Positive pole piece, electrochemical device and electric device
Patent Information
- Application Number
- CN202380028729.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2043-03-28
AI Technical Summary
The crystal structure of commercial lithium cobalt oxide cathode materials is unstable at high voltages, resulting in capacity fading. Existing modification methods are ineffective and cannot achieve stable cycle performance.
By controlling the aspect ratio of lithium cobalt oxide particles with a P63mc crystal structure within the range of 3 to 9, the active surface area is reduced and electrolyte side reactions are suppressed, and by introducing Mn, Ni and other elements and lithium with an R-3m crystal structure Cobalt oxide particles improve structural stability and form a lamellar morphology to reduce cycle attenuation.
Significantly improves the cycle performance and energy density of electrochemical devices at high voltages, and has both good kinetic performance and capacity retention.
Smart Images

Figure CN118922962A_ABST
Abstract
Description
Positive electrode sheet, electrochemical device and power-consuming device Technical Field
[0001] The present application relates to the field of battery technology, and in particular to a positive electrode sheet, an electrochemical device, and an electrical device. Background Art
[0002] The crystal structure of currently commercialized lithium cobalt oxide cathode materials is extremely unstable at high voltages, accompanied by severe capacity decay, which prevents them from fully realizing their theoretical capacity. Although modifications to lithium cobalt oxide cathode materials, such as doping (Al, Mg, Ti, etc.) and coating (Al2O3, MgO, etc.), can alleviate the problem of rapid capacity decay at high voltages to a certain extent, the improvement effect is not significant, and stable cycling performance at high voltages cannot be achieved.
[0003] Summary of the Invention
[0004] In view of the above-mentioned problems existing in the prior art, the present application provides a positive electrode plate and an electrochemical device and an electrical device including the positive electrode plate, so as to improve the cycle performance of the electrochemical device under high voltage.
[0005] In a first aspect, the present application provides a positive electrode plate, which includes a positive electrode current collector and a positive electrode active material layer located on the surface of the positive electrode current collector, the positive electrode active material layer contains a positive electrode material, and the positive electrode material includes a first lithium cobalt oxide particle having a P63mc crystal structure. In a cross-section of the positive electrode active material layer perpendicular to the surface of the positive electrode current collector, the aspect ratio a / b of the cross-section of the first lithium cobalt oxide particle satisfies: 3≤a / b≤9, wherein a is the longest diameter of the cross-section of the first lithium cobalt oxide particle, and b is the length of the short diameter in the cross-section of the first lithium cobalt oxide particle that is perpendicular to and bisects its longest diameter.
[0006] Under high voltage, lithium cobalt oxide with a P63mc crystal structure is less susceptible to spinel phase transitions and has higher discharge specific capacity. However, electrochemical devices using this type of cathode material also face the problem of rapid cycle decay. The inventors of this application have discovered that the cycle decay failure of electrochemical devices using lithium cobalt oxide cathode materials with a P63mc crystal structure is largely due to the lack of spinel phase protection on the active surface, which makes the electrolyte susceptible to side reactions on the active surface and causes failure. This application controls the aspect ratio of lithium cobalt oxide particles with a P63mc crystal structure within the range of 3 to 9. On the one hand, the lithium cobalt oxide particles have a relatively small active surface area, reducing the direct contact area with the electrolyte, thereby suppressing the occurrence of interfacial side reactions with the electrolyte. On the other hand, the lithium cobalt oxide particles with an aspect ratio within the above range tend to have a lamellar morphology. After cold pressing of the positive electrode sheet, they have an orientation, with the grain plane being an inactive surface and tending to be parallel to the current collector, which also helps to reduce the cycle decay caused by side reactions. When the value of a / b is too high, the migration barrier of lithium ions increases, which is also not conducive to the performance of the electrochemical device.
[0007] In some embodiments, 4≤a / b≤8. In this way, the electrochemical device can have both good cycle performance and kinetic performance at high voltage.
[0008] In some embodiments, the first lithium cobalt oxide particles have an average particle size of 5 μm to 20 μm.
[0009] In some embodiments, the first lithium cobalt oxide particles have a lamellar morphology.
[0010] In some embodiments, cracks exist within the cross-section of the first lithium cobalt oxide particles. During charge and discharge, the layers of lithium cobalt oxide with a P63mc crystal structure expand and contract by approximately 10%. These cracks can release lattice stress during charge and discharge, reducing further material breakage during cycling.
[0011] In some embodiments, the first lithium cobalt oxide includes Mn elements and Ni elements.
[0012] In some embodiments, the molar percentage of the Mn element in the first lithium cobalt oxide is 0.05% to 10% based on the molar amount of the metal elements excluding the Li element in the first lithium cobalt oxide.
[0013] In some embodiments, the molar percentage of Ni in the first lithium cobalt oxide is 0.05% to 10% based on the molar amount of the metal elements excluding Li in the first lithium cobalt oxide.
[0014] In some embodiments, the first lithium cobalt oxide further includes an M element, and the M element includes at least one of Na, Al, Mg, Ti, Zr, Fe, Zn, Nb, Cr, Ca, La, Y, Mo, W, Ta, Sn, V, Ce, Sr, Ge, Ga, Pb, Ba, or Cu. The introduction of the M element can further improve the structural stability of the material.
[0015] In some embodiments, the molar percentage of the M element in the first lithium cobalt oxide is 0.01% to 10% based on the molar amount of the metal elements excluding the Li element in the first lithium cobalt oxide.
[0016] In some embodiments, the first lithium cobalt oxide includes Li x1 Co y1 Ni z1 Mn q M s O 2±n T n , wherein 0.6≤x1≤1.1, 0.8≤y1<1, 0<z1≤0.1, 0<q≤0.1, 0≤s≤0.1, 0≤n≤0.05, M includes at least one of Na, K, Al, Mg, Ti, Zr, Fe, Zn, Nb, Cr, Ca, La, Y, Mo, W, Ta, Sn, V, Ce, Sr, Ge, Ga, Pb, Ba, Pr, Hf, Lu or Cu, and T is a halogen.
