Polymer electrolyte type styrene-butadiene emulsion binder for negative electrode of lithium battery as well as preparation method and application of polymer electrolyte type styrene-butadiene emulsion binder
By using strong electrolyte polymer styrene butadiene emulsion binder, the shortcomings of the negative electrode binder of lithium ion battery in terms of gel content and particle size are solved, the performance and stability of the battery are improved, and the efficient lithium ion battery is achieved. Cycle life.
Patent Information
- Application Number
- CN202411022194.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-29
AI Technical Summary
The existing lithium-ion battery negative electrode binder has shortcomings in high gel content and small particle size, which affects the performance and cycle life of the battery.
A strong electrolyte type polymer styrene butadiene emulsion binder consisting of repeating units produced by copolymerization of unsaturated olefins, sulfonate ionic repeating units, carboxylate ionic repeating units and difunctional acrylate microcrosslinking units, is adopted. Emulsion polymerization and alkali neutralization treatment improve gel content and bonding properties.
It significantly improves the skeleton stability of the negative electrode material and the cycle stability of the battery, improves the performance and life of lithium-ion batteries, and avoids the problem of medium-strong acid corrosion caused by persulfate initiators.
Smart Images

Figure CN118956296A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of lithium ion batteries, and in particular to a polymer electrolyte type styrene butadiene emulsion binder for a lithium battery negative electrode, and a preparation method and application thereof. Background Art
[0002] Lithium-ion batteries are widely used in consumer electronics, electric vehicles, aerospace vehicles, energy storage power stations and other fields due to their high voltage, high specific energy, stable discharge voltage, excellent cycle performance, safety and long life. A typical lithium-ion battery consists of a positive electrode, a negative electrode, a separator, an electrolyte (usually composed of lithium salt and an organic solvent) and a battery casing. Among them, the negative electrode is one of the core components of the battery, and its performance directly affects the efficiency and service life of the battery.
[0003] The negative electrode structure of lithium-ion batteries mainly includes negative electrode active materials, conductive agents, metal current collectors and binders. Although the amount of binder used is not large, it plays a vital role in the preparation of negative electrodes. The main function of the binder is to firmly bond the negative electrode active materials and conductive agent particles to the surface of the metal current collector to form a uniform and integrated structure, ensuring good electron and ion conduction between them, thereby reducing the internal resistance of the electrode and improving the performance and stability of the battery.
[0004] At present, styrene butadiene emulsion is a commonly used negative electrode binder. Styrene butadiene emulsion has good adhesion and chemical stability. In the preparation process of lithium batteries, it is often used in combination with sodium carboxymethyl cellulose (CMC) to improve the bonding effect and the structural stability of the electrode.
[0005] However, there is no literature report on the application of strong electrolyte polymer butadiene styrene emulsion with high gel content and small particle size in lithium battery negative electrode binder and its preparation method. This type of butadiene styrene emulsion can not only effectively enhance the bonding strength of electrode materials, but also maintain its structural stability during battery charging and discharging, thereby improving the performance and cycle life of lithium-ion batteries. Summary of the invention
[0006] The purpose of the present invention is to develop a lithium battery negative electrode binder with high gel content, small emulsion particle size and good bonding performance.
[0007] The first aspect of the present invention is:
[0008] A binder is provided.
[0009] The second aspect of the present invention is:
[0010] Provided is a method for preparing a binder.
[0011] The third aspect of the present invention is:
[0012] Application of the adhesive.
[0013] Specifically, the technical solution adopted according to the first aspect of the present invention is:
[0014] A binder comprising repeating units produced by copolymerization of unsaturated olefins, sulfonate ionic repeating units of formula (1), carboxylate ionic repeating units of formula (2), and difunctional acrylate micro-crosslinking units of formula (3);
[0015] Wherein, the structural formula of formula (1) is:
[0016]
[0017] Wherein, the structural formula of formula (2) is at least one of (2)-a, (2)-b and (2)-c:
[0018]
[0019] Wherein, the structural formula of formula (3) is:
[0020]
[0021] Among them, M 1 is one of Li, Na and K;
[0022] Among them, M 2 、M 3 、M 4 、M 5 and M 6 Each of the following is independently selected from one of Li, Na, K and H, and not all of them are H;
[0023] Wherein, R is one of C2-C8 alkyl, ethylene oxide, propylene oxide, polyoxyethylene and polyoxypropylene;
[0024] Among them, R 1 CH 3 or H.
[0025] According to the embodiments of the present invention, one of the technical solutions has at least one of the following advantages or beneficial effects:
[0026] In the binder of the present invention, the structures of formula (1) and formula (2) mainly function to increase the stability, electrolyte properties and ion transport properties of the emulsion; the structure of formula (3) mainly functions to increase the skeleton stability of the polymer, improve the gel content and increase the polymer's resistance to organic electrolytes.
[0027] Specifically, the structure of formula (3) can make the binder of the present invention have a certain degree of crosslinking, so that its gel content is increased to more than 90wt%, thereby greatly improving the skeleton stability of the negative electrode material in the organic solvent electrolyte; the structural units of formula (1) and formula (2) in the emulsion polymerization reaction (before neutralization M 2 、M 3 、M 4 、M 5 and M 6 Most of the carboxyl groups are concentrated on the surface of latex particles, and can form sufficient polarity and ionicity after neutralization with alkali (M after neutralization). 2 、M 3 、M 4 、M 5 and M 6 Most of the H is replaced by ions to form carboxylates), which have good compatibility with lithium salts and organic solvents that are components of the electrolyte. When used in combination with carboxymethyl cellulose, it has good compatibility and excellent dispersion stability for negative electrode active fillers and conductive agent particles.
[0028] In addition, the binder of the present invention has high emulsion ion content, good stability, good compatibility with carboxymethyl cellulose, and is beneficial to the transmission of lithium ions between the negative electrode interface and the electrolyte.
[0029] According to one embodiment of the present invention, the base used for neutralization includes LiOH.
[0030] According to one embodiment of the present invention, the repeating unit produced by copolymerization of unsaturated olefins is a repeating unit of a copolymer produced by copolymerization of butadiene and styrene initiated by an initiator.
[0031] According to one embodiment of the present invention, the repeating unit produced by copolymerization of unsaturated olefins is a repeating unit of a copolymer produced by emulsion copolymerization of butadiene and styrene initiated by a persulfate initiator.
[0032] In the emulsion polymerization process, butadiene and styrene undergo emulsion polymerization under the thermal initiation of a persulfate initiator. In addition to producing styrene monomer units (formula (4)) and butadiene isomeric units (formula (5)), a small amount of cross-linked monomer units (formula (6)) and initiator terminal units with ionic properties (formula (7)), persulfate decomposes to produce free radicals and then initiates the monomer polymerization reaction, and also decomposes as shown below to produce a medium-strong acid in hydrogen sulfate, thereby making the system acidic. Not only will it cause greater corrosion to the metal, causing the introduction of high-priced metal ions into the emulsion to cause possible blockage of lithium ion channels, but it will also cause it to contact with the metal surface to produce more residues. Therefore, although the persulfate initiator can initiate the polymerization reaction of the present invention, it will also bring new problems, namely, it will cause more residues to be produced. Based on this, the present invention uses a buffer bicarbonate to neutralize the medium-strong acid produced by the persulfate initiator, thereby avoiding the corrosion of the medium-strong acid and solving the problems caused by the persulfate initiator.
