reliability of the test results.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118914870A_ABST
    Figure CN118914870A_ABST
Patent Text Reader

Abstract

The invention discloses an electrode testing method, a reference electrode, an electrode assembly, a battery and an electric device. The polarization performance of the reference electrode can be effectively tested. The testing method comprises the steps that a testing loop is constructed, the testing loop comprises a first electrode, a second electrode and a voltmeter connected between the first electrode and the second electrode, and the first electrode and the second electrode are immersed in electrolyte; adjusting the area of the second electrode immersed in the electrolyte to be a first area, and obtaining a first voltage measured by the voltmeter; adjusting the area of the second electrode immersed in the electrolyte to be a second area, and obtaining a second voltage measured by the voltmeter; and determining the polarization performance of the second electrode according to the first voltage and the second voltage.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of batteries, and in particular to an electrode testing method, a reference electrode, an electrode assembly, a battery and an electrical device. Background Art

[0002] The reference electrode is an electrode used as a reference when measuring the potential of the positive electrode and / or negative electrode in a battery. The polarization performance of the reference electrode directly affects the test results of the potential of the positive electrode and the negative electrode. Therefore, how to test the polarization performance of the reference electrode has become an urgent problem to be solved. Summary of the invention

[0003] The embodiments of the present application provide an electrode testing method, a reference electrode, an electrode assembly, a battery, and an electrical device, which can effectively test the polarization performance of the reference electrode.

[0004] In a first aspect, a method for testing an electrode is provided, the method comprising: constructing a test circuit, the test circuit comprising a first electrode, a second electrode, and a voltmeter connected between the first electrode and the second electrode, the first electrode and the second electrode being immersed in an electrolyte; adjusting the area of ​​the second electrode immersed in the electrolyte to a first area, and obtaining a first voltage measured by the voltmeter; adjusting the area of ​​the second electrode immersed in the electrolyte to a second area, and obtaining a second voltage measured by the voltmeter; and determining the polarization performance of the second electrode based on the first voltage and the second voltage.

[0005] In an embodiment of the present application, a test circuit for testing the polarization performance of an electrode includes a first electrode, a second electrode, and a voltmeter connected between the first electrode and the second electrode, wherein the first electrode, the second electrode and the electrolyte form a power supply, and the voltmeter serves as a load. The internal resistance of the voltmeter is usually much greater than the internal resistance of the electrode, so the resistance of the test circuit is mainly contributed by the internal resistance of the voltmeter, and the impedance change of the second electrode caused by the change in the area of ​​the second electrode immersed in the electrolyte has little effect on the resistance of the entire test circuit, so the current of the test circuit can be regarded as unchanged. In this way, based on the voltage division principle of the series circuit, when the area of ​​the second electrode immersed in the electrolyte changes and causes the impedance of the second electrode to change, the voltage division of the second electrode changes, and then the voltage division of the voltmeter also changes, and the change in the voltage measured by the voltmeter can directly reflect the change in the impedance of the second electrode. The impedance of the second electrode can be used as a parameter to measure its polarization performance. When the area of ​​the second electrode immersed in the electrolyte changes, the polarization performance of the second electrode can be effectively tested according to the change in the voltage measured by the voltmeter.

[0006] In one implementation, determining the polarization performance of the second electrode based on the first voltage and the second voltage includes: determining an indicator for representing the polarization performance of the second electrode based on the voltage difference between the first voltage and the second voltage, and the internal resistance of the voltmeter and / or the first voltage.

[0007] In this embodiment, the polarization performance of the second electrode can be evaluated by a corresponding index. The polarization performance of the second electrode is directly related to the voltage difference between the first voltage and the second voltage measured by the voltmeter, but the measurement result of the voltage difference is also affected by the internal resistance of the voltmeter and / or the first voltage. Since polarization is an intrinsic property of the electrode, when determining the index, the influence of the internal resistance of the voltmeter and / or the first voltage on the test result is considered at the same time, and the index is normalized using the internal resistance of the voltmeter and / or the first voltage, which can improve the accuracy of the test result.

[0008] For example, determining an indicator for representing the polarization performance of the second electrode based on the voltage difference between the first voltage and the second voltage, the internal resistance of the voltmeter and / or the first voltage includes: multiplying the voltage difference by the internal resistance of the voltmeter and dividing the result by the first voltage to obtain the indicator.

[0009] Among them, the larger the internal resistance of the voltmeter, the smaller the current of the test circuit, and the smaller the voltage change caused by the change in the area of ​​the second electrode immersed in the electrolyte. Therefore, the voltage difference can be multiplied by the internal resistance of the voltmeter; the larger the first voltage, the larger the current of the test circuit, and the larger the voltage change caused by the change in the area of ​​the second electrode immersed in the electrolyte. Therefore, the voltage difference can be divided by the first voltage.

[0010] In one implementation, the method also includes: adjusting at least one of the following parameters of the second electrode so that the indicator is within a predetermined range: the type of active material of the second electrode, the specific surface area of ​​the active material, the loading amount of the active material per unit size, and the size of the second electrode.

[0011] In this embodiment, the type of active material of the second electrode, the specific surface area of ​​the active material, the load of the active material per unit size, and the size of the second electrode will affect the polarization performance of the second electrode. In order to improve the polarization performance of the second electrode sheet, a material with a higher exchange current density may be used, or the specific surface area of ​​the active material on the surface of the second electrode may be increased, or the load of the active material per unit size may be increased, such as increasing the coating weight per unit area of ​​the active material, or increasing the electrode size.

[0012] The predetermined range is, for example, less than or equal to 10, wherein the voltage difference and the first voltage are in volts, and the internal resistance of the voltmeter is in megohms. When the second electrode of the indicator is within the range, when used as a reference electrode to test the potential of the positive electrode and the negative electrode of the battery, a better test result can be obtained.

[0013] In one implementation, the area of ​​the first electrode immersed in the electrolyte is larger than the area of ​​the second electrode immersed in the electrolyte, and the area of ​​the first electrode immersed in the electrolyte remains unchanged during the test. The area of ​​the first electrode immersed in the electrolyte can be much larger than the area of ​​the second electrode immersed in the electrolyte, thereby reducing the polarization of the first electrode, reducing the interference of the first electrode in the test process, and improving the accuracy of the test of the polarization performance of the second electrode.