[0017] In some embodiments, the positive electrode material further includes second lithium cobalt oxide particles having an R-3m crystal structure. In a cross-section of the positive electrode active material layer perpendicular to the surface of the positive electrode current collector, the cross-sectional aspect ratio (c / d) of the second lithium cobalt oxide particles is between 1 and 1.2, where c is the longest diameter of the cross-section of the second lithium cobalt oxide particle, and d is the length of the shortest diameter of the cross-section of the second lithium cobalt oxide particle perpendicular to and bisecting the longest diameter. By further including second lithium cobalt oxide particles having an R-3m crystal structure with a smaller aspect ratio (c / d) in the positive electrode active material layer, the positive electrode sheet can be improved in terms of capacity. Furthermore, the lamellar morphology of the first lithium cobalt oxide particles can cover and protect the active surfaces of the second lithium cobalt oxide particles, inhibiting side reactions of the electrolyte on their surfaces. This, in turn, improves the cycling performance of the electrochemical device at high voltages while also increasing the energy density of the electrochemical device.
[0018] In some embodiments, in a cross-section of the positive electrode active material layer perpendicular to the surface of the positive electrode current collector, the ratio S1 / S2 between the cross-sectional area S1 of the first lithium cobalt oxide particle and the cross-sectional area S2 of the second lithium cobalt oxide particle satisfies the following: 0.05 ≤ S1 / S2 ≤ 0.45. By controlling S1 / S2 within this range, the present application can achieve both good cycling performance and high capacity in the electrochemical device.
[0019] In some embodiments, 0.1≤S1 / S2≤0.35.
[0020] In some embodiments, the second lithium cobalt oxide particles have an average particle size of 10 μm to 25 μm.
[0021] In some embodiments, the molar percentage of the Co element in the second lithium cobalt oxide is 90% to 100% based on the molar amount of the metal elements excluding the Li element in the second lithium cobalt oxide.
[0022] In some embodiments, the second lithium cobalt oxide further includes an R element, wherein the R element includes at least one of Ni, Mn, Na, K, Al, Mg, Ti, Zr, Fe, Zn, Nb, Cr, Ca, La, Y, Mo, W, Ta, Sn, V, Ce, Sr, Ge, Ga, Pb, Ba, or Cu. In some embodiments, the molar percentage of the R element in the second lithium cobalt oxide is 0.01% to 10% based on the molar amount of the metal elements other than Li in the second lithium cobalt oxide. The introduction of the R element can improve the structural stability of the second lithium cobalt oxide at high voltages, thereby improving the cycling performance of the electrochemical device at high voltages.
[0023] In some embodiments, the second lithium cobalt oxide includes Li x2 Co y2 R z2 O 2±m T' m At least one of, wherein 0.6≤x2≤1.1, 0.9≤y2≤1, 0≤z2≤0.1, 0≤m≤0.05, R includes at least one of Ni, Mn, Na, K, Al, Mg, Ti, Zr, Fe, Zn, Nb, Cr, Ca, La, Y, Mo, W, Ta, Sn, V, Ce, Sr, Ge, Ga, Pb, Ba, Pr, Hf, Lu or Cu, and T' is a halogen.
[0024] In some embodiments, a mass ratio of the first lithium cobalt oxide particles to the second lithium cobalt oxide particles is 5:95 to 40:60.
[0025] In a second aspect, the present application provides an electrochemical device comprising the positive electrode sheet of the first aspect.
[0026] In a third aspect, the present application provides an electrical device comprising the electrochemical device of the second aspect.
[0027] By controlling the aspect ratio of the first lithium cobalt oxide particles having the P63mc crystal structure within a certain range, the present application can effectively reduce the interfacial side reactions between the positive electrode material and the electrolyte while increasing the capacity of the electrochemical device, thereby improving the cycle performance of the electrochemical device under high voltage. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] FIG1 is an XRD pattern of the positive electrode material of Example 1.
[0029] FIG2 is a SEM image of the positive electrode material of Example 1.
[0030] FIG3 is a cross-sectional SEM image of the positive electrode sheet of Example 1. DETAILED DESCRIPTION
[0031] The embodiments of the present application will be described in detail below. The embodiments of the present application should not be interpreted as limiting the present application.
[0032] In addition, amounts, ratios, and other numerical values are sometimes presented in this application in a range format. It should be understood that such a range format is used for convenience and brevity and should be interpreted flexibly to include not only the values explicitly specified as limits of the range, but also all individual values or sub-ranges encompassed within the range, as if each value and sub-range were explicitly specified.
[0033] In this application, a list of items connected by the terms "at least one of," "at least one of," "at least one of," or other similar terms may mean any combination of the listed items. For example, if items A and B are listed, the phrase "at least one of A and B" means only A; only B; or A and B. In another example, if items A, B, and C are listed, the phrase "at least one of A, B, and C" means only A; or only B; only C; A and B (excluding C); A and C (excluding B); B and C (excluding A); or all of A, B, and C. Item A may contain a single element or multiple elements. Item B may contain a single element or multiple elements. Item C may contain a single element or multiple elements.
[0034] 1. Positive electrode
[0035] The positive electrode sheet provided in the present application includes a positive electrode collector and a positive electrode active material layer located on the surface of the positive electrode current collector, the positive electrode active material layer contains a positive electrode material, and the positive electrode material includes a first lithium cobalt oxide particle having a P63mc crystal structure. In a cross section of the positive electrode active material layer perpendicular to the surface of the positive electrode current collector, the aspect ratio a / b of the cross section of the first lithium cobalt oxide particle satisfies: 3≤a / b≤9, wherein a is the longest diameter of the cross section of the first lithium cobalt oxide particle, and b is the length of the short diameter in the cross section of the first lithium cobalt oxide particle that is perpendicular to and bisects its longest diameter.
[0036] Under high voltage, lithium cobalt oxide with a P63mc crystal structure is less susceptible to spinel phase transitions and has higher discharge specific capacity. However, electrochemical devices using this type of cathode material also face the problem of rapid cycle decay. The inventors of this application have discovered that the cycle decay failure of electrochemical devices using lithium cobalt oxide cathode materials with a P63mc crystal structure is largely due to the lack of spinel phase protection on the active surface, which makes the electrolyte susceptible to side reactions on the active surface and causes failure. This application controls the aspect ratio of lithium cobalt oxide particles with a P63mc crystal structure within the range of 3 to 9. On the one hand, the lithium cobalt oxide particles have a relatively small active surface area, reducing the direct contact area with the electrolyte, thereby suppressing the occurrence of interfacial side reactions with the electrolyte. On the other hand, the lithium cobalt oxide particles with an aspect ratio within the above range tend to have a lamellar morphology. After cold pressing of the positive electrode sheet, they have an orientation, with the grain plane being an inactive surface and tending to be parallel to the current collector, which also helps to reduce the cycle decay caused by side reactions.
