Adhesive measuring device for measuring interface adhesive between electrode and separator and adhesive measuring method using same
By designing an adhesion measuring device, the electrode and the separator are immersed in the electrolyte, simulating the internal environment of the secondary battery, solving the problem of difficulty in accurately evaluating the adhesion between the electrode and the separator in the prior art, and realizing the wet state Accurate measurement improves the reliability of measurement.
Patent Information
- Application Number
- CN202380027536.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-11-02
- Filing Date
- 2023-10-30
- Publication Date
- 2024-11-08
Smart Images

Figure CN118922709A_ABST
Abstract
Description
Technical Field
[0001] This application claims the benefit of priority from Korean Patent Application No. 10-2022-0144739, filed on November 2, 2022, the disclosure of which is incorporated herein by reference in its entirety.
[0002] The present invention relates to an adhesion measuring device for measuring the interfacial adhesion between an electrode and a separator and a method for measuring adhesion using the device. Background Art
[0003] Recently, due to the depletion of fossil fuels, rising energy prices, and growing concerns about environmental pollution, the demand for environmentally friendly alternative energy is becoming an indispensable factor in future life. Therefore, research on various power generation technologies such as nuclear power, solar power, wind power, and tidal power is being carried out, and there is also great interest in energy storage devices for more efficient use of the generated energy.
[0004] In particular, with the development of technology and the increase in demand for mobile devices, the demand for batteries as energy sources is rapidly increasing, and research is being conducted on batteries that can meet various demands.
[0005] In terms of battery shape, there is a great demand for square-type secondary batteries and soft-pack secondary batteries, which can be applied to products such as mobile phones due to their thin thickness; in terms of materials, there is a great demand for lithium secondary batteries such as lithium-ion batteries and lithium-ion polymer batteries, which have advantages such as high energy density, discharge voltage and output stability.
[0006] Generally, these secondary batteries are configured with an electrode assembly embedded inside the battery case, the electrode assembly including a positive electrode, a negative electrode and a separator arranged between the positive electrode and the negative electrode, a positive electrode terminal tab and a negative electrode terminal tab welded to the two electrode terminal tabs and sealed to expose them to the outside of the battery case. These electrode terminal tabs are electrically connected to an external device via contacts, and the secondary battery supplies power to the external device via the electrode terminal tabs, or power is supplied to the secondary battery from the external device via the electrode terminal tabs.
[0007] Ensuring the safety of secondary batteries is an important issue in the manufacture and use of secondary batteries. In particular, due to various reasons related to the material properties and manufacturing processes of separators commonly used in secondary batteries, the interfacial adhesion between separators is hindered, resulting in wrinkles in the separators and causing stability problems such as internal short circuits in the wrinkled areas.
[0008] Figure 1 is a photograph showing an electrode assembly having wrinkles on the surface of the separator.
[0009] Reference Figure 1, it can be seen that during the manufacturing process of the secondary battery, after the electrode assembly stacked inside the battery housing is filled with electrolyte, the flow in the process causes the diaphragm to peel off from the electrode interface, resulting in wrinkles in the diaphragm. Because these wrinkles can cause internal short circuits, resulting in low voltage, which not only reduces the voltage efficiency but also causes degradation, these wrinkles can directly lead to stability problems. On the other hand, processes such as lamination or hot pressing can be performed to increase the adhesion between the electrode and the diaphragm, but in this case, excessive drying can lead to lithium plating on the negative electrode, which reduces the performance of the battery. Therefore, it is necessary to evaluate the interfacial adhesion between the electrode and the diaphragm as part of the physical property evaluation during the manufacturing process of secondary batteries.
[0010] Generally, in order to evaluate the interfacial adhesion between the electrode and the separator, the electrode and the separator formed with the electrode composite layer are cut into specific sizes, the electrode and the separator are overlapped with each other, a polyethylene terephthalate (PET) film is sandwiched between the electrode and the separator, and a measurement sample is made by heating and pressurizing with a flat press, and the adhesion is evaluated by separating the electrode and the separator with a universal testing machine (Universal Testing Machine, UTM) equipment. However, in this case, since the adhesion is measured in a dry state, it is difficult to determine the adhesion level between the electrode and the separator wetted by the electrolyte inside the actual secondary battery, and the measurement result shows a higher adhesion than the result measured in a wet state.
[0011] In addition, when the adhesion between the electrode and the separator in a wet state is evaluated by disassembling an actual secondary battery and measuring the adhesion between the obtained electrode and the separator, there is a problem that the electrolyte impregnated in the electrode and the separator volatilizes during the measurement time after disassembly, resulting in results different from the actual level.
[0012] Therefore, in order to more accurately evaluate the interfacial adhesion between electrodes and separators in secondary battery processes, it is necessary to develop a technology that can measure the adhesion of electrodes by simulating the electrode state inside an actual secondary battery. Summary of the invention
[0013] Technical issues
[0014] The present invention aims to solve the above problems and provides an apparatus for evaluating adhesion between an electrode and a separator in an environment equivalent to the conditions in which the electrode and the separator are immersed in an electrolyte in an actual secondary battery, and a method of measuring adhesion using the apparatus.
[0015] Technical Solution
[0016] The present invention provides an adhesion measurement device for measuring the interfacial adhesion between an electrode and a diaphragm. In one example, the adhesion measurement device according to the present invention includes: a fixing fixture having a space for arranging a measurement sample including an electrode and a diaphragm, the space containing an electrolyte to fix the measurement sample immersed in the electrolyte; and an adhesion strength meter, the adhesion strength meter is provided with a clamping member, the clamping member is used to clamp the end area of the diaphragm of the measurement sample, the adhesion strength meter is used to measure the force that separates the diaphragm from the electrode by pulling the clamped diaphragm in a direction perpendicular to the surface of the electrode, and the adhesion measurement device has a structure in which a part of the upper surface of the fixing fixture is recessed in a downward direction to form a receiving portion for receiving the electrolyte, and the adhesion measurement device measures the interfacial adhesion between the electrode and the diaphragm in a wet state by immersing the measurement sample in the electrolyte filled in the receiving portion.
[0017] In a specific example according to the present invention, the fixing jig has a structure including a cover that seals an opening portion of the accommodation portion to prevent volatilization of the electrolyte in the accommodation portion.
[0018] In addition, the fixing fixture includes a first fixing sill formed on the upper surface by protruding upward and bending inward; and a first guide groove formed between the bottom surface of the first fixing sill and the upper surface of the fixing fixture, and the adhesion measuring device has a structure in which the open space of the accommodating portion is closed or opened by slidingly inserting the cover into the open end of the first guide groove.
[0019] In another specific example according to the present invention, the accommodating portion includes a second fixed threshold portion formed by protruding inwardly from the side of the accommodating portion, and a second guide groove formed between a bottom surface of the second fixed threshold portion and a bottom surface of the accommodating portion, wherein the second fixed threshold portion and the second guide groove respectively include a pair of second fixed threshold portions and a pair of second guide grooves arranged face to face in the width direction of the accommodating portion, and the adhesion measuring device has a structure for inserting the measurement sample into the open ends of the pair of second guide grooves in a sliding manner.
[0020] Furthermore, the accommodation portion has a structure formed so that a ratio of a length between the pair of second fixing threshold portions to a length in the width direction of a region where the second fixing threshold portion is not formed is within a range of 0.7 to 0.85.
[0021] Furthermore, the accommodation portion has a structure formed so that the length of the region where the second guide groove is not formed in the width direction is greater than the length between the pair of second guide grooves.
[0022] In another specific example according to the present invention, the fixing jig has a structure in which an open space of the accommodation portion is sealed or opened / closed in such a manner that the cover is rotated by being hingedly connected to the cover.
[0023] In another example according to the present invention, the adhesion measuring device further includes a detection section that detects and displays a force that separates the electrode and the diaphragm of the measurement sample.
[0024] Furthermore, using the aforementioned adhesion measuring apparatus, there is provided an adhesion measuring method for measuring the interfacial adhesion between the electrode and the separator in a wet state.
[0025] In one example according to the present invention, the method includes: immersing the measurement sample in an electrolyte by placing the measurement sample in a fixing fixture containing the electrolyte; fixing the end of the diaphragm of the measurement sample immersed in the electrolyte to a clamp of an adhesion strength tester; and operating the adhesion strength tester to separate the electrode and the diaphragm of the measurement sample immersed in the electrolyte, thereby measuring the interfacial adhesion between the electrode and the diaphragm in a wetted state.
[0026] In a specific example according to the present invention, a measurement sample includes a positive electrode or a negative electrode and a separator obtained by disassembling a secondary battery.
