Low-cost hard carbon negative electrode material based on waste cotton spinning products, preparation method thereof, pole piece and sodium ion battery

By steaming, pre-carbonizing and pyrolyzing the waste cotton textiles, low-cost hard carbon materials are prepared, which solves the problem of high cost of hard carbon materials, achieves high energy density and cycle stability of sodium ion batteries, and reduces the Waste pollution.

CN118929623APending Publication Date: 2024-11-12SHENZHEN PANGU NAXIANG NEW ENERGY CO LTD +1

Patent Information

Application Number
CN202410983509.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the prior art, hard carbon materials are costly, and there is no method of obtaining low-cost hard carbon materials by using waste waste cotton textiles, resulting in waste of resources and environmental pollution.

Method used

By steaming, drying and crushing the waste cotton textile, pre-carbonizing and pyrolyzing the carbonization process, a low-cost hard carbon negative electrode material based on waste cotton textiles is prepared for the electrode sheet of sodium ion battery. The method includes pre-carbonization under an air atmosphere, pyrolytic carbonization under an inert atmosphere, and preparation of electrode sheets in combination with Super P carbon black, CMC and SBR.

Benefits of technology

The preparation of low-cost hard carbon materials is realized, the energy density and cycle stability of sodium ion batteries are improved, waste landfill and incineration are reduced, greenhouse gas emissions are reduced, and large-scale production is suitable.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118929623A_ABST
    Figure CN118929623A_ABST
Patent Text Reader

Abstract

The invention discloses a low-cost hard carbon negative electrode material based on a waste cotton spinning product and a preparation method thereof, a pole piece and a sodium ion battery, and the preparation method of the low-cost hard carbon negative electrode material based on the waste cotton spinning product comprises the following steps: cooking, drying and crushing the waste cotton spinning product to obtain a hard carbon precursor; pre-carbonizing the hard carbon precursor in an air atmosphere, and then cooling and grinding to obtain a pre-carbonized product; and pyrolyzing and carbonizing the pre-carbonized product in an inert atmosphere, cooling, grinding and sieving to obtain the low-cost hard carbon negative electrode material based on the waste cotton spinning product. According to the preparation method of the low-cost hard carbon negative electrode material based on the waste cotton spinning products, the waste cotton spinning products can be effectively recycled, and the hard carbon applied to the sodium battery is prepared.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of secondary batteries, and in particular to a low-cost hard carbon negative electrode material based on waste cotton textiles, a preparation method thereof, a pole piece and a sodium ion battery. Background Art

[0002] my country is rich in sodium resources, and sodium-ion batteries are considered to be the most suitable new type of battery for large-scale energy storage, and are expected to alleviate the problems of limited energy storage development caused by lithium resource shortages and uneven distribution. With the rapid industrialization of sodium-ion batteries, the demand for sodium-ion battery negative electrodes is increasing. From the classification of sodium-ion battery negative electrode materials, they can be roughly divided into five categories: one is carbon-based negative electrode materials, mainly including graphite, amorphous carbon, nanocarbon, etc.; the second is alloy negative electrode materials; the third is metal oxide and sulfide-based negative electrode materials; the fourth is embedded titanium-based negative electrode materials; and the fifth is organic negative electrode materials. Among them, amorphous hard carbon is the most mature and has the best compatibility with the current sodium-ion battery system.

[0003] At the same time, the domestic stock of waste textiles is nearly 400 million tons, with an annual increase of more than 20 million tons. Among them, chemical fibers made from cotton account for about 20%, while the recycling rate is less than 10%.

[0004] However, the cost of hard carbon materials is currently high, and there is no low-cost method for preparing hard carbon materials by utilizing waste and discarded cotton textiles. Summary of the invention

[0005] In view of the above-mentioned deficiencies in the prior art, the present invention proposes a low-cost hard carbon negative electrode material based on waste cotton textiles and its preparation method, electrode sheet and sodium ion battery, aiming to solve the problem that the current cost of hard carbon materials is relatively high and there is no low-cost method for preparing hard carbon materials by utilizing waste and discarded cotton textiles.

[0006] To achieve the above-mentioned purpose, the present invention proposes a low-cost hard carbon negative electrode material based on waste cotton textiles, comprising the following steps: steaming, drying and crushing the waste cotton textiles to obtain a hard carbon precursor; pre-carbonizing the hard carbon precursor in an air atmosphere, cooling and grinding after completion to obtain a pre-carbonized product; pyrolyzing and carbonizing the pre-carbonized product in an inert atmosphere, cooling, grinding and sieving to obtain a low-cost hard carbon negative electrode material based on waste cotton textiles.