[0033]
[0034] According to one embodiment of the present invention, in the structural formula (3) of the binder, the unit molecular weight of R is within 600.
[0035] According to one embodiment of the present invention, the repeating unit produced by copolymerization of unsaturated olefins includes structures represented by formula (4), formula (5), formula (6) and formula (7);
[0036] Wherein, formula (4) is:
[0037]
[0038] Wherein, the structural formula of formula (5) is one of (5)-a, (5)-b and (5)-c:
[0039]
[0040] Wherein, the structural formula of formula (6) is one of (6)-a, (6)-b and (6)-c:
[0041]
[0042] Wherein, formula (7) is:
[0043]
[0044] According to one embodiment of the present invention, the mass ratio of the sulfonate ionic repeating unit of formula (1) to the difunctional acrylate micro-crosslinking unit of formula (3) is 3-13:0.2-1.
[0045] According to one embodiment of the present invention, the binder further comprises 0 to 10 wt % of units obtained by copolymerization of unsaturated carboxylic acid esters.
[0046] According to one embodiment of the present invention, the binder further comprises units obtained by copolymerization of unsaturated carboxylic acid ester and unsaturated olefin nitrile.
[0047] According to one embodiment of the present invention, the unsaturated olefin nitrile includes at least one of 2-butenenitrile, 3-butenenitrile and 2-methyl-2-butenenitrile.
[0048] According to one embodiment of the present invention, the unsaturated carboxylic acid ester includes at least one of acrylate, methacrylate, maleic acid diester and itaconic acid diester.
[0049] According to one embodiment of the present invention, the acrylic acid ester includes at least one of hydroxyethyl acrylate, hydroxypropyl acrylate, hydroxybutyl acrylate and C4-C8 alkyl acrylate.
[0050] According to one embodiment of the present invention, the methacrylate includes at least one of hydroxyethyl methacrylate, hydroxypropyl methacrylate, hydroxybutyl methacrylate and C4-C8 alkyl methacrylate.
[0051] According to one embodiment of the present invention, the maleic acid diester includes at least one of dimethyl maleate, diethyl maleate, dibutyl maleate, and diisooctyl maleate.
[0052] According to one embodiment of the present invention, the itaconate diester includes at least one of dimethyl itaconate, diethyl itaconate, dibutyl itaconate, and diisooctyl itaconate.
[0053] According to one embodiment of the present invention, the average particle size of the binder is 70 to 200 nm.
[0054] According to one embodiment of the present invention, the glass transition temperature of the binder is -10°C to +20°C.
[0055] Specifically, the technical solution adopted according to the second aspect of the present invention is:
[0056] A method for preparing the binder comprises the following steps:
[0057] S1 mixes styrene, additive 1 and water, and pre-emulsifies to obtain a monomer pre-emulsion;
[0058] S2. Mix the monomer pre-emulsion, initiator, water and additive 2 in a high pressure or normal pressure reaction device, and heat and react to obtain a slightly acidic seed emulsion;
[0059] S3: mixing the slightly acidic seed emulsion, additive 3, initiator and water in a high pressure reaction device, and heating and reacting to obtain a slightly acidic emulsion;
[0060] S4 adjusts the pH value of the slightly acidic emulsion to alkaline, and obtains the binder by heating and reducing pressure.
[0061] According to the embodiments of the present invention, one of the technical solutions has at least one of the following advantages or beneficial effects:
[0062] The binder of the invention is a strong electrolyte type polymer butadiene styrene emulsion. Firstly, since the amount of the binder used in the negative electrode raw material composition is small, its bonding force mainly comes from the particle bonding force of the latex particles. Therefore, the emulsion with small particle size and large polarity is more conducive to its dispersion and bonding. The average particle size of the binder emulsion of the invention is 70-200nm, the polarity is strong, the dispersion is good, and it is conducive to the improvement of the bonding force; secondly, the binder of the invention has a gel content of more than 90%, a stable skeleton structure, and is conducive to the cycle stability of the battery; thirdly, the binder of the invention contains a large amount of phenyl sulfonate side groups and carboxylate side groups, has good dispersibility, and is used in combination with CMC at a lower dosage, and has good dispersibility and good bonding performance for active materials and conductive agent particles; finally, the glass transition temperature of the binder emulsion of the invention when dried to form a film is within the range of -10°C to 20°C, and it is easy to construct and shape at room temperature or slightly lower temperature, and has a wide range of application.
[0063] According to one embodiment of the present invention, the additive 1 includes at least one of an emulsifier and a polymerizable monomer, and at least includes an emulsifier.
[0064] According to one embodiment of the present invention, the additive 2 includes at least one of bicarbonate, ionization functional monomer, butadiene-containing and thiol chain transfer agent, and at least includes bicarbonate and ionization functional monomer.
[0065] According to one embodiment of the present invention, the additive 3 includes an emulsifier, butadiene, styrene, a difunctional acrylate and an ionization functional monomer.
[0066] According to one embodiment of the present invention, the additive 3 includes a polymerizable monomer and / or a thiol chain transfer agent.
[0067] According to one embodiment of the present invention, the difunctional acrylate includes at least one of 1,2-ethylene glycol diacrylate, 1,2-propylene glycol diacrylate, 1,3-propylene glycol dipropionate, 1,4-butylene glycol diacrylate, 1,6-hexanediol diacrylate, ethylene glycol diacrylate, ethylene glycol dimethacrylate, propylene glycol diacrylate, propylene glycol dimethacrylate, polyethylene glycol diacrylate, polyethylene glycol dimethacrylate, polypropylene glycol diacrylate, and polypropylene glycol dimethacrylate.
[0068] According to one embodiment of the present invention, the molecular weight of the difunctional acrylate is not more than 600.
[0069] According to one embodiment of the present invention, in step S3, when difunctional acrylate is not used, the gel content of the obtained slightly acidic styrene butadiene emulsion is relatively low, below 85 wt% or even lower, because the conjugated diene monomer butadiene is only partially cross-linked during emulsion polymerization (Formula (6)), and a large part of it still retains the cis ((5)-a in Formula (5)), trans ((5)-b in Formula (5)) isomers or the terminal double bond structure ((5)-c in Formula (5)) of Formula (5).
[0070] According to one embodiment of the present invention, the polymerizable monomer includes at least one of acrylate, methacrylate, maleic acid diester, itaconate diester and unsaturated olefin nitrile.