[0014] In one implementation, the second electrode is arranged between the positive electrode and the negative electrode of the battery as a reference electrode, and the size of the second electrode in its width direction is less than or equal to a preset value, and the preset value is negatively correlated with the lithium ion transmission performance between the positive electrode and the negative electrode, and the width direction is perpendicular to the extension direction of the electrode ear of the reference electrode.

[0015] It can be understood that the larger the area of ​​the second electrode, the smaller its polarization. However, when the second electrode is used as a reference electrode, since it is disposed between the positive electrode and the negative electrode of the battery, the larger the area of ​​the second electrode, the greater the hindrance to the lithium ion transmission between the positive electrode and the negative electrode, which is not conducive to the transmission of lithium ions. For this reason, in this embodiment, the area of ​​the second electrode is set to be small enough, for example, its width is less than or equal to a preset value, so that its influence on the lithium ion transmission performance between the positive electrode sheet and the negative electrode sheet is within an acceptable range.

[0016] For example, the preset value may be 1 mm, that is, the size of the second electrode in its width direction is less than or equal to 1 mm.

[0017] In one implementation, the second electrode includes a metal substrate and an active material covering the surface of the metal substrate, the metal substrate is metal wire or carbon fiber, the size of the metal substrate in the width direction is less than or equal to 0.1 mm, and the preset value is 0.2 mm.

[0018] A filamentary electrode can be used, for example, by electroplating or coating an active material layer on the surface of a metal wire or carbon fiber, thereby forming a second electrode with a total diameter of less than 0.2 mm. When such an electrode is arranged between the positive electrode and the negative electrode of a battery as a reference electrode, it will not cause significant obstruction to the lithium ion transport between the positive electrode and the negative electrode.

[0019] In one implementation, the second electrode includes a metal substrate and an active material covering the surface of the metal substrate, the metal substrate is a metal foil, and the preset value is 1 mm.

[0020] A sheet-shaped electrode can be used, for example, by electroplating or coating an active material layer on the surface of a metal foil to form a second electrode with a width of less than 1 mm. When such an electrode is arranged between the positive electrode and the negative electrode of a battery as a reference electrode, it will not cause significant obstruction to the lithium ion transmission between the positive electrode and the negative electrode.

[0021] In one implementation, the electrode is tested multiple times, and the performance of the second electrode is determined based on the voltage difference between the first voltage and the second voltage, including: determining the performance of the second electrode based on the multiple voltage differences obtained from the multiple tests, wherein the proportion of the change in the area of ​​the second electrode immersed in the electrolyte is the same in the multiple tests.

[0022] The above test process can be performed multiple times, that is, the area of ​​the second electrode immersed in the electrolyte is continuously changed, and the voltages obtained twice are subtracted in sequence to obtain multiple voltage differences, and the final test results are determined based on the multiple voltage differences, thereby reducing the test error and improving the test accuracy and stability. In order to make the data of multiple tests comparable, the proportion of the change in the area of ​​the second electrode immersed in the electrolyte each time is the same, that is, the area is reduced or increased by the same proportion each time.

[0023] In a second aspect, a method for testing an electrode is provided, the method comprising: obtaining voltage parameters of a test circuit, the test circuit comprising a first electrode, a second electrode, and a voltmeter connected between the first electrode and the second electrode, the first electrode and the second electrode being immersed in an electrolyte, the voltage parameters comprising a first voltage measured by the voltmeter when an area of ​​the second electrode immersed in the electrolyte is a first area, and a second voltage measured by the voltmeter when an area of ​​the second electrode immersed in the electrolyte is a second area; determining an indicator for representing the polarization performance of the second electrode based on the voltage parameters.

[0024] In the embodiments of the present application, an indicator for representing the polarization performance of an electrode is also proposed, which can quantify the polarization performance of the electrode and improve the accuracy of the test results.

[0025] In one implementation, the indicator is determined based on a voltage difference between the first voltage and the second voltage, an internal resistance of the voltmeter, and the first voltage.

[0026] In one implementation, the indicator is equal to a ratio of a product of the voltage difference and an internal resistance of the voltmeter to the first voltage.

[0027] In a third aspect, a reference electrode is provided, which is used to be arranged between the positive electrode and the negative electrode of the battery, the dimension of the reference electrode in its width direction is less than or equal to a preset value, the preset value is negatively correlated with the lithium ion transmission performance between the positive electrode and the negative electrode, and the width direction is perpendicular to the extension direction of the electrode ear of the reference electrode.

[0028] In the embodiment of the present application, a reference electrode is also provided. Generally, the larger the area of ​​the reference electrode, the smaller its polarization. However, since the reference electrode is usually arranged between the positive electrode and the negative electrode of the battery, the larger the area of ​​the reference electrode, the greater the hindrance to the lithium ion transmission between the positive electrode and the negative electrode, which is not conducive to the transmission of lithium ions. For this reason, the area of ​​the reference electrode in the embodiment of the present application is set to be small enough, for example, its width is less than or equal to a preset value, so that its influence on the lithium ion transmission performance between the positive electrode sheet and the negative electrode sheet is within an acceptable range. The preset value is, for example, 1 mm.

[0029] In one implementation, the reference electrode includes a metal substrate and an active material covering the surface of the metal substrate, the metal substrate is a metal wire or a carbon fiber, the dimension of the metal substrate in the width direction is less than or equal to 0.1 mm, and the preset value is 0.2 mm.

[0030] In one implementation, the reference electrode includes a metal substrate and an active material covering the surface of the metal substrate, the metal substrate is a metal foil, and the preset value is 1 mm.

[0031] In a fourth aspect, an electrode assembly is provided, the electrode assembly comprising a positive electrode sheet, a negative electrode sheet, and a reference electrode disposed between the positive electrode sheet and the negative electrode sheet, the reference electrode comprising: the reference electrode according to the third aspect or any implementation of the third aspect; and / or, the second electrode in the test method according to the second aspect or any implementation of the second aspect. Optionally, the index for evaluating the reference electrode is within a predetermined range. The predetermined range is, for example, less than or equal to 10.

[0032] In a fifth aspect, a battery is provided, comprising the electrode assembly according to the fourth aspect or any implementation manner of the fourth aspect; and a shell for accommodating the electrode assembly.