[0027] In another specific example according to the present invention, the composition of the electrolyte is the same as that of the electrolyte stored inside the disassembled secondary battery.
[0028] In still another specific example of the present invention, the secondary battery is a secondary battery that has undergone an activation process.
[0029] In another example according to the present invention, immersing the measurement sample in the electrolyte by placing the measurement sample in a fixing fixture containing the electrolyte includes: attaching a double-sided tape to a surface of an electrode of the measurement sample, and immersing the measurement sample attached to the glass substrate in the electrolyte in a state where the measurement sample attached with the double-sided tape is attached to a surface of the glass substrate.
[0030] In yet another example according to the present invention, immersing the measurement sample in the electrolyte by placing the measurement sample in a fixing fixture containing the electrolyte includes: covering the fixing fixture with a cover to prevent the electrolyte contained in the fixing fixture from volatilizing during a waiting time for a sufficient amount of the electrolyte to be able to immerse the measurement sample immersed in the electrolyte.
[0031] Beneficial Effects
[0032] The adhesion measuring device and the adhesion measuring method using the adhesion measuring device according to the present invention are advantageous in that the interfacial adhesion between the electrode and the separator can be easily measured in an environment equivalent to an actual secondary battery by simulating the conditions inside a secondary battery containing an actual electrolyte, thereby predicting the interfacial adhesion between the electrode and the separator inside an actual secondary battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 is a photograph showing folds obtained by disassembling a conventional secondary battery.
[0034] Figure 2 is a perspective view showing an adhesion measuring device according to an exemplary embodiment of the present invention.
[0035] Figure 3 is a plan view showing a fixing jig according to an exemplary embodiment of the present invention.
[0036] Figure 4 It is shown that the cutting direction is along the A-A' direction. Figure 3 A cross-sectional cut view of the fixing fixture of the fixing fixture.
[0037] Figure 5 is a perspective view illustrating coupling of a fixing fixture and a cover according to an exemplary embodiment of the present invention.
[0038] Figure 6 is a perspective view illustrating coupling of a fixing fixture and a cover according to another exemplary embodiment of the present invention.
[0039] Figure 7 This is a graph showing the results of measuring the adhesion between the negative electrode or the positive electrode and the separator depending on whether the negative electrode or the positive electrode and the separator are impregnated with an electrolyte solution.
[0040] Figure 8 is a graph showing the results of measuring the adhesion between the negative electrode and the separator at different stages of the process.
[0041] Fig. 9 is a flow chart showing the flow of a method for measuring the interfacial adhesion between an electrode and a separator in a wetted state. DETAILED DESCRIPTION
[0042] The present invention may have various modifications and various examples, and specific examples are shown in the drawings and described in detail in the specification. However, it should be understood that the present invention is not limited to specific embodiments, and includes all modifications, equivalents or substitutions within the spirit and technical scope of the present invention.
[0043] The terms "including" or "having" are used herein to indicate the presence of features, quantities, steps, actions, parts or components or combinations thereof described in the specification, and it should be understood that the possibility of the presence or addition of one or more other features, quantities, steps, actions, parts, components or combinations thereof is not excluded in advance. In addition, when a portion of a layer, film, region or plate is disposed "on" another portion, this includes not only the case where one portion is "directly" disposed on the other portion, but also the case where a third portion is inserted therebetween. Conversely, when a portion of a layer, film, region or plate is disposed "below" another portion, this includes not only the case where one portion is "directly" disposed below the other portion, but also the case where a third portion is inserted therebetween. In addition, in the present application, "on" may include not only the case where it is disposed on the upper portion, but also the case where it is disposed on the lower portion.
[0044] The present invention provides an adhesion measuring device for measuring interfacial adhesion between an electrode and a separator and a method for measuring adhesion using the same.
[0045] Generally, the measurement method between the electrode and the separator is to cut the electrode and the separator formed with the electrode composite layer into a specific size, then overlap the electrode and the separator, sandwich the PET film between the electrode and the separator, heat and pressurize with a flat press to make a measurement sample, and then separate the electrode and the separator with a universal testing machine (UTM) equipment to measure the adhesion.
[0046] However, in this case, since the adhesion is measured in a dry state, it is difficult to determine the adhesion level between the electrode and the separator actually wetted by the electrolyte inside an actual secondary battery, and the measurement results show higher adhesion than those measured in an actual electrolyte wet state.
[0047] In addition, when the adhesion between the electrode and the separator in a wet state is measured by disassembling the actual secondary battery and measuring the adhesion between the obtained electrode and the separator, there is a problem that the electrolyte impregnated in the electrode and the separator volatilizes during the measurement time after disassembly, resulting in results different from the actual level.
[0048] Therefore, in order to more accurately evaluate the interfacial adhesion between electrodes and separators in secondary battery processes, it is necessary to develop a technology that can measure the adhesion of electrodes by simulating the electrode state inside an actual secondary battery.
[0049] Therefore, in order to solve the above problems, the present invention provides an apparatus for evaluating adhesion between an electrode and a separator in an environment equivalent to the conditions in which the electrode and the separator are immersed in an electrolyte in an actual secondary battery, and a method of measuring adhesion using the apparatus.
[0050] Hereinafter, an adhesion measuring device for measuring interfacial adhesion between an electrode and a separator according to the present invention, and a method of measuring adhesion using the adhesion measuring device are provided.
[0051] Figure 2 is a perspective view showing an adhesion measuring device according to an exemplary embodiment of the present invention. Figure 2 , an adhesion measuring device 1 according to the present invention includes: a fixing jig 10 having a space for arranging a measurement sample 30 including an electrode 31 and a diaphragm 32, the space containing an electrolyte to fix the measurement sample 30 immersed in the electrolyte; and an adhesion strength meter 20, the adhesion strength meter 20 being provided with a clamping member 21, the clamping member 21 being used to clamp an end region of the diaphragm 32 of the measurement sample 30, and being used to measure a force for separating the diaphragm 32 from the electrode 31 by pulling the clamped diaphragm 32 in a direction perpendicular to a surface of the electrode 31, and the adhesion measuring device 1 having a structure in which a portion of an upper surface of the fixing jig 10 is recessed in a downward direction to form a containing portion 11 for containing the electrolyte, and the adhesion measuring device 1 measures the interfacial adhesion between the electrode 31 and the diaphragm 32 in a wet state by immersing the measurement sample 30 in the electrolyte filled in the containing portion 11.
[0052] In the present invention, the term "measurement sample 30" refers to an object to be measured using the adhesion measurement device 1 according to the present invention, which object may be specifically an electrode 31 assembly. The electrode 31 assembly may include an electrode 31 having an electrode 31 composite layer formed thereon and a separator 32, wherein the electrode 31 may be a positive electrode or a negative electrode having an electrode 31 composite layer formed on one side or both sides of an electrode 31 current collector.
[0053] The fixing fixture 10 may be formed with a receiving portion 11 having a space in which the measurement sample 30 may be placed. The receiving portion 11 may be a space formed by a portion of the upper surface of the fixing fixture 10 being recessed in a downward direction. The space formed by such a recess refers to a space in which the measurement sample 30 may be placed and a space in which the electrolyte may be contained, and the receiving portion 11 may be formed at a predetermined depth so that the electrolyte may be contained therein and the measurement sample 30 may be fully impregnated by the electrolyte. The fixing fixture 10 may be formed of various forms of metal (e.g., carbon steel, stainless steel, aluminum, or alloys thereof), and is not limited to any particular metal.
[0054] Meanwhile, the adhesion strength meter 20 may include a clamp 21 for clamping the end of the diaphragm 32 of the measurement sample 30, and the clamped diaphragm 32 may be pulled in a unidirectional direction to measure the force required to separate the diaphragm 32 from the electrode 31. In one example, the adhesion strength meter 20 may be a typical universal testing machine (UTM), for example, a peel tester. In a specific example, in order to measure the interfacial adhesion between the electrode 31 and the diaphragm 32 of the measurement sample 30, the electrode 31 and the diaphragm 32 of a part of the measurement sample 30 are manually separated, and then the end of the diaphragm 32 separated from the electrode 31 is fixed by the clamp 21 of the adhesion strength meter 20 to pull the diaphragm 32 at an angle of 90° relative to the surface of the electrode 31 to measure the force to peel the diaphragm 32 from the electrode 31 (90° peel test).