[0071] According to one embodiment of the present invention, the ionization functional monomer comprises unsaturated carboxylic acid and vinylbenzene sulfonate. In the structural formula of the binder, the unit of formula (1) is derived from the vinylbenzene sulfonate in the ionization functional monomer.
[0072] According to one embodiment of the present invention, the unsaturated carboxylic acid comprises at least one of maleic acid, fumaric acid, itaconic acid and methacrylic acid. In the structural formula of the binder, the unit of formula (2) is derived from the unsaturated carboxylic acid and needs to be obtained by adjusting the pH value of the acidic emulsion to alkaline in step S4.
[0073] According to one embodiment of the present invention, the emulsifier includes at least one of C8-C16 long-chain alkyl sulfate, C8-C16 long-chain alkylbenzene sulfonate, and C8-C16 long-chain alkyl diphenyl ether disulfonate.
[0074] According to one embodiment of the present invention, the sulfate in the C8-C16 long-chain alkyl sulfate is a sodium salt, a potassium salt or a lithium salt.
[0075] According to one embodiment of the present invention, the sulfonate in the C8-C16 long-chain alkylbenzene sulfonate and the C8-C16 long-chain alkyl diphenyl ether disulfonate is a sodium salt, a potassium salt or a lithium salt.
[0076] According to one embodiment of the present invention, the initiator comprises persulfate.
[0077] According to one embodiment of the present invention, the persulfate includes at least one of sodium persulfate, potassium persulfate and ammonium persulfate.
[0078] According to one embodiment of the present invention, the bicarbonate includes at least one of sodium bicarbonate and potassium bicarbonate.
[0079] According to one embodiment of the present invention, the mercaptan chain transfer agent includes at least one of tert-dodecyl mercaptan and dodecyl mercaptan.
[0080] According to one embodiment of the present invention, in step S2, the heating reaction is carried out at a temperature of 75 to 90°C.
[0081] According to one embodiment of the present invention, in step S2, the heating reaction is a two-step heating reaction, the temperature in the first step is 75-85°C, and the temperature in the second step is 85-90°C.
[0082] According to one embodiment of the present invention, the slightly acidic seed emulsion obtained in step S2 has a solid content of 25 to 35 wt %.
[0083] According to one embodiment of the present invention, in step S3, the heating reaction is a heating reaction carried out at 70-85° C. and a pressure of less than 9 kg.
[0084] According to one embodiment of the present invention, in step S4, the pH value of the slightly acidic styrene butadiene emulsion is adjusted to 8-9.5.
[0085] According to one embodiment of the present invention, in step S4, the heating and reduced pressure treatment is performed at a temperature of 70 to 85°C.
[0086] According to one embodiment of the present invention, step S4 further includes the following steps: adjusting the pH value of the acidic emulsion to alkaline by adding an alkali solution, wherein the alkali solution is LiOH·H 2 O, NaOH or KOH.
[0087] According to one embodiment of the present invention, a method for preparing the binder comprises the following steps:
[0088] A1 mixes styrene, polymerizable monomers, an emulsifier and water, and pre-emulsifies to obtain a monomer pre-emulsion liquid;
[0089] A2 mixes the monomer pre-emulsion, initiator, bicarbonate, ionized functional monomer and water in a normal pressure reaction device, and heats and reacts to obtain a slightly acidic seed emulsion;
[0090] A3: mixing the slightly acidic seed emulsion, emulsifier, butadiene, styrene, difunctional acrylate, polymerization monomer, thiol chain transfer agent, ionization functional monomer, bicarbonate, water and initiator in a high-pressure reaction device after deoxygenation treatment, and heating and reacting to obtain a slightly acidic emulsion;
[0091] A4 adjusts the pH value of the slightly acidic emulsion to alkaline, and then heats and decompresses the emulsion to obtain the binder.
[0092] According to the embodiments of the present invention, one of the technical solutions has at least one of the following advantages or beneficial effects:
[0093] According to the method of the present invention, in steps A1-A2, butadiene is not added, so that the slightly acidic rigid-structured polystyrene seed emulsion prepared in A2 is a seed emulsion without a butadiene structure, and the latex particles of the seed emulsion have a rigid structure but no cross-linking structure, and the gel content is 0, so that in step A3, the latex particles of the seed emulsion can well adsorb and disperse the monomer, so that the latex particles swell, the monomers are firmly combined on the surface of the latex particles and grow larger through polymerization, which is conducive to forming hard-core-soft-shell core-shell structure particles and improving the bonding performance.
[0094] According to one embodiment of the present invention, sodium bicarbonate is added to construct a buffer system. If sodium bicarbonate is not added during the preparation of the binder, a large amount of residue will be generated during the preparation process.
[0095] According to one embodiment of the present invention, in step A2, the ratio of sodium bicarbonate to initiator is 1-1.5:20-60.
[0096] According to one embodiment of the present invention, a method for preparing the binder comprises the following steps:
[0097] B1 mixes styrene, polymerization monomer, mercaptan chain transfer agent, emulsifier and water, and pre-emulsifies to obtain monomer pre-emulsion;
[0098] B2 Mix the monomer pre-emulsion, initiator, bicarbonate, butadiene, ionized functional monomer and water in a high pressure reaction device, and heat to react to obtain a slightly acidic butadiene styrene seed emulsion;
[0099] B3: mixing the acidic styrene butadiene seed emulsion, emulsifier, styrene, difunctional acrylate, polymerization monomer, thiol chain transfer agent, butadiene, ionization functional monomer, initiator, bicarbonate and water in a high pressure reaction device, and heating and reacting to obtain an acidic emulsion;
[0100] B4 adjusts the pH value of the slightly acidic emulsion to alkaline, and obtains the binder by heating and reducing pressure.
[0101] According to the embodiments of the present invention, one of the technical solutions has at least one of the following advantages or beneficial effects:
[0102] The method of the present invention introduces butadiene in step B1-B2, so that the slightly acidic butadiene styrene seed emulsion prepared in step B2 is a seed emulsion containing a butadiene structure, the seed emulsion contains a cross-linked structure and the gel content is not 0; in step B3, during the process of introducing a butadiene-containing monomer into the seed emulsion for repolymerization and growth, the unit composition of the mixed monomer is similar to that of the latex particles of the seed emulsion, which is beneficial to the adsorption and dispersion of the mixed monomer on the surface of the seed emulsion particles, so that the mixed monomer is firmly combined on the surface of the particles and grows larger through polymerization, thereby obtaining a stable emulsion.
[0103] Another aspect of the present invention further provides a lithium battery negative electrode, including the binder as described in the first embodiment. Since the application adopts all the technical solutions of the above binder, it at least has all the beneficial effects brought by the technical solutions of the above embodiment.
[0104] Other features and advantages of the present invention will be set forth in the description which follows, and in part will be apparent from the description, or may be learned by practice of the present invention. DETAILED DESCRIPTION
[0105] In the description of the present invention, if there is a description of first, second, etc., it is only for the purpose of distinguishing technical features, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features or implicitly indicating the order of the indicated technical features.