[0037] In some embodiments, a / b is 3, 3.5, 4, 4.5, 5, 5.5, 6, 6.5, 7, 7.5, 8, 8.5, 9, or a range consisting of any two of these values. The lithium ion channels of lithium cobalt oxide with a lamellar morphology are two-dimensional channels parallel to the transition metal layer. A larger a / b value means a smaller proportion of active surface area for lithium ion intercalation and deintercalation. When the a / b value is too low, the grains tend to be spherical, the active surface area is larger, the contact area with the electrolyte is correspondingly larger, and side reactions are more likely to occur. When the a / b value is too high, the grains tend to be flattened. Although the active surface area is smaller, the migration barrier of lithium ions increases, which is also not conducive to the performance of the electrochemical device. In some embodiments, 3 ≤ a / b ≤ 8. In some embodiments, 4 ≤ a / b ≤ 8. In some embodiments, 4 ≤ a / b ≤ 6. This allows the electrochemical device to have both good cycling performance and kinetic performance at high voltages.
[0038] In the present application, the aspect ratio a / b of the cross section of the first lithium cobalt oxide particle is obtained by using an ion polisher (CP) to obtain a cross section of the positive electrode active material layer perpendicular to the surface of the positive electrode current collector, and using a scanning electron microscope (SEM) to measure the maximum long diameter of the first lithium cobalt oxide particle in the cross section and the length of the short diameter perpendicular to and bisecting its maximum long diameter. Wherein, the length of the short diameter perpendicular to and bisecting the maximum long diameter is the distance between the perpendicular midline of the maximum long diameter in the cross section and the two intersection points of the surface of the first lithium cobalt oxide particle. For specific statistical testing methods, please refer to the test method in the specific embodiments below.
[0039] In some embodiments, the first lithium cobalt oxide particles have an average particle size of 5 μm to 20 μm. In some embodiments, the first lithium cobalt oxide particles have an average particle size of 5 μm, 8 μm, 10 μm, 15 μm, 20 μm, or a range consisting of any two of these values. In this application, the average particle size of the first lithium cobalt oxide particles is the average value of the longest diameter a of the cross section of the first lithium cobalt oxide particles.
[0040] In some embodiments, the first lithium cobalt oxide particles have a lamellar morphology.
[0041] In some embodiments, cracks exist within the cross-section of the first lithium cobalt oxide particles. During charge and discharge, lithium cobalt oxide with a P63mc crystal structure experiences approximately 10% expansion and contraction between layers. These cracks can release lattice stress during charge and discharge, reducing further material breakage during cycling. In some embodiments, the cracks can be at least one of closed at both ends, closed at one end, open at one end, or extending through the entire particle.
[0042] In some embodiments, the first lithium cobalt oxide includes Mn elements and Ni elements.
[0043] In some embodiments, the molar percentage of the Mn element in the first lithium cobalt oxide is 0.05% to 10% based on the molar amount of the metal elements other than Li in the first lithium cobalt oxide. In some embodiments, the molar percentage of the Mn element is 0.05%, 0.1%, 0.5%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, or a range consisting of any two of these values.
[0044] In some embodiments, the molar percentage of Ni in the first lithium cobalt oxide is 0.05% to 10% based on the molar amount of the metal elements other than Li in the first lithium cobalt oxide. In some embodiments, the molar percentage of Ni is 0.05%, 0.1%, 0.5%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, or a range consisting of any two of these values.
[0045] In some embodiments, the first lithium cobalt oxide further includes an M element, and the M element includes at least one of Na, Al, Mg, Ti, Zr, Fe, Zn, Nb, Cr, Ca, La, Y, Mo, W, Ta, Sn, V, Ce, Sr, Ge, Ga, Pb, Ba, or Cu. The introduction of the M element can further improve the structural stability of the material.
[0046] In some embodiments, the molar percentage of the M element in the first lithium cobalt oxide is 0.01% to 10% based on the molar amount of the metal element other than Li in the first lithium cobalt oxide. In some embodiments, the molar percentage of the M element is 0.01%, 0.1%, 0.5%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, or a range consisting of any two of these values.
[0047] In some embodiments, the first lithium cobalt oxide includes Li x1 Co y1 Ni z1 Mn q M s O 2±n T n , wherein 0.6≤x1≤1.1, 0.8≤y1<1, 0<z1≤0.1, 0<q≤0.1, 0≤s≤0.1, 0≤n≤0.05, M comprises at least one of Na, K, Al, Mg, Ti, Zr, Fe, Zn, Nb, Cr, Ca, La, Y, Mo, W, Ta, Sn, V, Ce, Sr, Ge, Ga, Pb, Ba, Pr, Hf, Lu, or Cu, and T is a halogen. In the present application, the halogen may be fluorine, chlorine, bromine, or iodine.
[0048] In some embodiments, the positive electrode material further includes second lithium cobalt oxide particles having an R-3m crystal structure. In a cross-section of the positive electrode active material layer perpendicular to the surface of the positive electrode current collector, the cross-sectional aspect ratio (c / d) of the second lithium cobalt oxide particles is between 1 and 1.2, where c is the longest diameter of the cross-section of the second lithium cobalt oxide particle, and d is the length of the shortest diameter of the cross-section of the second lithium cobalt oxide particle perpendicular to and bisecting the longest diameter. By further including second lithium cobalt oxide particles having an R-3m crystal structure with a smaller aspect ratio (c / d) in the positive electrode active material layer, the positive electrode sheet can be improved in terms of capacity. Furthermore, the lamellar morphology of the first lithium cobalt oxide particles can cover and protect the active surfaces of the second lithium cobalt oxide particles, inhibiting side reactions of the electrolyte on their surfaces. This, in turn, improves the cycling performance of the electrochemical device at high voltages while also increasing the energy density of the electrochemical device. In some embodiments, c / d is 1, 1.05, 1.08, 1.1, 1.13, 1.15, 1.16, 1.18, 1.2, or a range consisting of any two of these values. In this application, the aspect ratio c / d of the cross section of the second lithium cobalt oxide particle is measured in the same manner as the aspect ratio a / b of the cross section of the first lithium cobalt oxide particle.
[0049] In some embodiments, in a cross-section of the positive electrode active material layer perpendicular to the surface of the positive electrode current collector, the ratio S1 / S2 between the cross-sectional area S1 of the first lithium cobalt oxide particle and the cross-sectional area S2 of the second lithium cobalt oxide particle satisfies the following: 0.05 ≤ S1 / S2 ≤ 0.44. By controlling S1 / S2 within this range, the present application can achieve both good cycling performance and high capacity in the electrochemical device.