[0055] In addition, the clamp 21 of the adhesion strength meter 20 may include a metal jaw face having a grid formed on its surface. During the operation of the adhesion strength meter 20, when the diaphragm 32 is pressed by the clamp 21, the diaphragm 32 may slide. Therefore, by forming a grid on the jaw face of the clamp 21, the fixing force of the clamp 21 on the diaphragm 32 can be increased. The metal jaw face can be formed of various forms of metal (e.g., carbon steel, stainless steel, aluminum, or alloys thereof). In addition, the metal jaw face can have a grid-like pattern having an engraved surface or an embossed surface, and the grid-like pattern can have various lengths, including but not limited to the width length and recessed depth of the engraved pattern or the protruding height of the embossed pattern.
[0056] Figure 3 is a plan view showing a fixing jig according to an exemplary embodiment of the present invention, and Figure 4 It is shown that the cutting direction is along the A-A' direction. Figure 3 A cross-sectional cut view of the fixing fixture. Figure 3 and Figure 4, the fixing jig 10 may have a structure including a cover 40, and the cover 40 seals the opening of the receiving portion 11 to prevent the electrolyte contained in the receiving portion 11 from volatilizing. In a specific example, since a time interval is formed between when the secondary battery is disassembled and when the secondary battery is placed in the receiving portion 11 of the fixing jig 10 containing the electrolyte, and during this time interval, the electrolyte may volatilize into the air, so that the measurement sample 30 obtained by disassembling the secondary battery may be different from the situation inside the secondary battery. In this case, in order to achieve a situation equivalent to the situation inside the secondary battery, a sufficient waiting time may be required to immerse the electrode 31 sample in the electrolyte for a certain period of time so that the electrolyte can fully impregnate the electrode 31 sample. However, during the waiting time, the electrolyte contained in the receiving portion 11 of the fixing jig 10 may volatilize into the air, which may cause the electrode 31 sample to be not fully wetted, and this can be prevented by sealing the opening of the receiving portion 11 of the fixing jig 10 with the cover 40 to prevent the electrolyte from volatilizing.
[0057] Figure 5 is a perspective view showing a combination of a fixing fixture and a cover according to an exemplary embodiment of the present invention. Figure 5 The fixing clamp 10 includes a first fixing threshold portion 12 formed on the upper surface by protruding upward and bending inward, and a first guide groove 13 formed between the bottom surface of the first fixing threshold portion 12 and the upper surface of the fixing clamp 10, and the cover can be inserted into the open end of the first guide groove 13 in a sliding manner, so that the open space of the accommodating portion 11 is sealed or opened / closed.
[0058] For example, the first fixing threshold portion 12 may have a shape formed by protruding upward on the upper surface of the fixing jig 10 and bending inward in a region of the upper surface of the fixing jig 10 where the accommodation portion 11 is not formed. The bottom surface of the first fixing threshold portion 12 has a certain step from the upper surface of the fixing fixture 10, and the first guide groove 13 may be formed between the bottom surface of the first fixing threshold portion 12 and the upper surface of the fixing fixture 10. The depth of the first guide groove 13 corresponds to the length of the bent end of the first fixing threshold portion 12 and is not limited to a certain depth.
[0059] At the same time, a pair of first fixed thresholds 12 and a pair of first guide grooves 13 are arranged face to face and parallel to each other in the width direction of the fixing clamp 10, and a structure is provided in which a cover can be slidably removed at the opening end of the first guide groove 13, so that the open space of the accommodating portion 11 can be sealed or opened / closed.
[0060] Figure 6 is a perspective view showing the coupling of a fixing fixture and a cover according to another exemplary embodiment of the present invention. Figure 6, the fixing fixture 10 can be connected to the cover by a hinge 41, so that the open space of the accommodating portion 11 is sealed or opened / closed in a manner that the cover pivots. The hinge 41 is not limited to a hinge 41 having a specific structure, but can be a hinge 41 including a first mold and a second mold that can rotate relative to each other around an imaginary rotation axis. For example, the first mold can be connected to one side of the fixing fixture 10, and the second mold can be connected to the cover, so that the first mold and the second mold can rotate relative to each other, so that the open space of the accommodating portion 11 of the fixing fixture 10 can be sealed or opened / closed. In addition, the number of hinges 41 connecting the fixing fixture 10 and the cover is not limited to a specific number, but considering the coupling force between the fixing fixture 10 and the cover, it is preferably connected by two or more hinges 41.
[0061] In another example of the present invention, the housing 11 includes a second fixing threshold portion 14 protruding inwardly from a side surface of the housing 11, and a second guide groove 15 formed between a bottom surface of the second fixing threshold portion 14 and a bottom surface of the housing 11, wherein the second fixing threshold portion 14 and the second guide groove 15 respectively include a pair of second fixing threshold portions 14 and a pair of second guide grooves 15 disposed face to face in a width direction of the housing 11, and wherein the measurement sample 30 is inserted into the open ends of the pair of second guide grooves 15 in a sliding manner. The process of measuring the interfacial adhesion between the electrode 31 and the diaphragm 32 of the electrode 31 sample is performed by clamping the end of the diaphragm 32 with the clamping member 21 of the adhesion strength meter 20 and pulling the diaphragm 32 at an angle of 90° to the surface of the electrode 31 to peel the diaphragm 32 from the electrode 31. At this time, if the electrode 31 sample is not fixed, when the diaphragm 32 is removed from the electrode 31, the electrode 31 may move together with the diaphragm 32, making it difficult to perform accurate measurement. Therefore, by providing a separate second fixing threshold portion 14 and second guide groove 15 in the accommodation portion 11, and by inserting the measurement sample 30 into the second guide groove 15 so as to be restrained, the electrode 31 can be fixed so that the electrode 31 does not move along the diaphragm 32 during the process of separating the diaphragm 32 from the electrode 31 by the adhesion strength meter 20. In this case, it is necessary to make the measurement sample 30 have the electrode 31 and the diaphragm 32 of different width lengths so that only the electrode 31 of the measurement sample 30 crosses the second fixing threshold portion 14, and the diaphragm 32 of the measurement sample 30 does not cross the second fixing threshold portion 14.
[0062] Reference Figure 3 and Figure 4 The accommodation portion 11 may be formed such that a ratio of a length w′ between a pair of second fixing threshold portions to a length w in the width direction of a region where the second fixing threshold portion 14 is not formed is in a range of 0.7 to 0.85.
[0063] If the ratio of the width length w' of the accommodating portion 11 formed with the second fixed threshold portion 14 to the length w in the width direction of the accommodating portion 11 without the second fixed threshold portion 14 is greater than 0.85, the electrode 31 of the measurement sample 30 may not be sufficiently spanned by the second fixed threshold portion 14; if the ratio is less than 0.7, it may be smaller than the length of the diaphragm 32 of the measurement sample 30 in the width direction, and therefore an additional process of cutting the diaphragm 32 may be required.
[0064] Meanwhile, in another specific example of the present invention, the structure of the accommodating portion 11 may be such that the length w of the region where the second guide groove 15 is not formed in the width direction is greater than the length w" between the pair of second guide grooves 15. It is a structure in which, after the measurement sample 30 is placed in the space where the second guide groove 15 is not formed in the accommodating portion 11, the measurement sample 30 is inserted into the second guide groove 15 by sliding the measurement sample 30 into the space where the pair of second guide grooves 15 are formed. In order to fix the measurement sample 30 inserted into the second guide groove 15 so that it does not swing left and right, the length w" between the pair of second guide grooves 15 may be formed to be approximately the length of the width of the measurement sample 30. On the other hand, the space where the second guide groove 15 of the accommodating portion 11 is not formed is the space where the measurement sample 30 is placed before being inserted between the pair of second guide grooves 15, so that the operator can easily place the measurement sample 30 in the space where the second guide groove 15 is not formed while clamping the measurement sample 30. The length w of the region where the second guide groove 15 is not formed in the width direction may be formed to be greater than the length of the measurement sample 30 in the width direction. Therefore, the length w" between the pair of second guide grooves 15 is set to a length similar to the length of the measurement sample 30 in the width direction, so that the measurement sample 30 inserted between the pair of second guide grooves 15 is fixed, and the length w in the width direction of the second guide grooves 15 where the accommodation portion 11 is not formed is formed to be longer than the length between the pair of second guide grooves 15, so that the operator can easily place the measurement sample 30 in the accommodation portion 11 while clamping the measurement sample 30.
[0065] The adhesion measurement device 1 may further include a detection section (not shown) for detecting and displaying a force separating the electrode 31 of the measurement sample 30 from the diaphragm 32. The detection section may digitally represent the interfacial adhesion force between the electrode 31 of the measurement sample 30 and the diaphragm 32. This may be a structure provided in the adhesion strength meter 20.