[0007] Optionally, the steaming time is 1 h to 2 h.

[0008] Optionally, the pre-carbonization temperature is 200° C. to 400° C., the heating rate is 5° C. / min to 10° C. / min, and the insulation time is 2 h to 4 h.

[0009] Optionally, the pyrolysis carbonization temperature is 700°C to 1000°C, the heating rate is 5°C / min to 10°C / min, and the holding time is 9h to 11h.

[0010] Optionally, the gas of the inert atmosphere includes one of nitrogen, argon, and a hydrogen-argon mixture.

[0011] Optionally, the hydrogen-argon mixed gas includes 5% by volume of H2 and 95% by volume of Ar.

[0012] In order to achieve the above object, the present invention also proposes a low-cost hard carbon negative electrode material based on waste cotton textiles, which is prepared by the above method.

[0013] In order to achieve the above-mentioned purpose, the present invention also proposes an electrode plate, comprising the above-mentioned low-cost hard carbon negative electrode material based on waste cotton textiles.

[0014] Optionally, the slurry for preparing the electrode plate includes the low-cost hard carbon negative electrode material based on waste cotton textiles, Super P carbon black, CMC and SBR.

[0015] In order to achieve the above object, the present invention also provides a sodium ion battery, comprising the above electrode plate.

[0016] Beneficial effects of the present invention: The method for preparing low-cost hard carbon negative electrode materials based on waste cotton textiles provided by the present invention will pre-treat cotton textiles, remove impurities and improve their structural properties, making them more suitable for the subsequent carbonization process. During the carbonization process, cotton textiles are heated in an oxygen-free environment to convert organic matter into a stable carbon structure. Since cotton textiles themselves contain a high mass ratio of cellulose, this property gives them a natural advantage when converted into hard carbon. Due to the wide availability of cotton textiles, this method is also conducive to large-scale production to meet the growing demand for energy storage and conversion materials. At the same time, the present invention also converts waste into valuable materials, reduces the landfill and incineration of waste, and reduces greenhouse gas emissions. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.

[0018] Figure 1 1 is a charge and discharge curve of an embodiment of the present invention. DETAILED DESCRIPTION

[0019] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. It should be understood that the following embodiments are only used to explain the present invention and are not used to limit the present invention.

[0020] Unless defined otherwise, all technical and scientific terms used herein have the common meaning in the art to which the claimed subject matter pertains.

[0021] It should be noted that if the embodiments of the present invention involve directional indications (such as up, down, left, right, front, back, etc.), the directional indications are only used to explain the relative position relationship, movement status, etc. between the components under a certain specific posture (as shown in the accompanying drawings). If the specific posture changes, the directional indication will also change accordingly.

[0022] In addition, if there are descriptions involving "first", "second", etc. in the embodiments of the present invention, the descriptions of "first", "second", etc. are only used for descriptive purposes and cannot be understood as indicating or implying their relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In addition, if the meaning of "and / or" appearing in the full text is to include three parallel schemes, taking "A and / or B" as an example, it includes scheme A, or scheme B, or a scheme that satisfies both A and B. In addition, the technical solutions between the various embodiments can be combined with each other, but it must be based on the ability of ordinary technicians in this field to implement. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such a combination of technical solutions does not exist and is not within the scope of protection required by the present invention.

[0023] From the perspective of the classification of negative electrode materials for sodium-ion batteries, they can be roughly divided into five categories: one is carbon-based negative electrode materials, mainly including graphite, amorphous carbon, nanocarbon, etc.; two is alloy negative electrode materials; three is metal oxide and sulfide-based negative electrode materials; four is embedded titanium-based negative electrode materials; five is organic negative electrode materials. Among them, amorphous hard carbon is the most mature and has the best compatibility with the current sodium-ion battery system.

[0024] At the same time, the domestic stock of waste textiles is nearly 400 million tons, with an annual increase of more than 20 million tons. Among them, chemical fibers made from cotton account for about 20%, while the recycling rate is less than 10%.

[0025] Currently, hard carbon materials are generally derived from biomass, starch or resin, etc., which are relatively expensive. There is no low-cost method for preparing hard carbon materials by utilizing waste and discarded cotton textiles.