[0106] The words "preferably", "more preferably", etc. in the present invention refer to embodiments of the present invention that may provide certain beneficial effects in certain circumstances. However, other embodiments may also be preferred under the same circumstances or other circumstances. In addition, the description of one or more preferred embodiments does not imply that other embodiments are not applicable, nor is it intended to exclude other embodiments from the scope of the present invention.
[0107] When a numerical range is disclosed herein, the above range is considered to be continuous and includes the minimum and maximum values of the range, as well as every value between such minimum and maximum values. Further, when a range refers to an integer, every integer between the minimum and maximum values of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be combined. In other words, unless otherwise indicated, all ranges disclosed herein should be understood to include any and all subranges included therein.
[0108] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of the present invention.
[0109] Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.
[0110] Example 1
[0111] The binder of Example 1 contains units of the following formulae (1) to (3):
[0112]
[0113] Prepare the raw materials and reagents as follows:
[0114] Dissolve 0.95 g of initiator potassium persulfate in 48.89 g of deionized water to prepare an initiator aqueous solution 1, then add 0.16 g of sodium bicarbonate to neutralize, to obtain 50 g of initiator composite aqueous solution 1 for later use;
[0115] 1.0 g of ionizable functional monomer sodium 4-vinylbenzenesulfonate and 1.5 g of maleic acid were dissolved in 37.5 g of deionized water to obtain 40 g of ionizable functional monomer aqueous solution 1 (see Table 1 for details);
[0116] A fixed mass of 75.0 g of butadiene was introduced into one of the tanks of a 1-liter stainless steel autoclave equipped with four pressure-resistant dropping tanks that had been nitrogen-purged, deoxygenated, and decompressed, and the mixture was set aside;
[0117] In a normal pressure device, 90.3 g of styrene, 2.0 g of tripropylene glycol diacrylate, 1.8 g of hydroxyethyl methacrylate, 2.0 g of dibutyl itaconate and 0.2 g of tert-dodecyl mercaptan were weighed and mixed to obtain 96.3 g of a monomer mixture (see Table 3 for details), which was placed in a mixed monomer storage tank of a high-pressure reactor for standby use;
[0118] 1.9 g of initiator potassium persulfate was dissolved in 97.8 g of deionized water, and then 0.3 g of sodium bicarbonate was added for neutralization to obtain 100 g of initiator composite aqueous solution 2, which was placed in a water phase initiator storage tank of a high-pressure reactor for standby use;
[0119] Dissolve 2.0 g of sodium 4-vinylbenzenesulfonate and 6.9 g of itaconic acid in 91.1 g of deionized water to prepare 100 g of ionized functional monomer aqueous solution 2, and place it in the fourth storage tank of the autoclave for standby use;
[0120] A method for preparing a binder comprises the following steps:
[0121] S1 92.5 g of styrene and 5 g of dibutyl maleate were uniformly mixed, and then added dropwise to a mixed solution containing 1.0 g of emulsifier sodium dodecyl sulfate, 1.0 g of sodium dodecylbenzene sulfonate, 1.0 g of sodium dodecyl diphenyl ether disulfonate and 134.84 g of deionized water under high-speed stirring at room temperature at 660 rpm for pre-emulsification to obtain 235.34 g of monomer pre-emulsion;
[0122] S2: Weigh 45g of monomer pre-emulsion and put it into a normal pressure reactor as a base material, add 10g of the prepared initiator composite aqueous solution 1, stir the reactor at 200rpm, raise the oil bath temperature to 80°C, and start dripping the remaining monomer pre-emulsion and the remaining initiator aqueous solution 1 and ionizable functional monomer aqueous solution 1 when the reaction liquid appears blue light, keep the reaction liquid temperature at 80°C, and the dripping time is 0.8h. After the dripping is completed, keep the oil bath temperature at 90°C for 2 hours, cool, and pass through a 200-mesh filter to obtain 325.0g of acidic polystyrene seed emulsion, and the dry weight of the filter residue after filtration is 0.12g;
[0123] S3 weighed 66.6g of slightly acidic polystyrene seed emulsion, 0.8g of sodium dodecyl sulfate, 0.8g of sodium dodecylbenzene sulfonate, 0.8g of sodium dodecyl diphenyl ether disulfonate and 47.1g of deionized water, mixed evenly to obtain a base material mixture, placed it in a high-pressure reactor, and then the high-pressure reactor was heated to 75°C, the stirring speed of the reactor was 150rpm, butadiene, monomer mixture, initiator composite aqueous solution 2, ionized functional monomer aqueous solution 2 were added dropwise at a pressure below 9 kg and reacted, the reaction liquid temperature was maintained at 75°C, the dropping time was 1h, after the dropwise addition was completed, the temperature was raised to 85°C and the reaction was kept warm for 2 hours, cooled, and passed through a 200-mesh filter to obtain 485g of slightly acidic butadiene-styrene emulsion, the solid content was measured to be 41.5wt%, the pH value was 2, and the total dry weight of the filter residue after filtration was 0.39g;
[0124] S4 Add 10 wt% LiOH·H 2 O alkaline solution was neutralized for 10 minutes. 42.0 g (94.2 wt% of the theoretical amount) was required to neutralize to pH 9. At this time, most of the carboxyl -COOH had been converted into -COOLi. Finally, it was heated to 80 ° C and vacuum distilled for 2 h to remove unreacted volatile monomers. After cooling, 510 g of the above-mentioned binder was obtained after filtering through a 200-mesh filter.
[0125] The slightly acidic polystyrene seed emulsion obtained in step S2 has a solid content of 30.4 wt %, an average particle size of 79 nm, and an emulsion pH of 3. 32.5 g of the sample is added with 5% NaOH and stirred for 3 minutes to neutralize to a pH of 9, and 2.0 g is required, which is 96.7 wt % of the theoretical amount of maleic acid to be neutralized.
[0126] The binder obtained in step S4 has a solid content of 39.6 wt %, an average particle size of 133 nm, a dry film gel content (THF) of 93.7 wt %, and a dry film glass transition temperature of 2.4° C.