[0066] In addition, the adhesion measurement device 1 may further include a storage unit (not shown). The storage unit may receive and store measurement data of the interfacial adhesion between the electrode 31 and the separator 32 of the measurement sample 30. Optionally, the storage unit may further include a function of database-ing the measurement results, which are divided into various types, such as the type, thickness and ratio of the metal collector, the electrode 31 composite layer and the separator 32. Therefore, based on the databased data, the possibility of wrinkling the separator 32, the possibility of internal short circuit, etc. due to the deterioration of the adhesion between the electrode 31 and the separator 32 inside the actual secondary battery can be predicted.
[0067] Furthermore, the present invention provides a method of measuring the interfacial adhesion between an electrode and a separator in a wet state using the aforementioned adhesion measuring apparatus.
[0068] Fig. 9 : is a flow chart showing the flow of a method for measuring the interfacial adhesion between an electrode and a separator in a wetted state in one example of the present invention. Fig. 9 According to the present invention, an adhesion measurement method for measuring the interfacial adhesion between an electrode and a diaphragm in a wet state includes: immersing the measurement sample in an electrolyte by placing the measurement sample in a fixing fixture containing an electrolyte (S10); fixing the end of the diaphragm of the measurement sample immersed in the electrolyte to a clamp of an adhesion strength tester (S20); and operating the adhesion strength tester to separate the electrode and the diaphragm of the measurement sample immersed in the electrolyte, thereby measuring the interfacial adhesion between the electrode and the diaphragm in a wet state (S30).
[0069] First, the step S10 of immersing the measurement sample in the electrolyte refers to placing the measurement sample including the electrode and the diaphragm in a receiving portion containing the electrolyte so that the electrolyte can impregnate the measurement sample. This step may include a case where the measurement sample is placed in the receiving portion when the electrolyte is in the receiving portion, and a case where the electrolyte is accommodated after the measurement sample is placed in the receiving portion. That is, the electrolyte may be accommodated before the measurement sample is placed in the receiving portion and after the measurement sample is placed in the receiving portion. Preferably, a sufficient amount of electrolyte is added to immerse the measurement sample placed in the receiving portion in the electrolyte.
[0070] In addition, the measurement sample to be immersed in the receiving portion may be immersed alone, or if necessary, a double-sided tape may be attached to the surface of the electrode of the measurement sample, and the measurement sample may be attached to the surface of the glass substrate with the double-sided tape, and the measurement sample attached to the glass substrate may be immersed in the electrolyte. The process of bonding the electrode sample to the glass substrate may include attaching the measurement sample to the glass substrate and pressing it down with a roller 5 to 10 times.
[0071] At the same time, it is necessary to fix the measurement sample so that the measurement sample under test does not move left and right or up and down during the subsequent measurement of the adhesive strength using the adhesive strength tester. This can be achieved by inserting the measurement sample into a pair of second guide grooves located inside the accommodating portion as described above to fix the measurement sample. Specifically, when the accommodating portion is longitudinally divided into an area where a pair of second guide grooves are formed and an area where a pair of second guide grooves are not formed, the operator can place the measurement sample in the area of the accommodating portion where a pair of second guide grooves are not formed, and then slide the measurement sample between the pair of second guide grooves so that the measurement sample is inserted into the pair of second guide grooves.
[0072] In addition, the step S10 of immersing the measurement sample in the electrolyte may include waiting for a certain period of time so that the measurement sample immersed in the electrolyte is immersed in a sufficient amount of electrolyte. The waiting time may include covering the fixing fixture with a cover to prevent the electrolyte from volatilizing during the waiting time. When the measurement sample is disassembled from the secondary battery and transferred to the receiving portion containing the electrolyte, the electrolyte immersed in the measurement sample may volatilize due to exposure to the air, and the waiting time may be required to immerse the measurement sample in the electrolyte for a long enough time to replenish the volatilized electrolyte. Here, the process may further include covering the opening of the receiving portion with a cover to prevent the electrolyte contained in the receiving portion from volatilizing into the air during the waiting time, thereby preventing the electrolyte from being further supplied to the receiving portion. In addition, covering the opening of the receiving portion with a cover can prevent the electrolyte contained in the receiving portion from overflowing due to being blocked by the cover even if the fixing fixture is subjected to an external impact.
[0073] Meanwhile, in the step S10 of immersing the measurement sample in the electrolyte, the measurement sample may include a positive electrode or a negative electrode and a separator obtained by disassembling a secondary battery. Since the present invention is intended to measure the interfacial adhesion between the electrode and the separator wetted in the electrolyte to solve the problem of the separator wrinkling caused by the reduced adhesion between the electrode and the separator inside the actual secondary battery after the electrode assembly embedded in the battery housing is injected with the electrolyte, the measurement sample is characterized in that the measurement sample is obtained by disassembling the electrode assembly embedded in the battery housing.
[0074] At the same time, the electrolyte in the receiving portion can be an electrolyte having the same composition as the electrolyte stored inside the disassembled secondary battery. By setting the composition of the electrolyte in the receiving solution to be the same as the composition of the electrolyte inside the secondary battery, the reliability of the measurement result can be improved by simulating the same situation as the actual situation inside the secondary battery.
[0075] In addition, the secondary battery includes a secondary battery that has undergone an activation process, and the secondary battery that has undergone an activation process can be disassembled to obtain a measurement sample. When the secondary battery undergoes an activation process during the manufacturing process of the secondary battery, a volume flow of the secondary battery is generated by charging and discharging, which may cause the interface adhesion between the electrode and the diaphragm to change, thereby causing the diaphragm to wrinkle. Therefore, the adhesion between the electrode and the diaphragm of the measurement sample obtained by disassembling different types of secondary batteries can be measured based on whether the secondary battery is activated and the degree to which it is activated, and the state of the interface adhesion between the electrode and the diaphragm inside the secondary battery before and after activation or depending on the degree of activation can be predicted based on the result.
[0076] At the same time, the term "activation" used in this article may be understood to include any reaction accompanying the initial charging of a secondary battery, for example, applying a certain amount of electricity to a secondary battery cell that has no electrical properties so that the positive electrode and the negative electrode have electrical properties, and non-limiting examples of reactions accompanying the initial charging may include the formation of an SEI film, partial charging of the battery capacity, and activation of the negative electrode, for example, lithiation of a carbon-based negative electrode active material.
[0077] Next, the present invention includes a step S20 of fixing the end of the diaphragm of the measurement sample immersed in the electrolyte to the clamp of the adhesion strength tester. The electrode and the diaphragm at one end of the measurement sample can be separated first, and then the end of the diaphragm of the measurement sample immersed in the electrolyte solution is fixed to the clamp of the adhesion strength tester. The clamp of the adhesion strength tester can be a typical universal testing machine (UTM), for example, a peel tester, and the clamp can include a metal jaw plate surface, and a grid is formed on the surface of the metal jaw plate surface to prevent the diaphragm fixed by the clamp from sliding.
[0078] Next, the present invention may include step S30 of operating an adhesive strength tester to separate the electrode and the separator of the measurement sample immersed in the electrolyte, thereby measuring the interface adhesiveness between the electrode and the separator in a wet state.
[0079] As a specific example, in order to measure the interfacial adhesion between the electrode and the diaphragm of the measurement sample, the load of the adhesion strength meter is set to a zero base, and the load speed is set to a range of 5 mm / min to 200 mm / min, the electrode and the diaphragm are manually separated in a partial area of the measurement sample, so that the end of the diaphragm separated from the electrode is fixed by the clamp of the adhesion strength meter, and then the adhesion strength meter is operated to pull the diaphragm at a 90° angle to the surface of the electrode, thereby measuring the force to peel the diaphragm from the electrode (90° peel test).
[0080] In addition, the process may include a process of database-forming the measurement results of the interfacial adhesion between the electrode and the separator of various types, thicknesses and proportions of metal current collectors, electrode composite layers and separators. Based on the data recorded in the database, the possibility of separator wrinkling due to deterioration of adhesion between the electrode and the separator or occurrence of internal short circuit inside the actual secondary battery can be predicted.
[0081] Meanwhile, the electrode of the present invention refers to a positive electrode or a negative electrode, wherein the positive electrode is a structure in which a positive electrode active material layer is stacked on one or both sides of a positive electrode current collector. In one example, the positive electrode active material layer includes a positive electrode active material, a conductive material, and a binder polymer, and if necessary, may further include a positive electrode additive commonly used in the art.
[0082] The positive electrode active material may be a lithium-containing oxide, and may be the same or different. As the lithium-containing oxide, a lithium-containing transition metal oxide may be used.