[0033] In a sixth aspect, an electrical device is provided, comprising: an electrode assembly according to the fourth aspect or any implementation of the fourth aspect; or a battery according to the fifth aspect or any implementation of the fifth aspect, wherein the battery is used to provide electrical energy to the electrical device. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments of the present application will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on the drawings without paying creative work.

[0035] Figure 1 It is a schematic flow chart of the electrode testing method of the embodiment of the present application.

[0036] Figure 2 It is a schematic diagram of establishing a test loop according to an embodiment of the present application.

[0037] Figure 3 It is an equivalent circuit diagram of the test circuit used in the electrode testing method of the embodiment of the present application.

[0038] Figure 4 It is a schematic diagram of an electrode assembly with a built-in reference electrode according to an embodiment of the present application.

[0039] Figure 5 It is a schematic flow chart of a method for testing an electrode according to another embodiment of the present application.

[0040] Figure 6 It is a schematic block diagram of an electrode assembly according to an embodiment of the present application. DETAILED DESCRIPTION

[0041] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0042] Unless otherwise defined, all technical and scientific terms used in this application have the same meaning as those generally understood by technicians in the technical field to which this application belongs; the terms used in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" in the specification and claims of this application and the above-mentioned figure descriptions and any variations thereof are intended to cover non-exclusive inclusions. The terms "first", "second", etc. in the specification and claims of this application or the above-mentioned figures are used to distinguish different objects, not to describe a specific order or a primary and secondary relationship. "Vertical" is not strictly perpendicular, but within the allowable error range. "Parallel" is not strictly parallel, but within the allowable error range.

[0043] Reference to "embodiments" in this application means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present application. The appearance of the phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described in this application may be combined with other embodiments.

[0044] In the description of this application, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", and "attached" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a direct connection, or an indirect connection through an intermediate medium, or it can be the internal communication of two elements. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.

[0045] The term "and / or" in this application is only a description of the association relationship of associated objects, indicating that there can be three relationships. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. In addition, the character " / " in this application generally indicates that the associated objects before and after are in an "or" relationship.

[0046] In the embodiments of the present application, the same reference numerals represent the same components, and for the sake of brevity, detailed descriptions of the same components are omitted in different embodiments. It should be understood that the thickness, length, width and other dimensions of various components in the embodiments of the present application shown in the drawings, as well as the overall thickness, length, width and other dimensions of the integrated device are only exemplary descriptions and should not constitute any limitation to the present application.

[0047] A battery generally refers to a single physical module that includes one or more battery cells to provide higher voltage and capacity. For example, the battery may include a battery module or a battery pack. Typically, a battery also includes a box for encapsulating one or more battery cells. The box can prevent liquid or other foreign matter from affecting the charging or discharging of the battery cells.

[0048] The battery cell includes an electrode assembly and an electrolyte. The electrode assembly is composed of a positive electrode sheet, a negative electrode sheet and a separator. The battery cell mainly relies on the movement of metal ions between the positive electrode sheet and the negative electrode sheet to work. The positive electrode sheet includes a positive electrode current collector and a positive electrode active material layer. The positive electrode active material layer is coated on the surface of the positive electrode current collector. The current collector not coated with the positive electrode active material layer protrudes from the current collector coated with the positive electrode active material layer. The current collector not coated with the positive electrode active material layer serves as the positive electrode tab. Taking lithium-ion batteries as an example, the material of the positive electrode current collector may be aluminum, and the positive electrode active material may be lithium cobalt oxide, lithium iron phosphate, ternary lithium or lithium manganese oxide, etc. The negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer. The negative electrode active material layer is coated on the surface of the negative electrode current collector. The current collector not coated with the negative electrode active material layer protrudes from the current collector coated with the negative electrode active material layer. The current collector not coated with the negative electrode active material layer serves as the negative electrode tab. The material of the negative electrode current collector may be copper, and the negative electrode active material may be carbon or silicon, etc. In order to reduce the probability of melting due to a large current, the number of positive electrode tabs is multiple and they are stacked together, and the number of negative electrode tabs is multiple and they are stacked together.

[0049] When testing the potential of the positive electrode and / or negative electrode of a battery, a reference electrode is usually disposed between the positive electrode and the negative electrode of the battery and connected to an external circuit, so a small current also flows through the reference electrode, which causes polarization of the reference electrode, resulting in deviation of the potential of the reference electrode, making the measured potential of the positive electrode or negative electrode inaccurate, thereby affecting the analysis and judgment of the measurement results. Generally, the smaller the polarization of the reference electrode, the smaller the deviation of its potential during the test process, and more accurate results can be obtained when testing the positive and negative electrodes.

[0050] To this end, the present application proposes a method for testing an electrode, which can effectively test the polarization performance of a reference electrode. In addition, the present application also proposes an index for characterizing the polarization performance of an electrode, which can quantify the polarization performance of an electrode and improve the accuracy of the test results.

[0051] Figure 1 is a schematic flow chart of the electrode testing method of the embodiment of the present application. Figure 1 As described above, the testing method 100 includes part or all of the following steps.

[0052] In step S110 , a test loop is constructed.

[0053] For example, Figure 2 As shown, the test circuit includes a first electrode 110, a second electrode 120, and a voltmeter 130 connected between the first electrode 110 and the second electrode 120. The first electrode 110 and the second electrode 120 are immersed in an electrolyte.

[0054] In step S120 , the area of ​​the second electrode 120 immersed in the electrolyte is adjusted to be a first area, and when the area of ​​the second electrode 120 immersed in the electrolyte is the first area, the first voltage measured by the voltmeter 130 is obtained.

[0055] In step S130 , the area of ​​the second electrode 120 immersed in the electrolyte is adjusted to a second area, and when the area of ​​the second electrode 120 immersed in the electrolyte is the second area, the second voltage measured by the voltmeter 130 is obtained.

[0056] In step S140 , the polarization property of the second electrode 120 is determined according to the first voltage and the second voltage.

[0057] In the test loop, the first electrode 110, the second electrode 120 and the electrolyte form a power source, and the voltmeter 130 serves as a load. Figure 3 The equivalent circuit of the test loop is shown in Figure 3 As shown, the internal resistance of the power supply includes the impedance R1 of the first electrode 110 and the impedance R2 of the second electrode 120, and the internal resistance of the voltmeter is Rv.