[0050] In some embodiments, S1 / S2 is 0.05, 0.1, 0.13, 0.15, 0.17, 0.2, 0.23, 0.25, 0.27, 0.3, 0.33, 0.35, 0.37, 0.4, 0.45, or a range consisting of any two of these values. In some embodiments, 0.1≤S1 / S2≤0.35.
[0051] In some embodiments, the second lithium cobalt oxide particles have an average particle size of 10 μm to 25 μm. In some embodiments, the second lithium cobalt oxide particles have an average particle size of 10 μm, 12 μm, 14 μm, 15 μm, 18 μm, 20 μm, 22 μm, 25 μm, or a range consisting of any two of these values. In this application, the average particle size of the second lithium cobalt oxide particles is the average of the longest cross-sectional diameter c of the second lithium cobalt oxide particles.
[0052] In some embodiments, the molar percentage of the Co element in the second lithium cobalt oxide is 90% to 100% based on the molar amount of the metal elements excluding the Li element in the second lithium cobalt oxide.
[0053] In some embodiments, the second lithium cobalt oxide further comprises an R element, and the R element comprises at least one of Ni, Mn, Na, K, Al, Mg, Ti, Zr, Fe, Zn, Nb, Cr, Ca, La, Y, Mo, W, Ta, Sn, V, Ce, Sr, Ge, Ga, Pb, Ba, or Cu. In some embodiments, the molar percentage of the R element in the second lithium cobalt oxide is 0.01% to 10% based on the molar amount of the metal elements other than Li in the second lithium cobalt oxide. The introduction of the R element can improve the structural stability of the second lithium cobalt oxide at high voltage, thereby improving the cycling performance of the electrochemical device at high voltage. In some embodiments, the molar percentage of the R element in the second lithium cobalt oxide is 0.01%, 0.1%, 0.5%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, or a range consisting of any two of these values.
[0054] In some embodiments, the second lithium cobalt oxide includes Li x2 Co y2 R z2 O 2±m T'm At least one of, wherein 0.6≤x2≤1.1, 0.9≤y2≤1, 0≤z2≤0.1, 0≤m≤0.05, R includes at least one of Ni, Mn, Na, K, Al, Mg, Ti, Zr, Fe, Zn, Nb, Cr, Ca, La, Y, Mo, W, Ta, Sn, V, Ce, Sr, Ge, Ga, Pb, Ba, Pr, Hf, Lu or Cu, and T' is a halogen.
[0055] In some embodiments, the mass ratio of the first lithium cobalt oxide particles to the second lithium cobalt oxide particles is 5:95 to 40:60. In some embodiments, the mass ratio of the first lithium cobalt oxide particles to the second lithium cobalt oxide particles is 5:95, 10:90, 15:85, 20:80, 30:70, 40:60, or a range consisting of any two of these values.
[0056] In some embodiments, the positive electrode active material layer further comprises a binder and a conductive agent. In some embodiments, the binder comprises at least one of polyvinylidene fluoride, polytetrafluoroethylene, vinylidene fluoride-hexafluoropropylene copolymer, acrylate polymer, polyacrylate, polyamide, or polyurethane. In some embodiments, the conductive agent comprises a carbon-based material such as carbon black, acetylene black, Ketjen black, carbon nanotubes, graphene, or carbon fiber; a metal-based material such as metal powder or metal fiber of copper, nickel, aluminum, silver, etc.; a conductive polymer such as a polyphenylene derivative; or a mixture thereof.
[0057] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver, silver alloy, etc.) on a polymer substrate.
[0058] The present application also provides a method for preparing a first lithium cobalt oxide having a P63mc crystal structure, which comprises subjecting a sodium-containing cobalt oxide and a lithium-containing compound to a solid-phase reaction, wherein the solid-phase reaction temperature is 180°C to 320°C and the solid-phase reaction time is 3 hours to 12 hours. In some embodiments, the solid-phase reaction temperature is 180°C, 190°C, 200°C, 210°C, 250°C, 260°C, 270°C, 300°C, 320°C, or a range consisting of any two of these values. In some embodiments, the solid-phase reaction time is 3 hours, 5 hours, 6 hours, 8 hours, 10 hours, 12 hours, or a range consisting of any two of these values.
[0059] According to some embodiments of the present application, the sodium-containing cobalt oxide has a P63 / mmc structure. According to some embodiments of the present application, the preparation method of the sodium-containing cobalt oxide includes the following steps: S1: providing an oxide precursor containing cobalt, manganese, nickel, and optionally M; S2: mixing the oxide precursor in S1 with a sodium salt and a flux, and calcining the mixture to obtain the sodium-containing cobalt oxide.
[0060] In some embodiments, in S1, the molar percentage of the cobalt element is 90% to 97% based on the total molar content of the metal elements in the oxide.
[0061] In some embodiments, in S2, the flux comprises ammonium chloride and / or boric acid. In some embodiments, the flux comprises 0.5% to 2% by weight, for example, 1% or 1.5% by weight, based on the total weight of the oxide precursor, sodium salt, and flux in S1. The a / b ratio of the first lithium cobalt oxide particles having a P63mc crystal structure is related to the presence or absence of the flux and the amount of flux added. The flux facilitates fusion between particles during the calcination process; a greater amount of flux added facilitates fusion between particles. Therefore, the a / b ratio can be controlled by adjusting the amount of flux added.
[0062] According to some embodiments of the present application, in S2, the calcination temperature is 700°C to 880°C. In the present application, the a / b ratio of the first lithium cobalt oxide particles is related to the sintering conditions of the sodium cobalt oxide in S2. The higher the sintering temperature, the smaller the a / b ratio. This may be because increasing the sintering temperature can promote grain growth, especially vertical growth, thereby increasing the thickness of the material grains and reducing the a / b ratio. Therefore, the a / b ratio can be regulated by adjusting the sintering temperature.
[0063] In some embodiments, in S2, the calcination time is 24 hours to 72 hours. In some embodiments, the sodium salt comprises sodium carbonate. In some embodiments, the molar ratio of the oxide precursor to the sodium salt in S1 is 0.3:1 to 0.5:1.
[0064] According to some embodiments of the present application, the preparation of the oxide precursor described in S1 may include the following steps: S11: mixing cobalt salt, manganese salt, nickel salt and optional M element salt with a solvent to obtain a first mixed solution; S12: adding a precipitant to the first mixed solution, and performing a precipitation reaction at a pH of 9 to 12 to obtain a precipitate; S13: calcining the precipitate.