[0083] For example, the lithium-containing transition metal oxide may be selected from Li x CoO2(0.5 <x<1.3)、Li x NiO2(0.5 <x<1.3)、Li x MnO2(0.5 <x<1.3)、Li x Mn2O4(0.5 <x<1.3)、Li x (Ni a Co b Mn c )O2(0.5 <x<1.3,0<a<1,0<b<1,0<c<1,a+b+c=1)、Li x Ni 1-y Co y O2(0.5 <x<1.3,0<y<1)、Li x Co 1-y Mn y O2(0.5 <x<1.3,0≤y<1)、Li x Ni 1-y Mn y O2(0.5 <x<1.3,O≤y<1)、Li x (Ni a Co b Mn c )O4(0.5 <x<1.3,0<a<2,0<b<2,0<c<2,a+b+c=2)、Li x Mn 2-z Ni z O4(0.5 <x<1.3,0<z<2)、Li x Mn 2-z Coz O4 (0.5 < x < 1.3, 0 < z < 2), Li x CoPO4 (0.5 < x < 1.3) and Li x A mixture of one or two or more kinds selected from the group consisting of FePO4 (0.5 < x < 1.3). In addition, the lithium-containing transition metal oxide may be coated with a metal or a metal oxide, for example, aluminum (Al). In addition, one or more of sulfides, selenides, and halides may be used in addition to the lithium-containing transition metal oxide.
[0084] The content of the positive electrode active material in the positive electrode active material layer may be in the range of 94.0 wt% to 98.5 wt%. When the content of the positive electrode active material satisfies the above range, it is beneficial to manufacture a high-capacity battery and provide sufficient positive electrode conductivity or inter-electrode adhesiveness.
[0085] The current collector used in the positive electrode may be any highly conductive metal to which the positive electrode active material slurry can be easily adhered and that does not react within the voltage range of the electrochemical device. Specifically, non-limiting examples of the positive electrode current collector include foils made of aluminum, nickel, or a combination thereof. The positive electrode active material layer further includes a conductive material.
[0086] The binder polymer may be any binder commonly used in the art without limitation. For example, when the binder is soluble in an organic solvent and insoluble in water, the binder may be a water-insoluble polymer, or when the binder is insoluble in an organic solvent and soluble in water, the binder may be a water-soluble polymer. Water-insoluble polymers include polyvinylidene fluoride (PVDF), polyvinylidene chloride (PVDC), polyacrylonitrile (PAN), polypropylene oxide (PPO), polyethylene oxide - polypropylene oxide copolymer (PEO - PPO), polytetrafluoroethylene (PTFE), polyimide (PI), polyetherimide (PEI), styrene - butadiene rubber (SBR), polyacrylate and its derivatives.
[0087] The water-soluble polymer may be one or more selected from the group consisting of various cellulose derivatives, for example, carboxymethyl cellulose (CMC), methyl cellulose (MC), cellulose acetate phthalate (CAP), hydroxypropyl methyl cellulose (HPMC), hydroxypropyl methyl cellulose phthalate (HPMCP), etc.
[0088] The content of the binder polymer is proportional to the content of the conductive material contained in the upper positive electrode active material layer and the lower positive electrode active material layer. This is to impart adhesiveness to the conductive material having a relatively very small particle size compared to the active material. When the content of the conductive material increases, more binder polymer is required, and when the content of the conductive material decreases, less binder polymer can be used.
[0089] The negative electrode is a structure having a negative electrode active material layer stacked on one or both sides of a negative electrode current collector. In one example, the negative electrode active material layer includes a negative electrode active material, a conductive material, and a binder polymer, and if necessary, may further include a negative electrode additive commonly used in the art.
[0090] The negative electrode active material may include a carbon material, lithium metal, silicon or tin. When a carbon material is used as the negative electrode active material, both low crystalline carbon and high crystalline carbon may be used. Examples of low crystalline carbon include soft carbon and hard carbon, while examples of high crystalline carbon include natural graphite, Kish graphite, pyrolytic carbon, mesophase pitch-based carbon fibers, mesophase carbon microbeads, mesophase pitch and high temperature calcined carbon, for example, coke derived from petroleum and coal tar pitch.
[0091] Non-limiting examples of the current collector for the negative electrode include foils made of copper, gold, nickel or copper alloys, or combinations thereof. In addition, the current collector may be a laminated substrate of any of the above materials.
[0092] In addition, the negative electrode may include a conductive material and a binder commonly used in the art.
[0093] The separator may be any porous material used in a lithium secondary battery, for example, the separator may use a polyolefin-based porous film or a non-woven fabric, but is not limited thereto.
[0094] Examples of polyolefin-based porous films include films formed of polyethylene such as high density polyethylene, linear low density polyethylene, low density polyethylene and ultra high molecular weight polyethylene alone or mixtures thereof; and polyolefin-based polymers such as polypropylene, polybutylene and polypentene alone or mixtures thereof.
[0095] In addition to polyolefin-based nonwoven fabrics, the nonwoven fabric can be made of, for example, polyethylene terephthalate, polybutylene terephthalate, polyester, polyacetal, polyamide, polycarbonate, polyimide, polyetheretherketone, polyethersulfone, polyphenylene ether, polyphenylene sulfide, polyphenylene sulfide, polyethylene naphthalene, and polymers (such as polyetheretherketone, polyethersulfone, polyphenylene ether, polyphenylene sulfide, polyphenylene sulfide and polyethylene naphthalene) alone or a mixture thereof.
[0096] The polymer as the porous polymer may be a polyvinylidene fluoride vinyl polymer. The polyvinylidene fluoride vinyl polymer may be polyvinylidene fluoride-co-hexafluoropropylene, polyvinylidene fluoride-trichloroethylene, polyvinylidene fluoride-co-trichloroethylene, polymethyl methacrylate, polybutyl acrylate, polyacrylonitrile, polyvinyl pyrrolidone, polyvinyl acetate, polyethylene-co-vinyl acetate and ethylene vinyl acetate copolymer, polyethylene oxide, polyarylate, cellulose acetate, cellulose acetate butyrate, cellulose acetate propionate, cellulose acetate propionate, cyanoethyl pullulan, cyanoethyl polyvinyl alcohol, cyanoethyl cellulose, cyanoethyl sucrose, pullulan or carboxymethyl cellulose.
[0097] In addition, an adhesive layer including electrospun polymer fibers can be formed on one or both sides of the diaphragm. The electrospun polymer fibers can be selected from the group consisting of polyvinylidene fluoride (PVdF) polymer, styrene-butadiene rubber (SBR), polytetrafluoroethylene (PTFE), polyethylene glycol (PEG), polypropylene glycol (PPG), or polypropylene glycol (PPG), toluene diisocyanate (TDI), polymethyl methacrylate and polyacrylonitrile, polyvinyl pyrrolidone, polyvinyl acetate, ethylene vinyl acetate copolymer, polyethylene oxide and polyethylene oxide, cellulose acetate, cellulose acetate butyrate, cellulose acetate propionate, cyanoethyl amylopectin, cyanoethyl polyvinyl alcohol, cyanoethyl cellulose, cyanoethyl sucrose, amylopectin, carboxymethyl cellulose, acrylonitrile-styrene-butadiene copolymer and polyimide, and can be selected from the group consisting of cyanoethyl sucrose, amylopectin, carboxymethyl cellulose, acrylonitrile-styrene-butadiene copolymer and polyimide, One or two or more mixtures.
[0098] The structure of the nonwoven fabric can be a spunbond nonwoven fabric or a meltblown nonwoven fabric composed of long fibers.
[0099] The thickness of the porous substrate is not particularly limited but may be 5 μm to 50 μm, and the pore size and porosity present in the porous substrate are also not particularly limited but may be 0.01 μm to 50 μm and 10% to 95%, respectively.
[0100] In order to improve the mechanical strength of the separator composed of the porous substrate and suppress a short circuit between the positive electrode and the negative electrode, at least one side of the porous substrate may further include a porous coating layer including inorganic particles and a binder polymer.
[0101] The electrolyte may include an organic solvent and an electrolyte salt, wherein the electrolyte salt is a lithium salt. The lithium salt may include, but is not limited to, lithium salts commonly used in non-aqueous electrolytes for lithium-ion batteries. For example, the lithium salt may include Li + as cations, and may include a group consisting of F - , Cl- Br - ,I - 、NO 3- 、N(CN) 2- , BF 4- , ClO 4- 、AlO 4- 、AlCl 4- PF 6- , SbF 6- , AsF 6- 、BF2C2O 4- ,BC4O 8- 、(CF3)2PF 4- 、(CF3)3PF 3- 、(CF3)4PF 2- 、(CF3)5PF - 、(CF3)6P - CF3SO 3- 、C4F9SO 3- CF3CF2SO 3- 、(CF3SO2)2N - 、(FSO2)2N - CF3CF2(CF3)2CO - 、(CF3SO2)2CH - 、(SF5)3C - 、(CF3SO2)3C - 、CF3(CF2)7SO 3- CF3CO 2- 、CH3CO 2- 、SCN - and (CF3CF2SO2)2N - One or more of the group consisting of ions serve as anions.