[0127] Example 2
[0128] The binder of Example 2 contains units of the following formulae (1) to (3):
[0129]
[0130] Prepare the raw materials and reagents as follows:
[0131] Dissolve 0.95 g of initiator potassium persulfate in 48.89 g of deionized water to prepare an initiator aqueous solution 1, then add 0.16 g of sodium bicarbonate to neutralize, to obtain 50 g of initiator composite aqueous solution 1 for later use;
[0132] 0.5 g of ionizable functional monomer sodium 4-vinylbenzenesulfonate and 2.0 g of methacrylic acid were dissolved in 37.5 g of deionized water to obtain 40 g of ionizable functional monomer aqueous solution 1 (see Table 1 for details);
[0133] A fixed mass of 65.0 g of butadiene is introduced into one of the tanks of a 1-liter stainless steel autoclave equipped with four pressure-resistant dropping storage tanks that has been treated with nitrogen, deoxygenation and decompression to obtain butadiene for step S3, which is set aside;
[0134] In a normal pressure device, 100.3 g of styrene, 2.0 g of triethylene glycol dimethacrylate, 1.8 g of hydroxyethyl methacrylate, 2.0 g of dibutyl itaconate and 0.2 g of tert-dodecyl mercaptan were weighed and mixed to obtain 106.3 g of a monomer mixture (see Table 3 for details), which was placed in a mixed monomer storage tank of a high-pressure reactor for standby use;
[0135] 1.9 g of initiator potassium persulfate was dissolved in 97.8 g of deionized water, and then 0.3 g of sodium bicarbonate was added for neutralization to obtain 100 g of initiator composite aqueous solution 2, which was placed in a water phase initiator storage tank of a high-pressure reactor for standby use;
[0136] 3.0 g of sodium 4-vinylbenzenesulfonate and 5.9 g of methacrylic acid were dissolved in 91.1 g of deionized water to prepare 100 g of an ionizable functional monomer aqueous solution 2, which was placed in the fourth storage tank of the autoclave for standby use;
[0137] A method for preparing a binder comprises the following steps:
[0138] S1 87.5 g of styrene and 10 g of dibutyl maleate were uniformly mixed, and then added dropwise to a mixed solution containing 1.0 g of emulsifier sodium dodecyl sulfate, 1.0 g of sodium dodecylbenzene sulfonate, 1.0 g of sodium dodecyl diphenyl ether disulfonate and 134.84 g of deionized water under high-speed stirring at room temperature at 660 rpm for pre-emulsification to obtain 235.34 g of monomer pre-emulsion;
[0139] S2: 45g of monomer pre-emulsion was put into a normal pressure reactor as a base material, 10g of the prepared initiator composite aqueous solution 1 was added, the reactor was stirred at 200rpm, the oil bath temperature was raised to 80°C, and when the reaction liquid showed blue light, the remaining monomer pre-emulsion, the remaining initiator aqueous solution 1 and the ionizable functional monomer aqueous solution 1 were added dropwise, the reaction liquid temperature was kept at 82°C, the dropping time was 0.8h, and after the dropping was completed, the oil bath temperature was kept at 90°C for 2 hours, cooled, and filtered through a 200-mesh filter to obtain 324.0g of a slightly acidic polystyrene seed emulsion, and the dry weight of the filter residue after filtration was 0.17g;
[0140] S3 weighed 66.6g of slightly acidic polystyrene seed emulsion, 0.8g of sodium dodecyl sulfate, 0.8g of sodium dodecylbenzene sulfonate, 0.8g of sodium dodecyl diphenyl ether disulfonate and 47.1g of deionized water, mixed evenly to obtain a base material mixture, placed it in a high-pressure reactor, and then the high-pressure reactor was heated to 80°C, the stirring speed of the reactor was 150rpm, butadiene, monomer mixture, initiator composite aqueous solution 2, ionized functional monomer aqueous solution 2 were added dropwise at a pressure below 9 kg and reacted, the reaction liquid temperature was maintained at 78°C, the dropping time was 1h, after the dropwise addition was completed, the temperature was raised to 80°C and the reaction was kept warm for 3 hours, cooled, and passed through a 200-mesh filter to obtain 483g of slightly acidic butadiene-styrene emulsion, the solid content was measured to be 41.6wt%, the pH value was 3, and the total dry weight of the filter residue after filtration was 0.45g;
[0141] S4: Add 10 wt% LiOH·H 2 O alkaline solution for neutralization for 10 minutes, and 27.0g (93.8wt% of the theoretical amount) is required to neutralize to pH 9. At this time, most of the carboxyl -COOH has been converted into -COOLi. Finally, it is heated to 80°C and distilled under reduced pressure for 2h to remove unreacted volatile monomers. After cooling, 493g of the above-mentioned binder is obtained after filtering through a 200-mesh filter.
[0142] The slightly acidic polystyrene seed emulsion obtained in step S2 has a solid content of 30.3 wt %, an average particle size of 74 nm, and an emulsion pH of 3. 32.4 g of the sample is added with 5% NaOH and stirred for 3 minutes to neutralize to a pH of 9, and 1.72 g is required, which is 92.5 wt % of the theoretical amount of methacrylic acid to be neutralized.
[0143] The binder obtained in step S4 has a solid content of 40.8 wt %, an average particle size of 128 nm, a dry film gel content (THF) of 94.2 wt %, and a dry film glass transition temperature of 11.3° C.
[0144] Example 3
[0145] The binder of Example 3 contains units of the following formulae (1) to (3):
[0146]
[0147] Prepare the raw materials and reagents as follows:
[0148] A fixed mass of 66.6 g of butadiene is introduced into one of the tanks in a 1-liter stainless steel autoclave 1 equipped with four pressure-resistant dropping tanks and treated with nitrogen, deoxygenation and decompression to obtain butadiene for step S2, which is set aside;
[0149] 1.9 g of initiator potassium persulfate was dissolved in 97.8 g of deionized water under normal pressure to prepare an initiator aqueous solution 3, and then 0.3 g of sodium bicarbonate was added for neutralization to obtain 100 g of initiator composite aqueous solution 3, which was placed in a water phase initiator storage tank of the autoclave 1 for standby use;
[0150] Dissolve 2.0 g of sodium 4-vinylbenzenesulfonate and 5.7 g of maleic acid in 92.3 g of deionized water to prepare an ionized functional monomer aqueous solution 3, and place the aqueous solution in the fourth storage tank of the autoclave 1 for standby use;
[0151] A fixed mass of 70.0 g of butadiene is introduced into one of the tanks of a 1-liter stainless steel autoclave 2 equipped with four pressure-resistant dropping tanks after nitrogen flow, deoxygenation and decompression treatment to obtain butadiene for step S3, which is set aside;
[0152] In a normal pressure device, 96.0 g of styrene, 2.0 g of 1,6-hexanediol diacrylate, 2.0 g of hydroxyethyl methacrylate, and 0.25 g of tert-dodecyl mercaptan were weighed and mixed to obtain 100.25 g of a monomer mixture (see Table 4 for details), which was placed in a mixed monomer storage tank of a high-pressure reactor 2 for standby use;
[0153] 1.7 g of initiator sodium persulfate was dissolved in 97.9 g of deionized water, and then 0.4 g of sodium bicarbonate was added for neutralization to obtain 100 g of initiator composite aqueous solution 4, which was placed in the water phase initiator storage tank of the autoclave 2 for standby use;
[0154] In addition, 5.0 g of potassium 4-vinylbenzenesulfonate and 10.0 g of maleic acid were dissolved in 85 g of deionized water to prepare 100 g of an ionizable functional monomer aqueous solution 4, which was placed in the fourth storage tank of the autoclave 2 for standby use.
[0155] The seed emulsion prepared in Example 3 is a seed emulsion containing a butadiene structure, and the seed emulsion contains a cross-linked structure and the gel content is not zero.