[0058] Since the internal resistance Rv of the voltmeter 130 is usually at the MΩ or GΩ level, and the impedance of the electrode is usually at the Ω level, the internal resistance Rv of the voltmeter is much larger than the impedance of the electrode, so the resistance of the test loop is mainly contributed by the internal resistance Rv of the voltmeter. When the area of ​​the second electrode 120 immersed in the electrolyte changes, the impedance of the second electrode 120 changes, but since the internal resistance Rv of the voltmeter 130 is large, the change in the resistance of the entire test loop can be ignored. The resistance of the entire test loop can be regarded as constant, or in other words, the current in the test loop can be regarded as constant.

[0059] like Figure 3As shown, the first electrode 110, the second electrode 120 and the voltmeter 130 are connected in series. Based on the voltage division principle of the series circuit, when the impedance of the second electrode 120 changes, the voltage shared by the second electrode 120 will change significantly. The voltage U of the second electrode 120 = I*R2, where I is the current of the test circuit. When the area of ​​the second electrode 120 immersed in the electrolyte changes, I remains unchanged, R2 changes, and the voltage division U of the second electrode 120 changes. At the same time, since the impedance of the first electrode 110 has not changed, the voltage division of the first electrode 110 remains unchanged, so the voltage measured by the voltmeter 130, that is, the voltage division of the voltmeter 130, will change significantly. It can be seen that the change in the voltage measured by the voltmeter 130 can directly reflect the change in the voltage division caused by the change in the area of ​​the second electrode 120. When the area of ​​the second electrode 120 changes and causes its impedance to increase, the divided voltage U of the second electrode 120 increases, and the voltage measured by the voltmeter 130 decreases; when the area of ​​the second electrode 120 changes and causes its impedance to decrease, the divided voltage U of the second electrode 120 decreases, and the voltage measured by the voltmeter 130 increases.

[0060] Since the internal resistance Rv of the voltmeter 130 is very large, the electrochemical process occurring in the electrolyte is very weak, and the impedance change of the second electrode 120 caused by the change in the area of ​​the second electrode 120 immersed in the electrolyte mainly comes from the change in the charge transfer resistance Rct. Generally, the charge transfer resistance Rct can be used as a parameter to measure the performance of the electrode. According to η=I×Rct, where I is the current flowing through the second electrode 120, that is, the current of the test circuit, and η is the overpotential of the second electrode 120 under the condition of current I, it can be seen that when the current I remains unchanged, the smaller the charge transfer resistance Rct, the smaller the overpotential η, the smaller the polarization of the second electrode 120, that is, the smaller the degree of deviation of the potential of the second electrode 120 from the equilibrium potential, and the better the polarization performance of the second electrode 120.

[0061] When the second electrode 120 is used as a reference electrode, it can be set between the positive electrode and the negative electrode of the battery to test the potential of the positive electrode and / or the negative electrode of the battery. The better the polarization performance of the reference electrode, the more accurate the test data obtained when testing the potential of the positive electrode and / or the negative electrode.

[0062] It can be understood that the resistance in the test circuit includes not only the impedance of the first electrode 110, the impedance of the second electrode 120 and the internal resistance of the voltmeter 130, but also the solution resistance of the electrolyte. However, the solution impedance is usually much smaller than the internal resistance Rv of the voltmeter, so the influence of the electrolyte can be ignored.

[0063] During the test, optionally, the area of ​​the first electrode 110 immersed in the electrolyte is larger than the area of ​​the second electrode 120 immersed in the electrolyte, and the area of ​​the first electrode 110 immersed in the electrolyte remains unchanged during the test. The area of ​​the first electrode 110 immersed in the electrolyte can be much larger than the area of ​​the second electrode 120 immersed in the electrolyte, for example, the area of ​​the first electrode 110 is more than 100 times the area of ​​the second electrode 120, thereby reducing the polarization of the first electrode 110, reducing the interference of the first electrode 110 on the test process, and improving the accuracy of the test of the polarization performance of the second electrode 120.

[0064] In an embodiment of the present application, a test circuit for testing the polarization performance of an electrode includes a first electrode 110, a second electrode 120, and a voltmeter 130 connected between the first electrode 110 and the second electrode 120, wherein the first electrode 110, the second electrode 120 and the electrolyte form a power supply, and the voltmeter 130 serves as a load. The internal resistance of the voltmeter 130 is usually much greater than the internal resistance of the electrode, so the resistance of the test circuit is mainly contributed by the internal resistance Rv of the voltmeter, and the impedance change of the second electrode 120 caused by the change in the area of ​​the second electrode 120 immersed in the electrolyte has little effect on the resistance of the entire test circuit, so the current of the test circuit can be regarded as unchanged. In this way, based on the voltage division principle of the series circuit, when the area of ​​the second electrode 120 immersed in the electrolyte changes and causes the impedance of the second electrode 120 to change, the voltage division of the second electrode 120 changes, and then the voltage division of the voltmeter 130 also changes, and the change in the voltage measured by the voltmeter 130 can directly reflect the change in the impedance of the second electrode 120. The impedance of the second electrode 120 can be used as a parameter to measure its polarization performance. When the area of ​​the second electrode 120 immersed in the electrolyte changes, the polarization performance of the second electrode 120 can be effectively tested based on the change in voltage measured by the voltmeter 130.

[0065] In one implementation, in step S140, the polarization performance of the second electrode 120 is determined based on the first voltage and the second voltage, including: determining an indicator for representing the polarization performance of the second electrode 120 based on the voltage difference between the first voltage and the second voltage, and the internal resistance of the voltmeter 130 and / or the first voltage.

[0066] The polarization performance of the second electrode 120 can be evaluated by a corresponding index. The polarization performance of the second electrode 120 is directly related to the voltage difference between the first voltage and the second voltage measured by the voltmeter 130, but the measurement result of the voltage difference is also affected by the internal resistance of the voltmeter 130 and / or the first voltage. Since polarization is an intrinsic property of the electrode, when determining this index, the influence of the internal resistance of the voltmeter 130 and / or the first voltage on the test result is considered at the same time. The internal resistance of the voltmeter 130 and / or the first voltage are used to normalize the index, which can improve the accuracy of the test result.

[0067] For example, the voltage difference may be multiplied by the internal resistance of the voltmeter 130 and divided by the first voltage to obtain the indicator.