[0102] The organic solvent included in the above-mentioned electrolyte may include, but is not limited to, those organic solvents commonly used in electrolytes of secondary batteries, for example, ethers, esters, amides, linear carbonates, cyclic carbonates, etc. may be used alone or in a mixture of two or more. Representatively, the organic solvent may include a carbonate compound as a mixture of cyclic carbonates, linear carbonates, or a mixture thereof.
[0103] Specific examples of cyclic carbonate compounds include any one or a mixture of two or more selected from the group consisting of ethylene carbonate (EC), propylene carbonate (PC), 1,2-butenyl carbonate, 2,3-butenyl carbonate, 1,2-pentenyl carbonate, 2,3-pentenyl carbonate, vinylene carbonate, vinyl ethylene carbonate, and halides thereof. For example, halides include but are not limited to fluoroethylene carbonate (FEC).
[0104] Specific examples of the linear carbonate compound include, but are not limited to, any one or a mixture of two or more selected from the group consisting of dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate, ethyl methyl carbonate (EMC), methylpropyl carbonate and ethylpropyl carbonate.
[0105] Among carbonate-based organic solvents, cyclic carbonates, ethylene carbonate, and propylene carbonate are high-viscosity organic solvents with high dielectric constants, which can better dissociate lithium salts in the electrolyte, and when these cyclic carbonates are mixed with low-viscosity, low-dielectric-constant linear carbonates (e.g., dimethyl carbonate and diethyl carbonate) in an appropriate proportion, an electrolyte with higher conductivity can be made.
[0106] The ether in the organic solvent may be any one or a mixture of two or more selected from the group consisting of dimethyl ether, diethyl ether, dipropyl ether, methyl ether, methyl propyl ether and ethyl propyl ether, but is not limited thereto.
[0107] The ester in the organic solvent may be any one or a mixture of two or more selected from the group consisting of methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, γ-butyrolactone, γ-valerolactone, γ-caprolactone, α-valerolactone and β-caprolactone, but is not limited thereto.
[0108] [Mode for carrying out the invention]
[0109] The present invention will be described in more detail below by way of examples. However, it should be understood that the configuration described in the examples described herein is only one embodiment of the present invention and does not represent all technical concepts of the present invention, and it can be replaced by various equivalents and modifications when submitted.
[0110] <Example>
[0111] Example 1
[0112] The positive electrode active material (LiNi 0.8 Co 0.1 Mn 0.1 O2, NCM811), a conductive material (carbon black) and a binder (polyvinylidene fluoride, PVdF) were added to N-methyl-2-pyrrolidone (NMP) at a weight ratio of 96:2:2, respectively, and mixed to prepare a positive electrode slurry, and the prepared positive electrode slurry was coated on a substrate with a capacity of 3.1 mAh / cm 2 A 12 μm-thick aluminum foil of the positive electrode current collector was used to prepare the positive electrode.
[0113] Artificial graphite, a conductive material (carbon black), and a binder (polyvinylidene fluoride (PVdF)) were added to N-methyl-2-pyrrolidone (NMP) at a weight ratio of 96:2:2, respectively, and then mixed to prepare a negative electrode slurry, and the prepared negative electrode slurry was applied to a substrate having a capacity of 3.1 mAh / cm 2 A 10 μm-thick aluminum foil of the negative electrode current collector was used to prepare the negative electrode.
[0114] Then, at 0.7g / m 2 The spinning solution containing PVdF-HFP (LBG from Arkema, HFP content 5%) was electrospun to form a porous web of ultrafine fibers. 2 The porous web was heated and pressed under a pressure of 100 μm to prepare a 14 μm thick separator.
[0115] Then, a wound electrode assembly is prepared by inserting a separator between the positive electrode and the negative electrode. The electrode assembly is inserted into the battery case, the electrolyte is injected, and the battery case is sealed to manufacture a cylindrical secondary battery with a diameter of 21 mm. The electrolyte is prepared by adding LiPF6 with a concentration of 1.4M to an organic solvent including ethylene carbonate (EC), ethyl methyl carbonate (EMC) and dimethyl carbonate (DMC) in a volume ratio of 20:20:60 (volume ratio). In addition, vinylene carbonate (3vol%) and succinonitrile (1vol%) are mixed in the electrolyte.
[0116] The lithium secondary battery prepared as described above was disassembled and the negative electrode was punched out into 23 mm×120 mm, and the separator in contact with the negative electrode was punched out into 20 mm×120 mm to prepare a measurement sample.
[0117] Example 2
[0118] A measurement sample was prepared in the same manner as in Example 1, except that the electrode of the measurement sample was changed to a negative electrode instead of a positive electrode.
[0119] Example 3 and Example 4
[0120] In Example 3 and Example 4, measurement samples were prepared in the same manner as in Example 1 and Example 2, respectively, except that the thickness of the separator was changed to 13 μm.
[0121] Example 5
[0122] A measurement sample was prepared in the same manner as in Example 2, except that the separator of the lithium secondary battery was changed to a polyethylene separator containing an acrylate-based adhesive mixture having a thickness of 14 μm.
[0123] Specifically, when the total amount of the inorganic material (Al2O3, 97wt%) and the acrylate-based adhesive (SG-L02 from GL Chem, 3wt%) was 100wt%, the acrylate-based adhesive mixture was prepared by adding a fluorinated nonionic surfactant (FC4430 from 3M, 0.001wt%) to solvent water and then stirring.
[0124] Example 6
[0125] The measurement sample was prepared in the same manner as in Example 5, except that the prepared lithium secondary battery was subjected to an activation process. Specifically, the activation process included initial charging (SOC, 3%), followed by degassing, including high temperature aging (60°C, 4 hours) and room temperature aging (12 hours). During room temperature aging, it was further charged to SOC 65%, then fully charged to SOC 100% (4.2V) and discharged to SOC 0% (2.5V).
[0126] Example 7 and Example 8
[0127] In Example 7 and Example 8, measurement samples were prepared in the same manner as in Example 5 and Example 6, respectively, except that the thickness of the separator was changed to 13 μm.
[0128] <Comparative Example>
[0129] Comparative Example 1
[0130] Artificial graphite, a conductive material (carbon black), and a binder (polyvinylidene fluoride (PVdF)) were added to N-methyl-2-pyrrolidone (NMP) at a weight ratio of 96:2:2, respectively, and then mixed to prepare a negative electrode slurry, and the prepared negative electrode slurry was coated on a 3.1 mAh / cm 2 A 10 μm-thick aluminum foil as a negative electrode current collector was used to prepare a negative electrode.
[0131] Then, at 0.7g / m 2 The spinning solution containing PVdF-HFP (LBG from Arkema, HFP content 5%) was electrospun to form a porous web of ultrafine fibers. 2 The porous web was heated and pressed under a pressure of 100 μm to prepare a 14 μm thick separator.
[0132] Then, the separator was stacked on the surface of the negative electrode, and the negative electrode and the separator were bonded using a hot press, pressed at 90°C and 200 kgf for 40 seconds. Subsequently, the negative electrode was punched into a size of 23 mm × 120 mm, and the separator in contact with the negative electrode was punched into a size of 20 mm × 120 mm to prepare a measurement sample.
[0133] Comparative Example 2
[0134] The positive electrode active material (LiNi 0.8 Co 0.1 Mn 0.1 O2, NCM811), a conductive material (carbon black) and a binder (polyvinylidene fluoride, PVdF) were added to N-methyl-2-pyrrolidone (NMP) at a weight ratio of 96:2:2, respectively, and mixed to prepare a positive electrode slurry, and the prepared positive electrode slurry was applied to a positive electrode collector with a capacity of 3.1 mAh / cm 2 A 12 μm thick aluminum foil was used to prepare the positive electrode.
[0135] Then, at 0.7g / m 2 The spinning solution containing PVdF-HFP (LBG from Arkema, HFP content 5%) was electrospun to form a porous web of ultrafine fibers. 2 The porous web was heated and pressed under a pressure of 100 μm to prepare a 14 μm thick separator.
[0136] Then, the separator was stacked on the surface of the negative electrode, and the negative electrode and the separator were bonded using a hot press, pressed at 90°C and 200 kgf for 40 seconds. Subsequently, the negative electrode was punched into a size of 23 mm × 120 mm, and the separator in contact with the negative electrode was punched into a size of 20 mm × 120 mm to prepare a measurement sample.