[0156] A method for preparing a binder comprises the following steps:
[0157] S1: 123.8 g of styrene, 1.9 g of hydroxyethyl methacrylate and 0.5 g of tert-dodecyl mercaptan were weighed and mixed in a normal pressure device, and the mixture was added dropwise to a mixed solution containing 253.1 g of deionized water, 4.0 g of sodium dodecyl sulfate and 2.0 g of sodium dodecylbenzene sulfonate under high-speed stirring at room temperature and 600 rpm for pre-emulsification to obtain 385.3 g of a monomer pre-emulsion solution free of butadiene (see Table 2 for details);
[0158] S2: 385.3g of monomer pre-emulsion liquid without butadiene is passed into the pre-emulsification stirring tank in the autoclave 1 which has been deoxygenated, and the rotation speed is maintained at 100rpm. First, 10wt% of the monomer pre-emulsion liquid is passed into the autoclave, and then the autoclave 1 is heated to 80°C, the stirring speed of the autoclave is 150rpm, butadiene, the initiator composite aqueous solution 3, the ionized functional monomer aqueous solution 3 and the remaining monomer pre-emulsion liquid are added dropwise at a pressure below 9 kg and reacted, the reaction liquid temperature is maintained at 80°C, the dropping time is 1h, and after the dropping is completed, the temperature is raised to 85°C and the reaction is kept warm for 2 hours, cooled, and passed through a 200-mesh filter to obtain 650g of a styrene-butadiene seed emulsion of a skeletal acidity. The total dry weight of the filter residue after filtration is 0.37g;
[0159] S3 weighs 50g of slightly acidic butadiene styrene seed emulsion, 1.0g of sodium dodecyl sulfate, 0.5g of sodium dodecylbenzene sulfonate and 63.6g of deionized water and mixes them evenly to obtain a base material mixture, which is placed in a high-pressure reactor 2, and then the high-pressure reactor 2 is heated to 70-80°C, the stirring speed of the reactor is 150rpm, butadiene, monomer mixture, initiator composite aqueous solution 4, ionized functional monomer aqueous solution 4 are added dropwise at a pressure below 9 kg and reacted, the reaction liquid temperature is maintained at 70-80°C, the dropping time is 1h, after the dropwise addition is completed, the temperature is raised to 80°C and the reaction is kept warm for 3 hours, cooled, and passed through a 200-mesh filter to obtain 481g of butadiene styrene emulsion, the solid content is measured to be 41.0wt%, the pH value is 3, the total dry weight of the filter residue after filtration is 0.47g, and a slightly acidic emulsion is obtained;
[0160] S4: Add 10 wt% LiOH·H 2 O alkaline solution was neutralized for 10 minutes. 70.0 g (96.6 wt% of the theoretical amount) was required to neutralize to pH 9. At this time, most of the carboxyl -COOH had been converted into -COOLi. Finally, it was heated to 80-85 ° C and vacuum distilled for 2 h to remove unreacted volatile monomers. After cooling, 530 g of the above-mentioned binder was obtained after filtering through a 200-mesh filter.
[0161] The slightly acidic styrene butadiene seed emulsion obtained in step S2 has a solid content of 30.1 wt %, an average particle size of 90 nm, and an emulsion pH of 3. 65 g of the sample is added with 5% NaOH and stirred for 3 minutes to neutralize to a pH of 9, and 7.2 g is required, which is 91.6 wt % of the theoretical amount of maleic acid to be neutralized.
[0162] The binder obtained in step S4 has a solid content of 37.4 wt %, an average particle size of 162 nm, a dry film gel content (THF) of 95.6 wt %, and a dry film glass transition temperature of 5.5° C.
[0163] Example 4
[0164] The binder of Example 4 contains units of the following formulae (1) to (3):
[0165]
[0166] Prepare the raw materials and reagents as follows:
[0167] A fixed mass of 66.6 g of butadiene is introduced into one of the tanks in a 1-liter stainless steel autoclave 1 equipped with four pressure-resistant dropping tanks and treated with nitrogen, deoxygenation and decompression to obtain butadiene for step S2, which is set aside;
[0168] 1.9 g of initiator potassium persulfate was dissolved in 97.8 g of deionized water to prepare an initiator aqueous solution 3, and then 0.3 g of sodium bicarbonate was added for neutralization to obtain 100 g of initiator composite aqueous solution 3, which was placed in a water phase initiator storage tank of the autoclave 1 for standby use;
[0169] 1.0 g of sodium 4-vinylbenzenesulfonate and 6.7 g of methacrylic acid are dissolved in 92.3 g of deionized water to prepare an ionizable functional monomer aqueous solution 3, which is placed in the fourth storage tank of the autoclave 1 for standby use;
[0170] A fixed mass of 70.0 g of butadiene is introduced into one of the tanks of a 1-liter stainless steel autoclave 2 equipped with four pressure-resistant dropping tanks after nitrogen flow, deoxygenation and decompression treatment to obtain butadiene for step S3, which is set aside;
[0171] In a normal pressure device, 81.0 g of styrene, 2.0 g of 1,6-hexanediol diacrylate, 2.0 g of hydroxyethyl methacrylate, and 0.25 g of tert-dodecyl mercaptan were weighed and mixed to obtain 85.25 g of a monomer mixture (see Table 4 for details), which was placed in a mixed monomer storage tank of a high-pressure reactor 2 for standby use;
[0172] 1.7 g of initiator sodium persulfate was dissolved in 97.9 g of deionized water, and then 0.4 g of sodium bicarbonate was added for neutralization to obtain 100 g of initiator composite aqueous solution 4, which was placed in the water phase initiator storage tank of the autoclave 2 for standby use;
[0173] 5.0 g of potassium 4-vinylbenzenesulfonate and 10.0 g of maleic acid were dissolved in 85 g of deionized water to prepare 100 g of ionizable functional monomer aqueous solution 4, which was placed in the fourth storage tank of the autoclave 2 for standby use;
[0174] The seed emulsion prepared in Example 4 is a seed emulsion containing a butadiene structure, and the seed emulsion contains a cross-linked structure and the gel content is not zero.