[0026] To solve the above problems, the present invention proposes a method for preparing a low-cost hard carbon negative electrode material based on waste cotton textiles, comprising the following steps:

[0027] S1: steaming, drying and crushing waste cotton products to obtain a hard carbon precursor;

[0028] In this embodiment, the steaming step is mainly to remove non-cellulose components in the fiber, such as wax, pectin, oil, etc., as well as some low molecular weight cellulose components, so as to obtain a relatively pure cellulose raw material. In some embodiments, the waste cotton textiles are waste waste cotton textiles that can no longer be used as the original fabric function of the waste cotton textiles. In some embodiments, bleaching agents are also added during steaming.

[0029] S2: Pre-carbonizing the hard carbon precursor in an air atmosphere, cooling and grinding it to obtain a pre-carbonized product; in this scheme, the temperature during the pre-carbonization process will affect the pore structure and specific surface area of ​​the carbon material, thereby affecting its adsorption and electrochemical properties, and can also improve the crystallinity of the material, which helps to form a more ordered carbon structure.

[0030] S3: Pyrolyzing and carbonizing the pre-carbonized product under an inert atmosphere, cooling, grinding and sieving to obtain a low-cost hard carbon negative electrode material based on waste cotton textiles.

[0031] During the heating process of pyrolysis carbonization, high molecular polymers (such as cellulose) in cotton textiles will undergo pyrolysis reactions and decompose into smaller molecules. At high temperatures, water molecules in cotton textiles will be removed, leaving carbon as the main product. During the carbonization process, hydrogen atoms in organic matter will also be removed, further increasing the carbon content. The small molecules produced by decomposition may recombine to form a larger carbon molecular structure. Under high temperature conditions, condensation reactions may occur between cellulose molecules to form a more stable carbon structure, and finally a carbonaceous conductive network is formed to obtain a low-cost hard carbon negative electrode material based on waste cotton textiles.

[0032] Furthermore, the cooking time is 1 hour to 2 hours. Appropriate cooking time helps to more effectively remove impurities in cotton textiles, but if the cooking time is too long, it may cause excessive degradation of cellulose and produce more short-chain fragments, which increases the difficulty of separation. The cooking time needs to be precisely controlled according to specific recycling goals and product quality requirements. In some embodiments of this scheme, the cooking time is preferably 1 hour.

[0033] Furthermore, the pre-carbonization temperature is 200°C to 400°C, the heating rate is 5°C / min to 10°C / min, and the holding time is 2h to 4h. The temperature and heating rate during the pre-carbonization process have an important influence on the structure and performance of the material, and need to be optimized and controlled according to specific application requirements. The heating temperature, heating rate, and holding time affect the evolution of the internal structure of the pre-carbonized product, the removal efficiency of volatile components, and the formation of pores, which in turn affect the purity and performance of the material, thereby affecting the characteristics of the electrode after application to the battery electrode.

[0034] In some embodiments of the present scheme, the pre-carbonization temperature is any value between 200°C and 400°C, such as 200°C, 250°C, 300°C, 350°C, 400°C, etc.

[0035] Furthermore, the temperature of the pyrolysis carbonization is 700°C to 1000°C, the heating rate is 5°C / min to 10°C / min, and the holding time is 9h to 11h. The increase in temperature will accelerate the rate of the pyrolysis reaction, affecting the decomposition and reforming of cellulose, hemicellulose and lignin, and the pyrolysis temperature, heating rate and holding time work together to regulate the graphitization degree of the cotton fiber carbonization product, the oxygen-containing functional groups on the surface of the product, and the product morphology and structure.

[0036] In some embodiments of the present scheme, the temperature of pyrolysis carbonization is 700°C, 750°C, 800°C, 850°C, 900°C, 950°C, 1000°C, or any value between 700°C and 1000°C.

[0037] Furthermore, the gas of the inert atmosphere includes one of nitrogen, argon, and a hydrogen-argon mixture. In this solution, pyrolysis is performed in an inert gas atmosphere to inhibit oxidation reactions and promote carbon retention, thereby improving the yield and quality of carbon.

[0038] Furthermore, the hydrogen-argon mixed gas includes 5% by volume of H2 and 95% by volume of Ar. Adding a small amount of reducing hydrogen into the argon gas can promote the reduction reaction during the pyrolysis process and improve its electrochemical performance.

[0039] To solve the above problems, the present invention also proposes a low-cost hard carbon negative electrode material based on waste cotton textiles prepared by the above preparation method. Due to the wide availability of cotton textiles, this method is also conducive to large-scale production to meet the growing demand for energy storage and conversion materials. At the same time, when the waste cotton textiles used are old and waste cotton textiles, the present invention also converts waste into valuable materials, reduces landfill and incineration of waste, and reduces greenhouse gas emissions.