[0068] The index for evaluating the polarization performance of the second electrode 120 is marked as M, and the index can be expressed as M=△U×Rv / U1, for example, wherein △U=U2-U1, U1 and U2 are respectively the values ​​of the first voltage and the second voltage measured by the voltmeter 130 before and after the area change of the second electrode 120, △U is the voltage difference between the second voltage and the first voltage, and Rv is the internal resistance of the voltmeter 130.

[0069] In the embodiment of the present application, M is positively correlated with ΔU. The larger ΔU is, the larger M is, and the worse the polarization performance of the second electrode 120 is; the smaller ΔU is, the smaller M is, and the better the polarization performance of the second electrode 120 is.

[0070] Furthermore, the indicator M can be normalized using the internal resistance Rv of the voltmeter 130 and / or the first voltage U1. Specifically, the larger the internal resistance Rv of the voltmeter 130, the smaller the current I of the test circuit, and the smaller the voltage change caused by the change in the area of ​​the second electrode 120 immersed in the electrolyte. Therefore, the voltage difference △U can be multiplied by the internal resistance Rv of the voltmeter 130; the larger the first voltage U1, the larger the current I of the test circuit, and the larger the voltage change caused by the change in the area of ​​the second electrode 120 immersed in the electrolyte. Therefore, the voltage difference △U can be divided by the first voltage U1. In this way, M = △U × Rv / U1 can be obtained. If the calculation result is negative, M takes an absolute value.

[0071] Optionally, the second electrode 120 with M within a predetermined range can be used as a reference electrode, for example, the polarization index of the reference electrode is M≤10, or, further, M≤5. The units of the voltage difference △U and the first voltage U1 are volts (V), and the unit of the internal resistance of the voltmeter 130 is megaohms (MΩ). The second electrode 120 with the index within the predetermined range can obtain better test results when used as a reference electrode to test the potential of the positive electrode and / or negative electrode of the battery.

[0072] The index of the second electrode 120 may be within the predetermined range by adjusting parameters related to the second electrode 120. For example, in one implementation, at least one of the following parameters of the second electrode 120 may be adjusted to make the index within the predetermined range: the type of active material of the second electrode 120, the specific surface area of ​​the active material, the loading amount of the active material per unit size, and the size of the second electrode 120.

[0073] The type of active material of the second electrode 120 , the specific surface area of ​​the active material, the loading amount of the active material per unit size, and the size of the second electrode 120 will affect the polarization performance of the second electrode 120 .

[0074] The type of active material of the second electrode 120 determines the size of the exchange current density, and the effective area of ​​the active material determines the size of the exchange current. Among them, the exchange current can be considered as the product of 1 / Rct and a fixed value. In order to make the indicator M within a suitable range so that the polarization performance of the second electrode 120 meets the requirements, a material with a higher exchange current density can be used to make the charge transfer resistance Rct of the second electrode 120 smaller. For example, the exchange current density of lithium is generally greater than the exchange current density of lithium iron phosphate. Alternatively, the effective area of ​​the active material on the surface of the second electrode 120 can be increased, for example, by increasing the specific surface area (BrunauerEmmettTeller, BET) of the active material, the unit is m 2 / g, or increase the loading amount of active material per unit size, such as increasing the coating weight per unit area of ​​active material.

[0075] The size of the second electrode 120 may also be appropriately increased to reduce the polarization of the second electrode 120. Considering that the larger the size of the second electrode 120 in the width direction, the greater the influence of the second electrode 120 on the lithium ion transmission between the positive electrode and the negative electrode when the second electrode 120 is disposed between the positive electrode sheet and the negative electrode sheet as a reference electrode, therefore, it may be preferred to increase the size of the second electrode 120 in the length direction to improve its polarization performance.

[0076] In one implementation, the second electrode 120 is disposed as a reference electrode between the positive electrode and the negative electrode of the battery, and the size of the second electrode 120 in its width direction is less than or equal to a preset value, which is negatively correlated with the lithium ion transmission performance between the positive electrode and the negative electrode.

[0077] It can be understood that the larger the area of ​​the second electrode 120, the smaller its polarization and the better the polarization performance. However, when the second electrode 120 is used as a reference electrode, it is usually arranged between the positive electrode and the negative electrode of the battery. Therefore, the larger the area of ​​the second electrode 120, the greater the obstacle to the lithium ion transmission between the positive electrode and the negative electrode, which is not conducive to the transmission of lithium ions. For this reason, in the embodiment of the present application, the area of ​​the second electrode 120 is set to be small enough, for example, its width is less than or equal to a preset value, so that its influence on the lithium ion transmission performance between the positive electrode sheet and the negative electrode sheet is within an acceptable range.

[0078] For example, the preset value may be 1 mm, that is, the size of the second electrode 120 in its width direction is less than or equal to 1 mm.

[0079] In the embodiment of the present application, the width direction of the second electrode 120 is perpendicular to the extension direction of the tab of the second electrode 120. When the second electrode 120 is used as a reference electrode and is disposed between the positive electrode sheet and the negative electrode sheet of the battery, the width direction of the second electrode 120 is perpendicular to the extension direction of the tab of the second electrode 120 and is parallel to the surface of the second electrode 120 facing the positive electrode sheet or the negative electrode sheet. The tab of the second electrode 120 can be in the same direction as the tab of the positive electrode sheet and the negative electrode sheet of the battery to facilitate the connection between the tabs. In this case, the width direction of the second electrode 120 is consistent with the length direction of the positive electrode sheet and the negative electrode sheet of the battery.

[0080] For example, Figure 4 In the electrode assembly shown, the second electrode 120 is used as a reference electrode and is arranged in the electrode assembly. The electrode assembly includes a positive electrode sheet 140, a negative electrode sheet 150 and a reference electrode 120. The reference electrode 120 is arranged between the positive electrode sheet 140 and the negative electrode sheet 150. A separator is arranged between the reference electrode 120 and the positive electrode sheet 140, and between the reference electrode 120 and the negative electrode sheet 150. The pole ear 141 of the positive electrode sheet 140, the pole ear 151 of the negative electrode sheet 150, and the pole ear 121 of the reference electrode 120 all extend along the direction Y, the width direction of the reference electrode 120 is the X direction, and the size of the reference electrode 120 in its width direction is W. Optionally, W≤1 mm.