[0175] A method for preparing a binder comprises the following steps:
[0176] S1: 123.8 g of styrene, 1.9 g of hydroxyethyl methacrylate and 0.5 g of tert-dodecyl mercaptan were weighed and mixed in a normal pressure device, and the mixture was added dropwise to a mixed solution containing 253.1 g of deionized water, 2.0 g of sodium dodecyl sulfate, 2.0 g of sodium dodecylbenzene sulfonate and 2.0 g of sodium dodecyl diphenyl ether disulfonate under high-speed stirring at room temperature and 600 rpm for pre-emulsification to obtain 385.3 g of a monomer pre-emulsion solution free of butadiene (see Table 2 for details);
[0177] S2: 385.3g of monomer pre-emulsion liquid without butadiene is passed into the pre-emulsification stirring tank of the autoclave 1 which has been deoxygenated, and the rotation speed is maintained at 100rpm. First, 10wt% of the monomer pre-emulsion liquid is passed into the autoclave 1, and then the autoclave is heated to 75°C, the stirring speed of the autoclave is 150rpm, butadiene, the initiator composite aqueous solution 3, the ionized functional monomer aqueous solution 3 and the remaining monomer pre-emulsion liquid are added dropwise at a pressure below 9 kg and reacted, the reaction liquid temperature is maintained at 75°C, the dropping time is 1h, and after the dropping is completed, the temperature is raised to 85°C and the reaction is kept warm for 2 hours, cooled, and passed through a 200-mesh filter to obtain 648g of a styrene-butadiene seed emulsion of a skeletal acidity. The total dry weight of the filter residue after filtration is 0.52g;
[0178] S3: 100g of slightly acidic styrene butadiene seed emulsion, 0.3g of sodium dodecyl sulfate, 0.3g of sodium dodecylbenzene sulfonate, 0.3g of sodium dodecyl diphenyl ether disulfonate and 28.6g of deionized water are weighed and mixed to obtain a base material mixture, which is placed in a high-pressure reactor 2, and then the high-pressure reactor 2 is heated to 78°C, the stirring speed of the reactor is 150rpm, butadiene, monomer mixture, initiator composite aqueous solution 4, ionized functional monomer aqueous solution 4 are added dropwise at a pressure below 9 kg and reacted, the reaction liquid temperature is maintained at 78°C, the dropping time is 1h, and after the dropwise addition is completed, the temperature is raised to 80°C and the reaction is kept warm for 3 hours, cooled, and passed through a 200-mesh filter to obtain 480g of slightly acidic styrene butadiene emulsion, the solid content is measured to be 41.3wt%, the pH value is 3, and the total dry weight of the filter residue after filtration is 0.40g;
[0179] S4 Add 10 wt% LiOH·H 2 O alkaline solution was neutralized for 10 minutes. 70.5 g (97.3 wt% of the theoretical amount) was required to neutralize to pH 9. At this time, most of the carboxyl -COOH had been converted into -COOLi. Finally, it was heated to 80-85 ° C and vacuum distilled for 2 h to remove unreacted volatile monomers. After cooling, 531 g of the above-mentioned binder was obtained after filtering through a 200-mesh filter.
[0180] The slightly acidic styrene butadiene seed emulsion obtained in step S2 has a solid content of 30.3 wt %, an average particle size of 84 nm, and an emulsion pH of 3. 64.8 g of the sample is added with 5% NaOH and stirred for 3 minutes to neutralize to a pH of 9, and 5.8 g is required, which is 93.1 wt % of the theoretical amount of methacrylic acid to be neutralized.
[0181] The binder obtained in step S4 has a solid content of 37.5 wt %, an average particle size of 137 nm, a dry film gel content (THF) of 94.1 wt %, and a dry film glass transition temperature of 3.8° C.
[0182] Comparative Example 1
[0183] Prepare the raw materials and reagents as follows:
[0184] Dissolve 0.95 g of initiator potassium persulfate in 48.89 g of deionized water to prepare an initiator aqueous solution 1, then add 0.16 g of sodium bicarbonate to neutralize, and obtain 50 g of initiator composite aqueous solution 1 (see Table 1 for details), which is set aside;
[0185] 0.5 g of ionizable functional monomer sodium 4-vinylbenzenesulfonate and 2.0 g of methacrylic acid were dissolved in 37.5 g of deionized water to obtain 40 g of ionizable functional monomer aqueous solution 1 (see Table 1 for details);
[0186] A method for preparing a binder comprises the following steps:
[0187] S1 88 g of styrene was uniformly mixed with 10 g of dibutyl maleate and 2.0 g of methacrylic acid, and then the mixture was added dropwise to a mixed solution containing 1.0 g of emulsifier sodium dodecyl sulfate, 1.0 g of sodium dodecylbenzene sulfonate, 1.0 g of sodium dodecyl diphenyl ether disulfonate and 172.34 g of deionized water under high-speed stirring at room temperature at 660 rpm for pre-emulsification to obtain 275.34 g of monomer pre-emulsion;
[0188] S2 Take 53g of monomer pre-emulsion and put it into the reactor as the base material, add 10g of the prepared initiator composite aqueous solution 1, stir at 200rpm in the reactor, raise the oil bath temperature to 80℃, and start adding the remaining monomer pre-emulsion and the remaining initiator aqueous solution 1 when the reaction liquid appears blue light, keep the reaction liquid temperature at 80℃, the dropping time is 0.8h, and after the dropping is completed, keep the oil bath temperature at 90℃ for 2 hours, cool, and pass through a 200-mesh filter to obtain 322.0g of slightly acidic polystyrene seed emulsion. The dry weight of the filter residue after filtration is 0.35g.
[0189] The slightly acidic polystyrene seed emulsion obtained in step S2 has a solid content of 30.1 wt %, an average particle size of 72 nm, and an emulsion pH of 4. 32.2 g of the sample is added with 5% NaOH and stirred for 3 minutes to neutralize to a pH of 9, and 0.899 g is required, which is 48.3 wt % of the theoretical amount of methacrylic acid to be neutralized.
[0190] Comparative Example 2
[0191] Prepare the raw materials and reagents as follows:
[0192] A fixed mass of 66.6 g of butadiene was introduced into one of the tanks of a 1-liter stainless steel autoclave equipped with four pressure-resistant dropping tanks that had been nitrogen-passed, deoxygenated, and decompressed, and was set aside;
[0193] The monomer pre-emulsion liquid not containing butadiene is placed in a mixed monomer storage tank of a high-pressure reactor for standby use;
[0194] 1.9 g of initiator potassium persulfate was dissolved in 98.1 g of deionized water to prepare 100 g of initiator composite aqueous solution 3, which was placed in a water phase initiator storage tank of a high-pressure reactor for standby use;
[0195] A method for preparing a binder comprises the following steps:
[0196] S1: 123.8 g of styrene, 1.9 g of hydroxyethyl methacrylate, 7.7 g of methacrylic acid and 0.5 g of tert-dodecyl mercaptan were weighed and mixed in a normal pressure device, and the mixture was added dropwise to a mixed solution containing 345 g of deionized water, 4.0 g of sodium dodecyl sulfate and 2.0 g of sodium dodecylbenzene sulfonate under high-speed stirring at room temperature and 600 rpm for pre-emulsification to obtain 484.9 g of a monomer pre-emulsion solution free of butadiene (see Table 2 for details);
[0197] S2: 484.9g of monomer pre-emulsion liquid that does not contain butadiene is passed into the pre-emulsification stirring storage tank in the high-pressure reaction device that has been deoxygenated, and the rotation speed is maintained at 100rpm. First, 10wt% of the monomer pre-emulsion liquid is passed into the high-pressure reactor, and then the high-pressure reactor is heated to 70-80°C, the reactor stirring speed is 150rpm, butadiene, the initiator composite aqueous solution 3 and the remaining monomer pre-emulsion liquid are added dropwise at a pressure below 9 kg and reacted, the reaction liquid temperature is maintained at 80°C, the dropping time is 1h, and after the dropping is completed, the temperature is raised to 85°C and the reaction is kept warm for 2 hours, cooled, and passed through a 200-mesh filter to obtain 640g of slightly acidic butadiene styrene seed emulsion. The total dry weight of the filter residue after filtration is 3.56g.