[0040] To solve the above problems, the present invention also proposes an electrode plate, including the above-mentioned low-cost hard carbon negative electrode material based on waste cotton textiles. Hard carbon has a unique pore structure and a large interlayer spacing, which enables it to store more charge in a smaller volume, thereby improving the energy density of the battery. The expansion and contraction of hard carbon during the charging and discharging process is relatively uniform, which helps to improve the cycle stability of the battery and extend its service life. The pore structure of hard carbon is conducive to the rapid insertion and extraction of sodium ions, thereby providing better charging and discharging performance.

[0041] Furthermore, the slurry for preparing the electrode plate includes the low-cost hard carbon negative electrode material based on waste cotton textiles, Super P carbon black, CMC and SBR. In this solution, CMC (carboxymethyl cellulose) and SBR (styrene-butadiene rubber) are a bonding system. CMC can ensure stable processing due to its extremely high slurry stability; at the same time, it can also improve the bonding force between hard carbon and negative electrode, thereby extending the service life of the battery.

[0042] In some embodiments, the method for preparing an electrode sheet includes: mixing a low-cost hard carbon negative electrode material based on waste cotton textiles, Super P carbon black, CMC and SBR in a mass ratio, grinding them evenly, adding deionized water and stirring to obtain an electrode slurry; evenly coating the battery slurry on an aluminum foil, and preparing it into a disc electrode after vacuum drying to obtain a hard carbon electrode sheet made of waste cotton textiles as raw materials.

[0043] In some embodiments, the mass ratio of the hard carbon negative electrode material, Super P carbon black, CMC and SBR is (88-91):(3-5):(2-5):(2-5).

[0044] In some embodiments, the mass ratio of the hard carbon negative electrode material, Super P carbon black, CMC and SBR is 90:5:2:3.

[0045] To solve the above problems, the present invention also provides a sodium ion battery, comprising the above electrode plate. After using the electrode prepared with low-cost hard carbon, the present solution can achieve excellent reversible capacity and first efficiency.

[0046] Embodiment 1:

[0047] The waste cotton products were steamed, dried and crushed for 1 hour to obtain a hard carbon precursor;

[0048] The hard carbon precursor was pre-carbonized at 350°C in an air atmosphere, with a heating rate of 5°C / min and a holding time of 3h. After completion, it was cooled and ground to obtain a pre-carbonized product.

[0049] The pre-carbonized product was pyrolyzed and carbonized at 800° C. in an atmosphere of 5% by volume H2 and 95% by volume Ar, with a heating rate of 5° C. / min and a holding time of 10 h, and then cooled, ground and sieved to obtain a low-cost hard carbon negative electrode material based on waste cotton textiles;

[0050] A low-cost hard carbon negative electrode material based on waste cotton textiles, Super P carbon black, CMC and SBR in a mass ratio of 90:5:2:3 are mixed, ground evenly, deionized water is added and stirred to obtain an electrode slurry; the battery slurry is evenly coated on an aluminum foil, and after vacuum drying, it is prepared into a disc electrode to obtain an electrode plate made of waste cotton textiles as raw materials, and the electrode plates are assembled into 2025 button batteries, in which the diaphragm is a PP diaphragm.

[0051] Embodiment 2:

[0052] The waste cotton products were steamed, dried and crushed for 1 hour to obtain a hard carbon precursor;

[0053] The hard carbon precursor was pre-carbonized at 350°C in an air atmosphere, with a heating rate of 10°C / min and a holding time of 3h. After completion, it was cooled and ground to obtain a pre-carbonized product.

[0054] The pre-carbonized product was pyrolyzed and carbonized at 850° C. in an atmosphere of 5% by volume H2 and 95% by volume Ar, with a heating rate of 10° C. / min and a holding time of 10 h, and then cooled, ground and sieved to obtain a low-cost hard carbon negative electrode material based on waste cotton textiles;

[0055] A low-cost hard carbon negative electrode material based on waste cotton textiles, Super P carbon black, CMC and SBR in a mass ratio of 90:5:2:3 are mixed, ground evenly, deionized water is added and stirred to obtain an electrode slurry; the battery slurry is evenly coated on an aluminum foil, and after vacuum drying, it is prepared into a disc electrode to obtain an electrode plate made of waste cotton textiles as raw materials, and the electrode plates are assembled into 2025 button batteries, in which the diaphragm is a PP diaphragm.