[0081] The second electrode 120 includes a metal substrate and an active material covering the surface of the metal substrate. In one implementation, the second electrode 120 is a filamentary electrode, for example, the metal substrate is a metal wire or a carbon fiber, and the size of the metal substrate in the width direction X is less than or equal to 0.1 mm, and the preset value is 0.2 mm.

[0082] For example, an active material layer can be electroplated or coated on the surface of a metal wire or carbon fiber with a diameter of less than or equal to 0.1 mm, thereby forming an electrode with a total diameter of less than or equal to 0.2 mm. When such an electrode is provided as a reference electrode between the positive electrode and the negative electrode of a battery, it will not cause significant obstruction to the lithium ion transport between the positive electrode and the negative electrode.

[0083] In another implementation, the second electrode 120 is a sheet-shaped electrode, for example, the metal substrate is a metal foil, and the preset value is 1 mm.

[0084] For example, an active material layer can be electroplated or coated on the surface of a metal foil to form an electrode with a width less than or equal to 1 mm. When such an electrode is placed between the positive electrode and the negative electrode of a battery as a reference electrode, it will not cause significant obstruction to the lithium ion transport between the positive electrode and the negative electrode.

[0085] Generally, when the second electrode 120 is a sheet-shaped electrode, its thickness can be ignored compared to its length and width. During the measurement process, the area of ​​the second electrode 120 immersed in the electrolyte can mainly consider the area formed by the length and width of the sheet-shaped electrode, for example Figure 4 The area of ​​the surface of the reference electrode 120 parallel to the X direction and the Y direction. When the second electrode 120 is a wire electrode, its end surface area can also be ignored. During the measurement process, the area of ​​the second electrode 120 immersed in the electrolyte can mainly consider the area of ​​the circumferential surface of the wire electrode. Of course, during the test process, the total area of ​​each surface of the second electrode 120 immersed in the electrolyte can also be considered.

[0086] The above-mentioned test process can be carried out multiple times, that is, the area of ​​the second electrode 120 immersed in the electrolyte is changed multiple times continuously, and the voltages obtained twice adjacent are subtracted in turn to obtain multiple voltage differences, and the final test result is determined based on the multiple voltage differences, for example, the test result is determined based on the mean or weighted average of the multiple voltage differences, thereby reducing the test error and improving the test accuracy and stability.

[0087] Assume that the measurement is performed N times, where N is a positive integer. For example, in the first measurement, the initial immersion area of ​​the second electrode 120 is A, the voltage measured by the voltmeter 130 is the first voltage, the area of ​​the second electrode 120 is adjusted to K1×A, the voltage measured by the voltmeter 130 is the second voltage, and the voltage difference △U1 between the first voltage and the second voltage is calculated; in the second measurement, the initial immersion area of ​​the second electrode 120 is A, the area of ​​the second electrode 120 is adjusted to K2×A, the voltage measured by the voltmeter 130 is the second voltage, and the voltage difference △U2 between the first voltage and the second voltage is calculated; ...; in the Nth measurement, the initial immersion area of ​​the second electrode 120 is A, the voltage measured by the voltmeter 130 is the first voltage, the area of ​​the second electrode 120 is adjusted to Kn×A, the voltage measured by the voltmeter 130 is the second voltage, and the voltage difference △Un between the first voltage and the second voltage is calculated.

[0088] Here, it is necessary to satisfy K1=K2=...=Kn. The values ​​of multiple voltage differences △U1, △U2, ..., △Un are averaged or weighted averaged to calculate the index M. Alternatively, the values ​​of multiple corresponding indexes M1, M2, ..., Mn can be calculated according to the values ​​of multiple voltage differences △U1, △U2, ..., △Un, and the values ​​of multiple indexes M1, M2, ..., Mn are averaged or weighted averaged to obtain the final measurement result M.

[0089] K1, K2, ..., Kn are preset values. For the convenience of operation, K1=K2=...=Kn<1 can be set, for example, equal to 30% or 50%.

[0090] In order to make the data of multiple tests comparable, the proportion of the change in the area of ​​the second electrode 120 immersed in the electrolyte each time is the same, that is, the area is reduced or increased by the same proportion each time.

[0091] In order to more clearly illustrate the method of testing the polarization performance of the electrode in the embodiment of the present application, the following detailed test process and results are given by taking copper wire plated with lithium and lithium iron phosphate (LiFePO4, LFP) electrode as examples.

[0092] refer to Figure 2 , immerse the first electrode 110 and the second electrode 120 into the electrolyte, and connect the voltmeter 130 between the first electrode 110 and the second electrode 120. Keep the area of ​​the first electrode 110 immersed in the electrolyte unchanged, adjust the area of ​​the second electrode 120 immersed in the electrolyte to the first area, and the first voltage measured by the voltmeter 130 is U1; adjust the area of ​​the second electrode 120 immersed in the electrolyte to the second area, and the second voltage measured by the voltmeter 130 is U2. The same voltmeter 130 and the same parameter settings are used throughout the test process.

[0093] Adjusting the area of ​​the second electrode 120 immersed in the electrolyte can be achieved in any manner. For example, a portion of the second electrode 120 can be sheared off to reduce the area of ​​the second electrode 120; or, a lifting electrode can be used to lift the second electrode 120 from the electrolyte by a certain distance each time to reduce the area of ​​the second electrode 120 immersed in the electrolyte.

[0094] The voltage difference △U=U2-U1 between the first voltage U1 and the second voltage U2 is calculated, and according to M=△U×Rv / U1. It should be noted that in the embodiment of the present application, in addition to using △U to calculate the index M, any relevant parameters of △U can also be used to calculate the index M. For example, according to △U=U2-U1=I×Rct and I=U1 / Rv, △U can be converted into a charge transfer resistance Rct, so that Rct is used to evaluate the polarization performance of the second electrode 120. Among them, the internal resistance Rv of the voltmeter 130 can be measured with an ohmmeter.