[0065] According to some embodiments of the present application, the preparation of the oxide precursor described in S1 includes the following steps: S11': mixing a cobalt salt, a manganese salt and a nickel salt with a solvent to obtain a first mixed solution; S12': adding a precipitant to the first mixed solution, and performing a precipitation reaction at a pH of 9 to 12 to obtain a precipitate; S13': mixing the precipitate with an optional M salt and then calcining it.
[0066] According to some embodiments of the present application, the cobalt salt includes at least one of cobalt sulfate, cobalt nitrate, cobalt chloride, or cobalt acetate. According to some embodiments of the present application, the manganese salt includes at least one of manganese sulfate, manganese nitrate, manganese chloride, or manganese acetate. According to some embodiments of the present application, the nickel salt includes at least one of nickel sulfate, nickel nitrate, nickel chloride, or nickel acetate.
[0067] According to some embodiments of the present application, the M element salt includes at least one of a chloride, acetate, sulfate, or nitrate containing the element M. In some embodiments, the M element includes at least one of K, Al, Mg, Ti, Zr, Fe, Zn, Nb, Cr, Ca, La, Y, Mo, W, Ta, Sn, V, Ce, Sr, Ge, Ga, Pb, Ba, Pr, Hf, Lu, or Cu.
[0068] According to some embodiments of the present application, in S13 and S13', the calcination temperature is 500°C to 750°C, and the calcination time is 8 hours to 24 hours.
[0069] According to some embodiments of the present application, the solvent includes at least one of water, methanol, ethanol, acetone, isopropanol or n-hexanol.
[0070] According to some embodiments of the present application, the precipitant includes at least one of aqueous ammonia, sodium hydroxide, potassium hydroxide, sodium bicarbonate, potassium bicarbonate, sodium carbonate or potassium carbonate.
[0071] According to some embodiments of the present application, the lithium-containing compound includes at least one of lithium sulfate, lithium carbonate, lithium nitrate, lithium halide, lithium carboxylate, lithium squarate, lithium alkoxide, or lithium hydroxide. In some embodiments, the lithium-containing compound includes at least one of lithium sulfate, lithium carbonate, lithium nitrate, lithium chloride, lithium bromide, lithium formate, lithium acetate, or lithium hydroxide.
[0072] 2. Electrochemical Device
[0073] The electrochemical device provided in the present application includes the positive electrode sheet described in the first aspect.
[0074] The electrochemical device provided herein further comprises a negative electrode sheet, which comprises a negative electrode current collector and a negative electrode active material layer located on the surface of the negative electrode current collector. In some embodiments, the negative electrode active material layer comprises a negative electrode active material and a binder, and optionally a conductive agent.
[0075] In some embodiments, the negative electrode active material may include a material that reversibly intercalates and deintercalates lithium ions, lithium metal, a lithium metal alloy, or a transition metal oxide. In some embodiments, the negative electrode active material includes at least one of a carbon material or a silicon-based material, the carbon material includes at least one of graphite, hard carbon, or soft carbon, and the silicon-based material includes at least one of silicon, a silicon-oxygen composite material, a silicon-carbon composite material, or a silicon alloy. In some embodiments, the binder includes at least one of styrene-butadiene rubber, polyacrylic acid, a polyacrylate, an acrylate polymer, a polyamide, or a styrene-acrylate copolymer. In some embodiments, the conductive agent includes at least one of conductive carbon black, acetylene black, Ketjen black, carbon nanotubes, or graphene.
[0076] In some embodiments, the negative electrode current collector comprises: copper foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam, a polymer substrate coated with a conductive metal, or any combination thereof.
[0077] The electrochemical device of the present application also includes a separator provided between the positive electrode sheet and the negative electrode sheet. The material and shape of the separator used in the electrochemical device of the present application are not particularly limited, and it can be any technology disclosed in the prior art. In some embodiments, the separator may include a substrate layer and a surface treatment layer. The substrate layer is a non-woven fabric, a film or a composite film having a porous structure, and the material of the substrate layer is selected from at least one of polyethylene, polypropylene, polyethylene terephthalate and polyimide. Specifically, a polypropylene porous film, a polyethylene porous film, a polypropylene non-woven fabric, a polyethylene non-woven fabric or a polypropylene-polyethylene-polypropylene porous composite film can be selected.
[0078] A surface treatment layer is provided on at least one surface of the substrate layer, and the surface treatment layer can be a bonding layer or a heat-resistant layer. The heat-resistant layer includes inorganic particles and a binder, and the inorganic particles are selected from at least one of aluminum oxide, silicon oxide, magnesium oxide, titanium oxide, hafnium dioxide, tin oxide, cerium dioxide, nickel oxide, zinc oxide, calcium oxide, zirconium oxide, yttrium oxide, silicon carbide, boehmite, aluminum hydroxide, magnesium hydroxide, calcium hydroxide and barium sulfate. The binder includes at least one of polyvinylidene fluoride, vinylidene fluoride-hexafluoropropylene copolymer, polyamide, polyacrylonitrile, acrylate polymer, polyacrylic acid, polyacrylic acid salt, polyvinylpyrrolidone, polytetrafluoroethylene or polyhexafluoropropylene. The bonding layer contains a polymer, and the material of the polymer is selected from at least one of polyamide, polyacrylonitrile, acrylate polymer, polyacrylic acid, polyacrylic acid salt, polyvinylpyrrolidone, polyvinylidene fluoride and vinylidene fluoride-hexafluoropropylene copolymer.
[0079] The electrochemical device of the present application further comprises an electrolyte. The electrolyte used in the present application may be an electrolyte known in the prior art.
[0080] In some embodiments, the electrolyte includes an organic solvent, a lithium salt, and optional additives. In some embodiments, the organic solvent includes, but is not limited to, ethylene carbonate (EC), propylene carbonate (PC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), ethyl propionate, or propyl propionate. In some embodiments, the lithium salt includes at least one of an organic lithium salt or an inorganic lithium salt. In some embodiments, the lithium salt includes, but is not limited to, lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium difluorophosphate (LiPO2F2), lithium bis(trifluoromethanesulfonyl)imide LiN(CF3SO2)2 (LiTFSI), lithium bis(fluorosulfonyl)imide Li(N(SO2F)2)(LiFSI), lithium bis(oxalatoborate) LiB(C2O4)2 (LiBOB), or lithium difluorooxalatoborate LiBF2(C2O4) (LiDFOB). In some embodiments, the additive includes at least one of fluoroethylene carbonate, vinyl ethylene carbonate, or adiponitrile.