[0137] Comparative Examples 3 and 4
[0138] Measurement samples were prepared in the same manner as in Comparative Examples 1 and 2, except that the thickness of the separator was changed to 13 μm in Comparative Examples 3 and 4, respectively.
[0139] Comparative Example 5
[0140] A measurement sample was prepared in the same manner as in Comparative Example 1, except that the separator was changed to a polyethylene separator containing an acrylate-based adhesive mixture having a thickness of 14 μm.
[0141] Specifically, when the total amount of the inorganic material (Al2O3, 97wt%) and the acrylate-based adhesive (SG-L02 from GL Chem, 3wt%) was 100wt%, the acrylate-based adhesive mixture was prepared by adding a fluorinated nonionic surfactant (FC4430 from 3M, 0.001wt%) to solvent water and then stirring.
[0142] Comparative Example 6
[0143] A measurement sample was prepared in the same manner as in Comparative Example 5, except that the thickness of the separator was changed to 13 μm.
[0144] <Experimental Example>
[0145] 1) Measure the adhesion between the electrode and the separator under dry or wet conditions.
[0146] The interfacial adhesion between the electrode and the separator of the measurement samples in Examples 1 to 4 and Comparative Examples 1 to 4 was measured using a UTM (LLOYD Instruments LF Plus) instrument.
[0147] Specifically, in Examples 1 to 4, the measurement sample was fixed to a fixing jig not immersed in an electrolyte, the measurement sample was immersed in the electrolyte so that the measurement sample was immersed in the electrolyte for about 1 hour, and then the interface adhesion between the electrode and the separator was measured. In contrast, in Comparative Examples 1 to 4, the measurement sample was fixed to a fixing jig not immersed in the electrolyte, and the interface adhesion between the electrode and the separator was immediately measured.
[0148] Then, the membranes of the measurement samples of Examples 1 to 4 and Comparative Examples 1 to 4 fixed to the fixing jig were fixed to the clamp of the UTM instrument, and the UTM instrument was operated to pull one side of the membrane at a speed of 100 mm / min, thereby measuring the force of peeling the membrane from the electrode. At this time, the measurement angle of the electrode and the membrane was 90°.
[0149] In this case, three measurement samples were prepared for each of Examples 1 to 4 and Comparative Examples 1 to 4, respectively, and the adhesion of each measurement sample was measured using the above-mentioned 90° peel test, and an average value was obtained, and the results are as follows: Figure 7 shown.
[0150] Reference Figure 7 , the average adhesion between the negative electrode and the separator of Comparative Example 1 prepared by the dry bonding process was about 63 gf / 20 mm, while the average adhesion between the negative electrode and the separator of Example 1 prepared by the wet bonding process was about 0.5 gf / 20 mm.
[0151] In addition, the average adhesion between the positive electrode of Comparative Example 2 prepared by the dry bonding process and the separator was about 141 gf / 20 mm, while the average adhesion between the positive electrode of Example 2 prepared by the wet bonding process and the separator was about 5 gf / 20 mm.
[0152] It can be seen that the dry bonding process without electrolyte wetting improves the adhesion between the negative electrode and the separator, but the wet bonding process with electrolyte wetting reduces the adhesion between the negative electrode and the separator, and the interfacial adhesion between the positive electrode or negative electrode and the separator immersed in the electrolyte (for example, inside a real secondary battery) is very different from the interfacial adhesion between the positive electrode or negative electrode and the separator prepared without electrolyte wetting.
[0153] This makes it necessary to evaluate the interfacial adhesion between the electrode and the separator in an electrolyte-wetted environment under the same conditions as those inside an actual secondary battery, and it has the effect of measuring the results of the interfacial adhesion between the electrode and the separator in an electrolyte-wetted state by simulating the conditions inside an actual secondary battery, thereby increasing the reliability of predicting changes in adhesion between the electrode and the separator that occur inside an actual secondary battery.
[0154] At the same time, refer to Figure 7 , the average adhesion between the negative electrode and the separator of Comparative Example 3 prepared by the dry bonding process was about 40 gf / 20 mm, while the average adhesion between the negative electrode and the separator of Example 3 prepared by the wet bonding process was about 3 gf / 20 mm.
[0155] In addition, the average adhesion between the positive electrode and the separator of Comparative Example 4 prepared by the dry bonding process was about 71 gf / 20 mm, while the average adhesion between the positive electrode and the separator of Example 2 prepared by the wet bonding process was about 4 gf / 20 mm.
[0156] Examples 3 and 4 and Comparative Examples 1 and 4 are the ones that measure the adhesion between the negative electrode or positive electrode and the separator under the same conditions as Examples 1 and 2 and Comparative Examples 1 and 2, except that the only difference is the thickness of the separator. It can be seen that Examples 3 and 4 and Comparative Examples 3 and 4 exhibit similar adhesion behaviors to those of Examples 1 and 2 and Comparative Examples 1 and 2 above, except that the gravity to which Examples 3 and 4 and Comparative Examples 3 and 4, in which the thickness of the separator is relatively thin, is less than the gravity to which Examples 1 and 2 and Comparative Examples 1 and 2, in which the thickness of the separator is relatively thick, is subjected, resulting in a relatively small value of the adhesion between the electrode and the separator. In other words, it can be seen that Comparative Examples 3 and 4, which undergo a dry bonding process, show significant differences in the amount of bonding when compared with Examples 3 and 4, which undergo a wet bonding process, respectively.
[0157] Therefore, even if the thickness of the membrane is different, the results of measuring the adhesion between the electrode and the membrane under non-wetting and wetting electrolyte conditions have large deviations, so it is necessary to measure the adhesion between the electrode and the membrane under the same electrolyte wetting conditions as inside the actual secondary battery, which can improve the reliability of predicting whether the membrane will wrinkle inside the actual secondary battery.
[0158] 2) Measuring the adhesion between electrode and separator at different process steps
[0159] The interfacial adhesion between the electrode and the separator of the measurement samples in Examples 5 to 8 and Comparative Examples 5 and 6 was measured using a UTM (LLOYD Instruments LF Plus) instrument.
[0160] Specifically, in Examples 5 and 7, the measurement sample obtained by disassembling the lithium secondary battery that has not undergone the activation process is fixed to the receiving portion of the fixing fixture that is not immersed in the electrolyte, and the measurement sample is immersed in the electrolyte for about 1 hour to impregnate the measurement sample with the electrolyte, and then the interface adhesion between the negative electrode and the separator is measured. At the same time, in Examples 6 and 8, the measurement sample obtained by disassembling the lithium secondary battery that has undergone the activation process is contained in a fixing fixture containing an electrolyte as in Examples 5 and 7, immersed in the electrolyte, and the interface adhesion between the negative electrode and the separator is measured. On the other hand, in Comparative Examples 5 and 6, the measurement sample is fixed in the receiving portion of the fixing fixture that is not immersed in the electrolyte, and the interface adhesion between the negative electrode and the separator is immediately measured.
[0161] Then, the separators of the measurement samples of Examples 5 to 8 and Comparative Examples 5 to 6 fixed to the fixing fixture were fixed to the clamp of the UTM instrument, and the UTM instrument was operated to pull one side of the separator at a speed of 100 mm / min to measure the force of the separator peeling from the negative electrode. At this time, the measurement angle of the electrode and the separator was 90°.
[0162] In this case, three measurement samples were prepared for each of Examples 5 to 8 and Comparative Examples 5 to 6, respectively, and the adhesion of each measurement sample was measured using the above-mentioned 90° peel test, and an average value was obtained, and the results are as follows: Figure 8 shown.
[0163] Reference Figure 8 , the average adhesion between the negative electrode and the separator of Example 5 prepared by the dry bonding process was about 14.5 gf / 20 mm, while the average adhesion between the negative electrode and the separator of Example 6 prepared by the wet bonding process and the lithium secondary battery prepared by disassembly without the activation process was about 1.5 gf / 20 mm. Meanwhile, the average adhesion between the negative electrode and the separator of Example 6 prepared by the wet bonding process and the lithium secondary battery prepared by disassembly for the activation process was about 4.5 gf / 20 mm.
[0164] As shown in Example 1 above, the dry bonding process improves the adhesion between the negative electrode and the separator, but the wet bonding process in which the electrolyte is wetted reduces the adhesion between the negative electrode and the separator, and the interfacial adhesion between the negative electrode and the separator immersed in the electrolyte (for example, inside a real secondary battery) is significantly different from the interfacial adhesion between the positive electrode or the negative electrode and the separator prepared without being wetted with the electrolyte.