[0095] Table 1 shows the test results of two different types of reference electrodes. Among them, the internal resistance of the voltmeter is 2.2GΩ. The first type of electrode shown in Table 1 is a filamentary copper wire lithium-plated electrode, which is obtained by, for example, using a 10% SOC LFP pole piece as the positive electrode, a 50-micron diameter copper wire as the negative electrode, and plating lithium for 1 hour using a constant current of 20 microamperes. The second type of electrode shown in Table 1 is a sheet-like 50% SOC LFP pole piece, which is, for example, adjusting the positive electrode LFP and the negative electrode graphite battery cell (nominal voltage 2.5V-3.65V) to 50% SOC, then disassembling the battery cell to remove the LFP pole piece, and cutting it into pole pieces with a width of 0.6mm and a length of 1cm with scissors. Two electrodes of each type are made, namely, copper wire lithium-plated pole piece 1, copper wire lithium-plated pole piece 2, 50% SOC LFP pole piece 1, and 50% SOC LFP pole piece 2.

[0096] Table 1

[0097]

[0098] The polarization size of the electrode is related to the type of active material on the electrode surface, the BET and other physical and chemical properties of the active material, the electrode size, etc. The polarization index M proposed in the embodiment of the present application is a quantitative index of the polarization size of the electrode, which can more accurately evaluate the polarization performance of various electrodes.

[0099] The index for representing the polarization performance of the electrode provided in the embodiment of the present application, such as M=△U×Rv / U1, can quantify the polarization performance of the electrode and improve the accuracy of the test results. According to the index, the polarization performance of the electrode can be judged. For example, the index can be determined by the following method 200. For example, Figure 5As shown, method 200 includes some or all of the following steps.

[0100] In step S210, the voltage parameters of the test loop are obtained.

[0101] The test circuit includes a first electrode 110 , a second electrode 120 , and a voltmeter 130 connected between the first electrode 110 and the second electrode 120 . The first electrode 110 and the second electrode 120 are immersed in an electrolyte.

[0102] The voltage parameter includes a first voltage measured by the voltmeter 130 when the area of ​​the second electrode 120 immersed in the electrolyte is a first area, and a second voltage measured by the voltmeter 130 when the area of ​​the second electrode 120 immersed in the electrolyte is a second area.

[0103] In step S220 , an index for representing the polarization performance of the second electrode 120 is determined according to the voltage parameter.

[0104] In one implementation, the indicator is determined based on the voltage difference between the first voltage and the second voltage, the internal resistance of the voltmeter 130 , and the first voltage.

[0105] In one implementation, the indicator is equal to a ratio of a product of the voltage difference and an internal resistance of the voltmeter 130 to the first voltage.

[0106] It can be understood that the specific details of determining the indicator M in the test method 200 can refer to the description of the indicator M in the aforementioned test method 200, and for the sake of brevity, it will not be repeated here.

[0107] The present application also provides a reference electrode, which is used to be arranged between the positive electrode and the negative electrode of the battery. The dimension of the reference electrode in its width direction is less than or equal to a preset value, and the preset value is negatively correlated with the lithium ion transmission performance between the positive electrode and the negative electrode. The width direction is perpendicular to the extension direction of the electrode ear of the reference electrode.

[0108] Generally, the larger the area of ​​the reference electrode, the smaller its polarization. However, since the reference electrode is usually arranged between the positive electrode and the negative electrode of the battery, the larger the area of ​​the reference electrode, the greater the hindrance to the lithium ion transmission between the positive electrode and the negative electrode, which is not conducive to the transmission of lithium ions. For this reason, the area of ​​the reference electrode in the embodiment of the present application is set to be small enough, for example, its width is less than or equal to a preset value, so that its influence on the lithium ion transmission performance between the positive electrode sheet and the negative electrode sheet is within an acceptable range. The preset value is, for example, 1 mm.

[0109] In one implementation, the reference electrode includes a metal substrate and an active material covering the surface of the metal substrate. The metal substrate is a metal wire or a carbon fiber. The size of the metal substrate in the width direction is less than or equal to 0.1 mm, and the preset value is 0.2 mm.

[0110] In one implementation, the reference electrode metal substrate and the active material covering the surface of the metal substrate, the metal substrate is a metal foil, and the preset value is 1 mm.

[0111] The present application also provides an electrode assembly, such as Figure 6 As shown, the battery 30 includes a positive electrode sheet 140, a negative electrode sheet 150, and a reference electrode 120 disposed between the positive electrode sheet 140 and the negative electrode sheet 150. The reference electrode 120 includes the second electrode 120 or the reference electrode 120 described in any of the above embodiments; or, the reference electrode 120 includes the second electrode 120 in the test method 100 or the test method 200 described in any of the above embodiments. Optionally, the index for evaluating the reference electrode is within a predetermined range.

[0112] The predetermined range is, for example, less than or equal to 10. That is, the battery 30 includes a positive electrode sheet 140, a negative electrode sheet 150, and a reference electrode 120 with M less than a preset value, for example, a reference electrode 120 with M≤10. The reference electrode 120 is disposed between the positive electrode sheet 140 and the negative electrode sheet 150, and is spaced from the positive electrode sheet 140 and the negative electrode sheet 150 by a separator.

[0113] The reference electrode 120 is used to test the potential of the positive electrode sheet 140 and / or the negative electrode sheet 150 .

[0114] An embodiment of the present application also provides a battery, comprising: the electrode assembly described in any of the above embodiments; and a shell for accommodating the electrode assembly.

[0115] An embodiment of the present application further provides an electrical device, which includes the battery described in any of the above embodiments, and the battery is used to provide electrical energy to the electrical device.

[0116] It should be noted that, under the premise of no conflict, the various embodiments described in this application and / or the technical features in each embodiment can be arbitrarily combined with each other, and the technical solution obtained after the combination should also fall within the protection scope of this application.

[0117] Those of ordinary skill in the art will appreciate that the units and algorithm steps of each example described in conjunction with the embodiments disclosed herein can be implemented in electronic hardware, or a combination of computer software and electronic hardware. Whether these functions are performed in hardware or software depends on the specific application and design constraints of the technical solution. Professional and technical personnel can use different methods to implement the described functions for each specific application, but such implementation should not be considered to be beyond the scope of this application.

[0118] Those skilled in the art can clearly understand that, for the convenience and brevity of description, the specific working processes of the systems, devices and units described above can refer to the corresponding processes in the above method embodiments and will not be repeated here.

[0119] In the several embodiments provided in the present application, it should be understood that the disclosed systems, devices and methods can be implemented in other ways. For example, the device embodiments described above are only schematic. For example, the division of the units is only a logical function division. There may be other division methods in actual implementation, such as multiple units or components can be combined or integrated into another system, or some features can be ignored or not executed. Another point is that the mutual coupling or direct coupling or communication connection shown or discussed can be through some interfaces, indirect coupling or communication connection of devices or units, which can be electrical, mechanical or other forms.