[0081] In some embodiments, the electrochemical device of the present application includes, but is not limited to, a primary battery or a secondary battery. In some embodiments, the electrochemical device includes a lithium-ion battery.
[0082] 3. Electrical devices
[0083] The present application further provides an electrical device, which includes the electrochemical device described above.
[0084] The electrical devices of the present application are not particularly limited. In some embodiments, the electrical devices of the present application include, but are not limited to, mobile phones, laptops, tablet computers, drones, electric cars, electric bicycles, power tools, Bluetooth headsets, etc.
[0085] In the following examples and comparative examples, all reagents, materials and instruments used are commercially available unless otherwise specified.
[0086] Examples and Comparative Examples
[0087] Example 1
[0088] 1. Preparation of positive electrode materials
[0089] Step 1: Weigh nickel nitrate (Ni(NO3)2), cobalt nitrate (Co(NO3)2), and manganese nitrate (Mn(NO3)2) in a molar ratio of 2:90:8. Add deionized water and rapidly stir to dissolve. Ammonia is then added to adjust the pH to 9 to 12 until the reaction is complete, forming a homogeneous hydroxide precipitate. The precipitate is sintered at 550°C for 12 hours and crushed and sieved to obtain a metal oxide precursor material.
[0090] Step 2: Sodium carbonate (Na2CO3) and ammonium chloride (NH4Cl) are uniformly mixed with the metal oxide precursor material to obtain a mixture, wherein the molar ratio of sodium carbonate to metal oxide precursor material is 0.45:1, and the ammonium chloride accounts for 1% of the mixture by weight. The mixture is incubated at 850°C for 48 hours and post-treated to obtain the corresponding sodium cobalt oxide material.
[0091] Step 3: The sodium cobalt oxide material, lithium nitrate and lithium hydroxide are mixed uniformly in a molar ratio of 1:2:3, placed in a corundum crucible, stirred and reacted at 250° C. for 6 hours, and cooled to obtain a mixture containing the first lithium cobalt oxide positive electrode material.
[0092] Step 4: The mixture is crushed and then washed with deionized water multiple times to remove soluble sodium and lithium salts until the conductivity of the supernatant is less than 200 uS / cm. The residual powder is then centrifuged, dried, and classified to obtain the first lithium cobalt oxide.
[0093] 2. Preparation of positive electrode sheet
[0094] The positive electrode active material (the first lithium cobalt oxide mentioned above), conductive carbon (SP), and binder polyvinylidene fluoride (PVDF) were mixed in a mass ratio of 90:5:5. N-methyl-2-pyrrolidone (NMP) was added as a solvent to form a slurry, which was then coated onto 12μm-thick aluminum foil. After drying, the slurry was cold-pressed, punched, and weighed to produce a positive electrode sheet.
[0095] 3. Preparation of button batteries
[0096] Under an inert atmosphere, the above-mentioned positive electrode sheet, isolation membrane, and metal lithium sheet are placed in a button battery steel shell in order. The isolation membrane is a porous polyethylene film with a thickness of 7 μm. An appropriate amount of electrolyte (ethylene carbonate (EC): ethyl methyl carbonate (EMC): diethyl carbonate (DEC) mass ratio is 1:1:1, and the mass concentration of LiPF6 in the electrolyte is 12.5%) is dripped into the shell, and the button battery is obtained after sealing.
[0097] Examples 2 to 3, Comparative Examples 1 and 2
[0098] The difference between Example 2 and Example 3 and Example 1 is that in step 1 of preparing the positive electrode material, the molar ratios of nickel nitrate, cobalt nitrate and manganese nitrate are adjusted to 5:92:3 and 3:95:2 respectively.
[0099] The difference between Comparative Example 1 and Example 1 is that ammonium chloride is not added in step 2 of preparing the positive electrode material.
[0100] The difference between Comparative Example 2 and Example 1 is that in step 1 of preparing the positive electrode material, the molar ratios of nickel nitrate, cobalt nitrate and manganese nitrate are adjusted to 10:85:5 respectively.
[0101] Examples 4 to 6, Comparative Example 3
[0102] The difference between Examples 4 to 6 and Comparative Example 3 and Example 2 is that the insulation temperature of the mixture in step 2 is adjusted to 830° C., 800° C., 750° C., and 950° C., respectively.
[0103] Example 7 to Example 10
[0104] The difference between Examples 7 to 10 and Example 3 is that the lithium hydroxide (LiOH) in step 3 is replaced by LiCl, LiBr, HCOOLi, and CH3COOLi, respectively.
[0105] Example 11 to Example 16
[0106] The difference between Examples 11 to 16 and Example 1 is that other metal sources are used to replace the manganese source in step 1. Specific adjustment measures are detailed in Table a.
[0107] Table a
[0108] Comparative Example 4
[0109] 1. Preparation of positive electrode active materials
[0110] Steps: Weigh 0.5 mol of cobalt sulfate (CoSO4) and add deionized water for rapid stirring to dissolve. Then, add ammonium carbonate to adjust the pH to 8 until the reaction is complete, forming a homogeneous cobalt carbonate precipitate. The precipitate is sintered at 650°C for 12 hours, crushed, and sieved to obtain the Co3O4 metal oxide material.
[0111] Step 2: Lithium carbonate (Li2CO3), aluminum oxide (Al2O3), and the aforementioned Co3O4 were weighed and mixed uniformly at a molar ratio of Li:Co:Al of 1.05:0.97:0.03. The mixture was then heated at 900°C for 12 hours. The resulting second lithium cobalt oxide material was then crushed and screened to obtain the corresponding material. XRD analysis revealed an R-3m crystal structure, and particle size distribution analysis revealed a Dv50 of 17.8 μm.
[0112] 2. Preparation of positive electrode sheet
[0113] The above-mentioned positive electrode active material, conductive carbon (SP) and binder polyvinylidene fluoride (PVDF) are mixed in a mass ratio of 96:2.5:1.5, and the solvent N-methyl-2-pyrrolidone (NMP) is added to make a slurry. The slurry is coated on an aluminum foil with a thickness of 12 μm. After drying, the slurry is cold pressed, punched, and weighed under a pressure of about 15 tons to obtain a positive electrode sheet.