[0165] This makes it necessary to evaluate the interfacial adhesion between the negative electrode and the separator under wetting conditions that simulate the same conditions inside a real secondary battery, which can improve the reliability of the prediction of the adhesion between the electrode and the separator that occurs inside a real secondary battery.
[0166] On the other hand, by examining the adhesion behaviors of Example 5 prepared by disassembling a lithium secondary battery without performing an activation process and Example 6 prepared by disassembling a lithium secondary battery performing an activation process, it can be seen that Example 6 shows higher adhesion than Example 5. This indicates that the interfacial adhesion between the negative electrode and the separator is improved by various factors during the stepwise charge and discharge process, the aging process, and the degassing process.
[0167] In addition, in each step of the activation process of the secondary battery, by measuring the adhesion between the electrode and the separator under a wet condition of a measurement sample made of a lithium secondary battery manufactured under different conditions, and based on the measurement results, the adhesion behavior between the internal electrode and the separator of the secondary battery can be predicted in advance according to the different conditions of each step of the activation process, thereby preventing the separator from wrinkling in each step of the activation process.
[0168] Reference Figure 7 , the average adhesion between the negative electrode and the separator of Example 6 prepared by the dry bonding process was about 3.5 gf / 20 mm, while the average adhesion between the negative electrode and the separator of Example 7 prepared by the wet bonding process and the lithium secondary battery prepared by disassembly without the activation process was about 0.9 gf / 20 mm. On the other hand, the average adhesion between the negative electrode and the separator of Example 8 prepared by the wet bonding process and the lithium secondary battery prepared by disassembly for the activation process was about 1.3 gf / 20 mm.
[0169] Examples 7 to 8 and Comparative Example 6, which are different from Examples 5 to 7 and Comparative Example 5 only in the thickness of the separator, show similar behavior to the adhesion results of Examples 5 to 7 and Comparative Example 5, except that Examples 7 to 8 and Comparative Example 6, which have relatively large thicknesses, have relatively higher adhesion than Examples 5 to 7 and Comparative Example 5, respectively. That is, Comparative Example 6, which has undergone a dry bonding process, has a significant difference in the amount of adhesion compared to Examples 7 and 8 prepared by a wet bonding process. This means that, as described above in Examples 5 to 6 and Comparative Example 5, the results of measuring the adhesion between the electrode and the separator under conditions without being wetted with an electrolyte and under conditions of being wetted with an electrolyte have a large deviation, so it is necessary to measure the adhesion between the electrode and the separator under conditions of being wetted with an electrolyte (which is the same as the inside of an actual secondary battery) to improve the reliability of predicting whether the separator is wrinkled inside an actual secondary battery.
[0170] In addition, Example 8 prepared by disassembling a secondary battery that has been subjected to an activation process shows higher adhesion than Example 7 prepared by disassembling a secondary battery that has not been subjected to an activation process. It is expected that in the activation process, the adhesion between the negative electrode and the separator is improved by various factors. At the same time, when the adhesion behavior is compared with Examples 5 and 6 having separators of different thicknesses, it can be seen that the thicker the separator, the greater the deviation in adhesion, depending on whether the activation process is performed.
[0171] The results show that the adhesion between the negative electrode and the separator changes depending on whether the electrolyte is wetted, whether it is removed from the secondary battery undergoing the activation process, and the thickness of the separator. Therefore, by setting not only the electrolyte wetting conditions to be the same as those inside the actual secondary battery, but also the activation process conditions and the separator thickness to be the same as those inside the actual secondary battery, the adhesion between the negative electrode and the separator can be measured, and the reliability of predicting the adhesion between the negative electrode and the separator inside the actual secondary battery under various conditions based on the results can be improved.
[0172] [reference numerals]
[0173] 1: Adhesion measurement device
[0174] 10: Fixing fixture
[0175] 11: Accommodation
[0176] 12: First fixed threshold
[0177] 13: First guide groove
[0178] 14: Second fixed threshold
[0179] 15: Second guide groove
[0180] 20: Adhesion Strength Meter
[0181] 21: Clamping parts
[0182] 30: Measurement samples
[0183] 31: Electrode
[0184] 32: Diaphragm
[0185] 40: Cover
[0186] 41: Hinge
Claims
1. An adhesion measuring device, comprising: a fixing jig having a space for accommodating a measurement sample including an electrode and a diaphragm, the space containing an electrolyte to fix the measurement sample immersed in the electrolyte; as well as an adhesive strength meter provided with a clamp for clamping an end region of the diaphragm of the measurement sample, the adhesive strength meter for measuring a force for separating the diaphragm from the electrode by pulling the clamped diaphragm in a direction perpendicular to a surface of the electrode, and The adhesion measuring device has a structure in which a portion of the upper surface of the fixing jig is recessed in a downward direction to form a receiving portion for receiving the electrolyte, and The adhesion measurement device measures the interfacial adhesion between the electrode and the separator in a wet state by immersing the measurement sample in the electrolytic solution filled in the housing.
2. The adhesion measuring device according to claim 1, wherein The fixing jig has a structure including a cover that seals an opening portion of the accommodation portion to prevent the electrolyte in the accommodation portion from volatilizing.
3. The adhesion measuring device according to claim 2, wherein: The fixing fixture includes a first fixing threshold portion formed on the upper surface by protruding upward and bending inward; and a first guide groove formed between a bottom surface of the first fixing threshold portion and the upper surface of the fixing fixture, and The adhesion measuring device has a structure in which the open space of the accommodation portion is closed or opened by the cover being inserted into the open end of the first guide groove in a sliding manner.
4. The adhesion measuring device according to claim 1, wherein The receiving portion includes a second fixing threshold portion formed by protruding inwardly at a side surface of the receiving portion, and a second guide groove formed between a bottom surface of the second fixing threshold portion and a bottom surface of the receiving portion, The second fixed threshold portion and the second guide groove respectively include a pair of second fixed threshold portions and a pair of second guide grooves arranged face to face in the width direction of the accommodation portion, and The adhesion measurement device has a structure in which the measurement sample is inserted into the open ends of the pair of second guide grooves in a sliding manner.
5. The adhesion measuring device according to claim 4, wherein The accommodation portion has a structure formed so that a ratio of a length between the pair of second fixing threshold portions to a length of a region in which the second fixing threshold portion is not formed in the width direction is within a range of 0.7 to 0.
85.
6. The adhesion measuring device according to claim 4, wherein The accommodation portion has a structure formed so that a length of a region in which the second guide groove is not formed in the width direction is greater than a length between the pair of second guide grooves.
7. The adhesion measuring device according to claim 2, wherein: The fixing jig has a structure in which the open space of the accommodation portion is sealed or opened / closed by being hinge-connected to the cover so that the cover is rotated.
8. The adhesion measuring device according to claim 2, wherein: The adhesion measurement device further includes a detection section that detects and displays a force that separates the electrode and the diaphragm of the measurement sample. 9 . An adhesion measurement method for measuring interfacial adhesion between an electrode and a separator in a wet state by using the adhesion measurement apparatus according to claim 1 .
10. The adhesion measurement method according to claim 9, comprising: immersing the measurement sample in the electrolyte by placing the measurement sample in a fixing fixture containing the electrolyte; fixing an end portion of the separator of the measurement sample immersed in the electrolyte to a clamp of an adhesive strength tester; as well as The adhesive strength tester is operated to separate the electrode and the separator of the measurement sample immersed in an electrolyte, thereby measuring the interface adhesiveness between the electrode and the separator in a wet state.
11. The adhesion measurement method according to claim 10, wherein: The measurement sample includes a positive electrode or a negative electrode and a separator obtained by disassembling a secondary battery.
12. The adhesion measurement method according to claim 11, wherein: The composition of the electrolyte is the same as that of the electrolyte stored inside the disassembled secondary battery.
13. The adhesion measurement method according to claim 11, wherein: The secondary battery is a secondary battery that has been subjected to an activation process.
14. The adhesion measurement method according to claim 10, wherein: By placing the measurement sample in a fixing fixture containing the electrolyte, immersing the measurement sample in the electrolyte comprises: A double-sided tape is attached to the surface of the electrode of the measurement sample, and the measurement sample attached to the glass substrate is immersed in the electrolyte in a state where the measurement sample to which the double-sided tape is attached is attached to the surface of a glass substrate.
15. The adhesion measurement method according to claim 10, wherein: By placing the measurement sample in a fixing fixture containing the electrolyte, immersing the measurement sample in the electrolyte comprises: The fixing jig is covered with a cover to prevent the electrolyte contained in the fixing jig from volatilizing during a waiting time for enabling a sufficient amount of the electrolyte to impregnate the measurement sample immersed in the electrolyte.