[0056] Embodiment 3:

[0057] The waste cotton products were steamed for 2 hours, dried and crushed to obtain a hard carbon precursor;

[0058] The hard carbon precursor was pre-carbonized at 300°C in an air atmosphere, with a heating rate of 5°C / min and a holding time of 3h. After completion, the pre-carbonized product was obtained by cooling and grinding.

[0059] The pre-carbonized product was pyrolyzed and carbonized at 850° C. in an atmosphere of 5% by volume H2 and 95% by volume Ar, with a heating rate of 10° C. / min and a holding time of 10 h, and then cooled, ground and sieved to obtain a low-cost hard carbon negative electrode material based on waste cotton textiles;

[0060] A low-cost hard carbon negative electrode material based on waste cotton textiles, Super P carbon black, CMC and SBR in a mass ratio of 90:5:2:3 are mixed, ground evenly, deionized water is added and stirred to obtain an electrode slurry; the battery slurry is evenly coated on an aluminum foil, and after vacuum drying, it is prepared into a disc electrode to obtain an electrode plate made of waste cotton textiles as raw materials, and the electrode plates are assembled into 2025 button batteries, in which the diaphragm is a PP diaphragm.

[0061] Embodiment 4:

[0062] The waste cotton products were steamed for 2 hours, dried and crushed to obtain a hard carbon precursor;

[0063] The hard carbon precursor was pre-carbonized at 300°C in an air atmosphere, with a heating rate of 5°C / min and a holding time of 3h. After completion, the pre-carbonized product was obtained by cooling and grinding.

[0064] The pre-carbonized product is pyrolyzed and carbonized at 750° C. in an atmosphere of 5% by volume H2 and 95% by volume Ar, with a heating rate of 5° C. / min and a holding time of 10 h, and then cooled, ground and sieved to obtain a low-cost hard carbon negative electrode material based on waste cotton textiles;

[0065] A low-cost hard carbon negative electrode material based on waste cotton textiles, Super P carbon black, CMC and SBR in a mass ratio of 92:3:2:3 are mixed, ground evenly, added with deionized water and stirred to obtain an electrode slurry; the battery slurry is evenly coated on an aluminum foil, and after vacuum drying, it is prepared into a disc electrode to obtain an electrode plate made of waste cotton textiles as raw materials, and the electrode plates are assembled into 2025 button batteries, in which the diaphragm is a PP diaphragm.

[0066] Embodiment 5:

[0067] The waste cotton products were steamed for 2 hours, dried and crushed to obtain a hard carbon precursor;

[0068] The hard carbon precursor was pre-carbonized at 300°C in an air atmosphere, with a heating rate of 5°C / min and a holding time of 3h. After completion, the pre-carbonized product was obtained by cooling and grinding.

[0069] The pre-carbonized product was pyrolyzed and carbonized at 900° C. in an atmosphere of 5% by volume H2 and 95% by volume Ar, with a heating rate of 10° C. / min and a holding time of 10 h, and then cooled, ground and sieved to obtain a low-cost hard carbon negative electrode material based on waste cotton textiles;

[0070] A low-cost hard carbon negative electrode material based on waste cotton textiles, Super P carbon black, CMC and SBR in a mass ratio of 90:5:2:3 are mixed, ground evenly, deionized water is added and stirred to obtain an electrode slurry; the battery slurry is evenly coated on an aluminum foil, and after vacuum drying, it is prepared into a disc electrode to obtain an electrode plate made of waste cotton textiles as raw materials, and the electrode plates are assembled into 2025 button batteries, in which the diaphragm is a PP diaphragm.

[0071] Embodiment 6:

[0072] The waste cotton products were steamed for 1.5 hours, dried and crushed to obtain a hard carbon precursor;

[0073] The hard carbon precursor was pre-carbonized at 300°C in an air atmosphere, with a heating rate of 5°C / min and a holding time of 3h. After completion, the pre-carbonized product was obtained by cooling and grinding.

[0074] The pre-carbonized product was pyrolyzed and carbonized at 800° C. in an atmosphere of 5% by volume H2 and 95% by volume Ar, with a heating rate of 5° C. / min and a holding time of 10 h, and then cooled, ground and sieved to obtain a low-cost hard carbon negative electrode material based on waste cotton textiles;

[0075] A low-cost hard carbon negative electrode material based on waste cotton textiles, Super P carbon black, CMC and SBR in a mass ratio of 90:5:2:3 are mixed, ground evenly, deionized water is added and stirred to obtain an electrode slurry; the battery slurry is evenly coated on an aluminum foil, and after vacuum drying, it is prepared into a disc electrode to obtain an electrode plate made of waste cotton textiles as raw materials, and the electrode plates are assembled into 2025 button batteries, in which the diaphragm is a PP diaphragm.