[0114] 3. Button battery preparation
[0115] Same as Example 1.
[0116] Example 17
[0117] The difference between Example 17 and Comparative Example 4 is that the positive electrode active material is obtained by uniformly mixing the first lithium cobalt oxide of Example 3 and the second lithium cobalt oxide of Comparative Example 4 in a mass ratio of 10:90.
[0118] Examples 18 to 24, Comparative Examples 5 to 6
[0119] The difference between Examples 18 to 24 and Comparative Examples 5 to 6 and Example 17 is that the ratio of the first lithium cobalt oxide and the second lithium cobalt oxide and the types of the first lithium cobalt oxide and the second lithium cobalt oxide are adjusted, wherein the c / d value of the second lithium cobalt oxide particles is regulated by crushing and screening conditions. Specific adjustment measures are detailed in Table B.
[0120] Table b
[0121] Test Method
[0122] 1. Test of aspect ratio and average particle size of lithium cobalt oxide particles
[0123] A positive electrode sheet was processed using a microtome to obtain a cross-section perpendicular to the surface of the positive electrode current collector. The cross-section was then photographed using a scanning electron microscope (SEM) to obtain a cross-sectional image. From the cross-sectional image, 50 first lithium cobalt oxide particles were randomly selected. The maximum major diameter of the first lithium cobalt oxide particles and the distance between the perpendicular bisector of the maximum major diameter and two intersection points on the surface of the first lithium cobalt oxide particles were measured as the minor diameter. The ratio of the maximum major diameter to the minor diameter was then calculated, and the average of these values was taken as the aspect ratio a / b of the first lithium cobalt oxide. The average value of the maximum major diameter of the first lithium cobalt oxide particles was the average particle size of the first lithium cobalt oxide particles.
[0124] The test of the aspect ratio c / d of the second lithium cobalt oxide particles is the same as the aspect ratio a / b of the first lithium cobalt oxide particles. The average value of the maximum major diameter of the second lithium cobalt oxide particles is the average particle size of the second lithium cobalt oxide particles.
[0125] 2. Test of the cross-sectional area ratio of the first lithium cobalt oxide and the second lithium cobalt oxide in the positive electrode sheet
[0126] In the above cross-sectional image, a 100 μm×80 μm region of the positive electrode active material layer was randomly selected, and the cross-sectional areas of the first lithium cobalt oxide particle and the second lithium cobalt oxide particle in the region were counted, and the corresponding cross-sectional area ratio S1 / S2 was calculated.
[0127] 3. Compaction density test of positive electrode active material layer
[0128] Take a positive electrode sheet coated on one side with a positive electrode active material layer and punch out a positive electrode sheet sample with an area of S. The weight of the sample is measured using an analytical balance and recorded as m1, and the thickness of the sample is measured using a micrometer and recorded as H. The positive electrode sheet sample is soaked in NMP to remove the positive electrode active material layer on the surface to obtain a positive electrode current collector. After drying, the weight of the positive electrode current collector is weighed using an analytical balance and recorded as m2, and its thickness is measured using a micrometer and recorded as h.
[0129] Compacted density of the positive electrode active material layer = (m1-m2) / ((Hh) x S).
[0130] 4. Electrochemical performance test
[0131] The button battery is 3V-4.6V (vs.Li / Li + ) voltage range, the charge and discharge test was carried out with a current density of 0.3 mA / cm 2 .
[0132] Specifically, at 25°C, the current size of the test is set to 0.3 mA / cm 2 , firstly charge at constant current to 4.6V, then charge at constant voltage to 50μA; then charge at 0.3mA / cm 2The battery is discharged at a constant current of 0.1 V to 3.0 V. This is one charge-discharge cycle. Repeat the above charge-discharge cycle 100 times.
[0133] First charge gram capacity = first charge capacity / positive electrode material mass;
[0134] First discharge capacity in grams = first discharge capacity / mass of positive electrode material;
[0135] Capacity retention rate after 100 cycles (%) = [discharge capacity at the 100th cycle / discharge capacity at the first cycle] × 100%.
[0136] Test results
[0137] Table 1 shows the effect of the a / b value of the first lithium cobalt oxide particles on the performance of the coin cell.
[0138] Table 1
[0139] The positive electrode material was subjected to XRD testing. Figure 1 shows the XRD pattern of the positive electrode material powder provided in Example 1, demonstrating that the resulting material has a P63mc crystal structure. Figure 2 shows a SEM image of the positive electrode material powder provided in Example 1, demonstrating that the positive electrode material provided in Example 1 has a lamellar morphology. Furthermore, Figure 3 shows a cross-sectional SEM image of the positive electrode material provided in Example 1 within a pole piece, further illustrating the lamellar morphology of the material.
[0140] The positive electrode materials provided in Comparative Examples 1 to 3 and Examples 1 to 16 were subjected to a drop test, and the electrical performance test results are shown in Table 1. The data in Table 1 show that the positive electrode materials with different a / b ratios have small differences in initial charge capacity, but large differences in initial discharge capacity and cycling stability. When the a / b ratio is within the range of 3 to 9, the positive electrode material has both high discharge capacity and cycling stability.
[0141] By comparing Comparative Example 1 and Example 1, it can be seen that although the material components of the two are the same, whether or not ammonium chloride flux is added in preparation step 2 will result in different a / b values of the materials.
[0142] Table 2 further studies the effect of the ratio of the first cobalt lithium oxide to the second cobalt lithium oxide in the positive electrode sheet on the performance of the button battery.
[0143] Table 2
[0144] The data in Table 2 show that the aspect ratio a / b of the first lithium cobalt oxide in the positive electrode sheet is in the range of 3 to 9, and the aspect ratio c / d of the second lithium cobalt oxide B particles is in the range of 1 to 1.2. Compared with Comparative Examples 5 and 6 in which the aspect ratio a / b of the first lithium cobalt oxide is not in the range of 3 to 9, the discharge capacity and cycle stability of the button cell can be better improved. This may be because when the aspect ratio a / b of the first lithium cobalt composite oxide is less than 3, it is difficult to suppress the side reaction of the electrolyte on its active surface and it is not able to effectively cover and protect the second lithium cobalt composite oxide. When the aspect ratio a / b of the first lithium cobalt composite oxide is greater than 9, the first lithium cobalt composite oxide and the second lithium cobalt composite oxide are difficult to match during the compaction process, which easily causes the first lithium cobalt composite oxide to break, resulting in an ineffective improvement in the cycle capacity retention rate.