[0120] The units described as separate components may or may not be physically separated, and the components displayed as units may or may not be physical units, that is, they may be located in one place or distributed on multiple network units. Some or all of the units may be selected according to actual needs to achieve the purpose of the solution of the embodiment of the present application.

Claims

1. A method for testing an electrode, characterized in that: The test method includes: constructing a test circuit, the test circuit comprising a first electrode, a second electrode, and a voltmeter connected between the first electrode and the second electrode, the first electrode and the second electrode being immersed in an electrolyte; adjusting the area of ​​the second electrode immersed in the electrolyte to a first area, and obtaining a first voltage measured by the voltmeter; adjusting the area of ​​the second electrode immersed in the electrolyte to a second area, and obtaining a second voltage measured by the voltmeter; The polarization property of the second electrode is determined according to the first voltage and the second voltage.

2. The testing method according to claim 1, characterized in that: The determining the polarization property of the second electrode according to the first voltage and the second voltage includes: An indicator for representing the polarization performance of the second electrode is determined according to a voltage difference between the first voltage and the second voltage, an internal resistance of the voltmeter and / or the first voltage.

3. The testing method according to claim 2, characterized in that: Determining an index representing the polarization performance of the second electrode according to the voltage difference between the first voltage and the second voltage, and the internal resistance of the voltmeter and / or the first voltage, includes: The voltage difference is multiplied by the internal resistance of the voltmeter and divided by the first voltage to obtain the index.

4. The testing method according to claim 3, characterized in that: The method further comprises: At least one of the following parameters of the second electrode is adjusted so that the indicator is within a predetermined range: The type of active material of the second electrode, the specific surface area of ​​the active material, the loading amount of the active material per unit size, and the size of the second electrode.

5. The testing method according to claim 4, characterized in that: The predetermined range is less than or equal to 10, wherein the voltage difference and the first voltage are in units of volts, and the internal resistance of the voltmeter is in units of megohms.

6. The testing method according to any one of claims 1 to 5, characterized in that: The area of ​​the first electrode immersed in the electrolyte is larger than the area of ​​the second electrode immersed in the electrolyte, and the area of ​​the first electrode immersed in the electrolyte remains unchanged during the test.

7. The testing method according to any one of claims 1 to 6, characterized in that: The second electrode is arranged between the positive electrode and the negative electrode of the battery as a reference electrode. The size of the second electrode in its width direction is less than or equal to a preset value, and the preset value is negatively correlated with the lithium ion transmission performance between the positive electrode and the negative electrode. The width direction is perpendicular to the extension direction of the electrode ear of the reference electrode.

8. The testing method according to claim 7, characterized in that: The second electrode includes a metal substrate and an active material covering the surface of the metal substrate. The metal substrate is a metal wire or a carbon fiber. The size of the metal substrate in the width direction is less than or equal to 0.1 mm, and the preset value is 0.2 mm.

9. The testing method according to claim 7, characterized in that: The second electrode includes a metal substrate and an active material covering the surface of the metal substrate. The metal substrate is a metal foil, and the preset value is 1 mm.

10. The testing method according to any one of claims 1 to 9, characterized in that: The electrode is tested multiple times, and the performance of the second electrode is determined according to the voltage difference between the first voltage and the second voltage, including: The performance of the second electrode is determined according to a plurality of the voltage differences obtained from a plurality of tests, wherein the proportion of changes in the area of ​​the second electrode immersed in the electrolyte is the same in the plurality of tests.

11. A method for testing an electrode, characterized in that: The method comprises: Acquire a voltage parameter of a test circuit, the test circuit comprising a first electrode, a second electrode, and a voltmeter connected between the first electrode and the second electrode, the first electrode and the second electrode being immersed in an electrolyte, the voltage parameter comprising a first voltage measured by the voltmeter when an area of ​​the second electrode immersed in the electrolyte is a first area, and a second voltage measured by the voltmeter when an area of ​​the second electrode immersed in the electrolyte is a second area; An index for representing the polarization performance of the second electrode is determined according to the voltage parameter.

12. The testing method according to claim 11, characterized in that: The indicator is determined based on a voltage difference between the first voltage and the second voltage, an internal resistance of the voltmeter, and the first voltage.

13. The testing method according to claim 11 or 12, characterized in that: The indicator is equal to the ratio of the product of the voltage difference and the internal resistance of the voltmeter to the first voltage.

14. A reference electrode, characterized in that The reference electrode is used to be arranged between the positive electrode sheet and the negative electrode sheet of the battery. The size of the reference electrode in its width direction is less than or equal to a preset value, and the preset value is negatively correlated with the lithium ion transmission performance between the positive electrode sheet and the negative electrode sheet. The width direction is perpendicular to the extension direction of the electrode ear of the reference electrode.

15. The reference electrode according to claim 14, characterized in that The reference electrode includes a metal substrate and an active material covering the surface of the metal substrate. The metal substrate is a metal wire or a carbon fiber. The size of the metal substrate in the width direction is less than or equal to 0.1 mm, and the preset value is 0.2 mm.

16. The reference electrode according to claim 14, characterized in that The reference electrode includes a metal substrate and an active material covering the surface of the metal substrate. The metal substrate is a metal foil, and the preset value is 1 mm.

17. An electrode assembly, characterized in that: The electrode assembly includes a positive electrode sheet, a negative electrode sheet, and a reference electrode disposed between the positive electrode sheet and the negative electrode sheet. include: The second electrode in the test method according to any one of claims 1 to 13; and / or, A reference electrode according to any one of claims 14 to 16.

18. The electrode assembly according to claim 17, characterized in that The index for evaluating the reference electrode is within a predetermined range.

19. The electrode assembly according to claim 18, characterized in that The predetermined range is less than or equal to 10.

20. A battery, characterized in that: The battery comprises: The electrode assembly according to any one of claims 17 to 19; and The shell is used to accommodate the electrode assembly.

21. An electrical device, characterized in that: The electrical device comprises: the electrode assembly according to any one of claims 17 to 19; or the battery according to claim 20, wherein the battery is used to provide electrical energy for the electrical device.