[0076] Furthermore, the test button cells finally prepared in Examples 1-6 were used for electrical performance testing, and the test parameters were 0.1C charge and discharge at room temperature. The results are shown in Table 1 below:

[0077] Table 1.

[0078]

[0079] This table confirms that cotton textiles will be pre-treated to remove impurities and improve their structural properties, making them more suitable for the subsequent carbonization process. During the carbonization process, cotton textiles are heated in an oxygen-free environment to convert organic matter into a stable carbon structure, and then the pole piece is applied to the electrode to prepare a sodium-ion battery, which can achieve excellent reversible capacity and first efficiency.

[0080] The above are only preferred embodiments of the present invention, and do not limit the patent scope of the present invention. For those skilled in the art, the present invention may have various changes and modifications. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the patent protection scope of the present invention.

Claims

1. A method for preparing a low-cost hard carbon negative electrode material based on waste cotton textiles, characterized in that: The following steps are involved: The waste cotton products are steamed, dried and crushed to obtain a hard carbon precursor; The hard carbon precursor is pre-carbonized in an air atmosphere, and after completion, it is cooled and ground to obtain a pre-carbonized product; The pre-carbonized product is pyrolyzed and carbonized under an inert atmosphere, cooled, ground and sieved to obtain a low-cost hard carbon negative electrode material based on waste cotton textiles.

2. The method for preparing a low-cost hard carbon negative electrode material based on waste cotton textiles according to claim 1, characterized in that: The cooking time is 1 h to 2 h.

3. The method for preparing a low-cost hard carbon negative electrode material based on waste cotton textiles according to claim 1, characterized in that: The pre-carbonization temperature is 200° C. to 400° C., the heating rate is 5° C. / min to 10° C. / min, and the heat preservation time is 2h to 4h.

4. The method for preparing a low-cost hard carbon negative electrode material based on waste cotton textiles according to claim 1, characterized in that: The temperature of the pyrolysis carbonization is 700° C. to 1000° C., the heating rate is 5° C. / min to 10° C. / min, and the heat preservation time is 9h to 11h.

5. The method for preparing a low-cost hard carbon negative electrode material based on waste cotton textiles according to claim 1, characterized in that: The gas of the inert atmosphere includes one of nitrogen, argon, and a hydrogen-argon mixed gas.

6. The method for preparing a low-cost hard carbon negative electrode material based on waste cotton textiles according to claim 5, characterized in that: The hydrogen-argon mixed gas includes 5% by volume of H2 and 95% by volume of Ar.

7. A low-cost hard carbon negative electrode material based on waste cotton textiles, characterized in that: It comprises a low-cost hard carbon negative electrode material based on waste cotton textiles prepared by the preparation method as described in any one of claims 1 to 6.

8. An electrode plate, characterized in that: Including the low-cost hard carbon negative electrode material based on waste cotton textiles as described in claim 7.

9. The electrode plate according to claim 8, characterized in that: The preparation slurry of the electrode plate includes the low-cost hard carbon negative electrode material based on waste cotton textiles, Super P carbon black, CMC and SBR.

10. A sodium ion battery, characterized in that: Comprising the electrode plate as described in claim 8 or 9.

Citation Information

Patent Citations

  • Hard carbon material and preparation method thereof

    CN111564630A

  • Preparation method of sodium ion battery hard carbon-based negative electrode material based on waste fabric recycling

    CN116705999A

  • Bamboo-based hard carbon negative electrode material, preparation method thereof and sodium ion battery negative electrode

    CN117658107A

  • Preparation method and application of hard carbon taking cotton and hemp biomass as raw material

    CN118047370A

  • High-first-effect high-specific-volume biomass hard carbon, acid pretreatment preparation method thereof and sodium ion battery

    CN118183705A

Cited By

  • Short-range graphite and closed pore synergistic hard carbon negative electrode material and preparation method thereof

    CN119528115A

  • Short-range graphite-like and closed-pore synergistic hard carbon negative electrode material and preparation method thereof

    CN119528115B

  • Method for preparing hard carbon material from high-performance resin leftover material and application

    CN119976805A

  • Modified hard carbon material and preparation method thereof, negative pole piece and sodium ion battery

    CN121247773A