[0145] In addition, from the comparison of Examples 17 to 21, it can be seen that when the cross-sectional area ratio S1 / S2 of the first lithium cobalt oxide and the second lithium cobalt oxide is in the range of 0.1 to 0.35, the first lithium cobalt oxide and the second lithium cobalt oxide can be better matched, so that the button battery can have both a higher discharge capacity and excellent cycle stability.
[0146] Although illustrative embodiments have been shown and described, those skilled in the art should understand that the above embodiments should not be construed as limitations on the present application, and that changes, substitutions, and modifications may be made to the embodiments without departing from the spirit, principles, and scope of the present application.
Claims
1. A positive electrode sheet, comprising a positive electrode current collector and a positive electrode active material layer located on the surface of the positive electrode current collector, wherein the positive electrode active material layer comprises a positive electrode material, wherein the positive electrode material comprises a P6 3 The first lithium cobalt oxide particle has an mc crystal structure, and in a cross section of the positive electrode active material layer perpendicular to the surface of the positive electrode current collector, the aspect ratio a / b of the cross section of the first lithium cobalt oxide particle satisfies: 3≤a / b≤9, in, a is the longest diameter of the cross section of the first lithium cobalt oxide particle, and b is the length of the short diameter of the cross section of the first lithium cobalt oxide particle that is perpendicular to and bisects the longest diameter.
2. The positive electrode sheet according to claim 1, in, The positive electrode sheet satisfies at least one of the following conditions (1) to (2): (1)4≤a / b≤8; (2) The average particle size of the first lithium cobalt oxide particles is 5 μm to 20 μm.
3. The positive electrode sheet according to claim 1, in, The positive electrode sheet satisfies at least one of the following conditions (1) to (2): (1) The morphology of the first lithium cobalt oxide particles is lamellar; (2) Cracks exist in the cross section of the first lithium cobalt oxide particle.
4. The positive electrode sheet according to claim 1, in, The positive electrode sheet satisfies at least one of the following conditions (1) to (3): (1) the first lithium cobalt oxide includes Mn and Ni elements, and based on the molar amount of the metal elements other than Li in the first lithium cobalt oxide, the molar percentage of Mn in the first lithium cobalt oxide is 0.05% to 10%, and the molar percentage of Ni in the first lithium cobalt oxide is 0.05% to 10%; (2) the first lithium cobalt oxide includes an M element, wherein the M element includes at least one of Na, Al, Mg, Ti, Zr, Fe, Zn, Nb, Cr, Ca, La, Y, Mo, W, Ta, Sn, V, Ce, Sr, Ge, Ga, Pb, Ba or Cu, and the molar percentage of the M element in the first lithium cobalt oxide is 0.01% to 10% based on the molar amount of the metal element other than the Li element in the first lithium cobalt oxide; (3) The first lithium cobalt oxide includes Li x1 Co y1 Ni z1 Mn q M s O 2±n T n , wherein 0.6≤x1≤1.1, 0.8≤y1<1, 0<z1≤0.1, 0<q≤0.1, 0≤s≤0.1, 0≤n≤0.05, M includes at least one of Na, K, Al, Mg, Ti, Zr, Fe, Zn, Nb, Cr, Ca, La, Y, Mo, W, Ta, Sn, V, Ce, Sr, Ge, Ga, Pb, Ba, Pr, Hf, Lu or Cu, and T is a halogen.
5. The positive electrode sheet according to claim 1, in, The positive electrode material also includes a second lithium cobalt oxide particle having an R-3m crystal structure. In a cross section of the positive electrode active material layer perpendicular to the surface of the positive electrode current collector, the aspect ratio c / d of the cross section of the second lithium cobalt oxide particle is 1 to 1.2, wherein c is the longest diameter of the cross section of the second lithium cobalt oxide particle, and d is the length of the short diameter in the cross section of the second lithium cobalt oxide particle that is perpendicular to and bisects its longest diameter.
6. The positive electrode sheet according to claim 5, in, In a cross section of the positive electrode active material layer perpendicular to the surface of the positive electrode current collector, a ratio S1 / S2 between a cross-sectional area S1 of the first lithium cobalt oxide particle and a cross-sectional area S2 of the second lithium cobalt oxide particle satisfies: 0.05≤S1 / S2≤0.
45.
7. The positive electrode sheet according to claim 6, in, 0.1≤S1 / S2≤0.
35.
8. The positive electrode sheet according to claim 5, in, The positive electrode sheet satisfies at least one of the following conditions (1) to (5): (1) the average particle size of the second lithium cobalt oxide particles is 10 μm to 25 μm; (2) Based on the molar amount of the metal element other than the Li element in the second lithium cobalt oxide, the molar percentage of the Co element in the second lithium cobalt oxide is 90% to 100%; (3) the second lithium cobalt oxide includes an R element, wherein the R element includes at least one of Ni, Mn, Na, K, Al, Mg, Ti, Zr, Fe, Zn, Nb, Cr, Ca, La, Y, Mo, W, Ta, Sn, V, Ce, Sr, Ge, Ga, Pb, Ba or Cu, and the molar percentage of the R element in the second lithium cobalt oxide is 0.01% to 10% based on the molar amount of the metal element other than the Li element in the second lithium cobalt oxide; (4) The second lithium cobalt oxide includes Li x2 Co y2 R z2 O 2±m T' m At least one of, wherein 0.6≤x2≤1.1, 0.9≤y2≤1, 0≤z2≤0.1, 0≤m≤0.05, R comprises at least one of Ni, Mn, Na, K, Al, Mg, Ti, Zr, Fe, Zn, Nb, Cr, Ca, La, Y, Mo, W, Ta, Sn, V, Ce, Sr, Ge, Ga, Pb, Ba, Pr, Hf, Lu or Cu, and T' is a halogen; (5) The mass ratio of the first lithium cobalt oxide particles to the second lithium cobalt oxide particles is 5:95 to 40:
60.
9. An electrochemical device comprising the positive electrode sheet according to any one of claims 1 to 8.
10. An electrical device comprising the electrochemical device according to claim 9.
Citation Information
Patent Citations
Positive electrode and electrochemical device
CN113875042A
Positive electrode active material, electrochemical device, and electronic device
CN114497525A
Lithium composite metal oxide, cathode active material for lithium secondary battery, cathode for lithium secondary battery and lithium secondary battery
JP2019167291A
Cited By
Positive electrode material, electrochemical device, and electronic device
WO2026207672A1