[0198] The experimental results show that the slightly acidic styrene butadiene seed emulsion obtained in step S2 has a solid content of 30.5wt%, an average particle size of 93nm, and an emulsion pH of 1, which is particularly acidic. 64g of the sample is taken, and 4.4g is required when 5% NaOH is added and stirred for 3 minutes to neutralize to a pH of 9, which is 61.4wt% of the theoretical amount of methacrylic acid.
[0199] Comparative Example 3
[0200] Prepare the raw materials and reagents as follows:
[0201] A fixed mass of 65.0 g of butadiene was introduced into one of the tanks of a 1-liter stainless steel autoclave equipped with four pressure-resistant dropping tanks that had been nitrogen-passed, deoxygenated, and decompressed, and was set aside;
[0202] In a normal pressure device, 100.3 g of styrene, 2.0 g of triethylene glycol dimethacrylate, 1.8 g of hydroxyethyl methacrylate, 2.0 g of dibutyl itaconate, 6.9 g of methacrylic acid and 0.2 g of tert-dodecyl mercaptan were weighed and mixed to obtain 113.2 g of a monomer mixture (see Table 3 for details), which was placed in a mixed monomer storage tank of a high-pressure reactor for standby use;
[0203] Dissolve 1.9 g of initiator potassium persulfate in 97.9 g of deionized water to prepare 100 g of initiator composite aqueous solution 2, and place it in a water phase initiator storage tank of a high-pressure reactor for standby use;
[0204] A method for preparing a binder comprises the following steps:
[0205] S1 weighs 66.6g of the acidic polystyrene seed emulsion prepared in Example 2, 0.8g of sodium dodecyl sulfate, 0.8g of sodium dodecylbenzene sulfonate, 0.8g of sodium dodecyl diphenyl ether disulfonate and 138.0g of deionized water, and mixes them evenly to obtain a base material mixture, which is placed in a high-pressure reactor, and then the high-pressure reactor is heated to 70-80°C, the stirring speed of the reactor is 150rpm, and butadiene, monomer mixture, and initiator composite aqueous solution 2 are added dropwise at a pressure below 9 kg and reacted, maintaining the reaction liquid temperature at 70-80°C, the dropping time is 1h, and after the dropwise addition is completed, the temperature is raised to 80°C and the reaction is kept warm for 3 hours, cooled, and 470g of butadiene-styrene emulsion is obtained after passing through a 200-mesh filter screen. The total dry weight of the filter residue after filtration is 2.5g. Sampling is measured, and its solid content is 40.8wt%, and the pH value is 1;
[0206] 47 g of the styrene butadiene emulsion obtained in S2 was treated with 10 wt% LiOH·H 2 The binder was obtained by neutralizing with an alkali solution of 0 for 10 minutes until the pH value was 9. The neutralization required 1.7 g of alkali solution, which was 50.4% of the theoretical amount to neutralize all carboxyl groups.
[0207] The components of the raw materials used in the preparation of the slightly acidic seed emulsion in steps S1-S2 in the preparation methods of Examples 1-2 and Comparative Example 1 were statistically analyzed, and the statistical results are shown in Table 1.
[0208] Table 1
[0209]
[0210]
[0211] After testing, the dry film of the slightly acidic polystyrene seed emulsion obtained in step S2 of Example 1-2 and Comparative Example 1 had a gel content of 0 in tetrahydrofuran (THF), indicating that it was not cross-linked and could be completely dissolved in THF.
[0212] According to the test, the dry film of the polystyrene seed emulsion of the slightly acidic styrene butadiene seed emulsion obtained in step S2 of Example 3 has a gel content of 65 wt % in tetrahydrofuran (THF).
[0213] According to the test, the dry film of the polystyrene seed emulsion of the slightly acidic styrene butadiene seed emulsion obtained in step S2 of Example 4 has a gel content of 62 wt % in tetrahydrofuran (THF).
[0214] According to the test, the dry film of the polystyrene seed emulsion of the slightly acidic styrene butadiene seed emulsion obtained in step S2 of comparative example 2 has a gel content of 60 wt % in tetrahydrofuran (THF).
[0215] From the test results of the polystyrene seed emulsion prepared in the formula of Table 1 and each embodiment and comparative example, it is known that, using the process method of the present invention, the ionized monomer is placed in the aqueous monomer for dropwise addition, most of the carboxyl groups in the obtained polymer emulsion can be quickly neutralized, requiring more alkali, while in comparative example 1, ionized methacrylic acid is placed in the monomer mixture, and a large part of the carboxyl groups in the emulsion formed after polymerization are coated with hydrophobic groups and cannot be quickly neutralized. At the same time, the ionized monomer used in Examples 1-2 contains vinylbenzene sulfonate, which can make the obtained polymer emulsion more stable and produce less slag.
[0216] The components of the raw materials used in the steps S1-S2 for preparing the slightly acidic seed emulsion in the methods of Examples 3-4 and Comparative Example 2 were statistically analyzed, and the statistical results are shown in Table 2.
[0217] Table 2
[0218]
[0219] As can be seen from the test results of the styrene-butadiene seed emulsion in the formulation process and the embodiment of Table 2, the styrene-butadiene seed emulsion prepared by the process and formulation of the present invention has suitable acidity, and has little residue, stable particle size, and most of the carboxyl groups are on the surface of the colloid particles, which are easy to be quickly neutralized. However, the emulsion prepared in Comparative Example 2 is too acidic (the pH value reaches 1, and the reason for the excessive acidity is that the persulfate is decomposed into acidic sulfonic acid groups without weakly alkaline sodium carbonate to neutralize), is easy to corrode metals under high temperature and high pressure, and the amount of residue produced is too much, and a large part of the carboxyl groups are coated by hydrophobic groups, which cannot be quickly neutralized, resulting in the polymer ionicity being not strong.
[0220] The components of the raw materials used in the binder prepared in steps S3-S4 in the methods of Examples 1-2 and Comparative Example 3 were statistically analyzed, and the statistical results are shown in Table 3.
[0221] Table 3
[0222]
[0223]
[0224] The components of the raw materials used in the binder prepared in steps S3-S4 in the method of Example 2-3 were statistically analyzed, and the statistical results are shown in Table 4.
[0225] Table 4
[0226]
[0227]
[0228] It can be seen from the formulation process and actual test results that the styrene butadiene emulsion prepared by the present invention using polystyrene emulsion or styrene butadiene emulsion as seeds has a certain acidity from the carboxyl group before neutralization, will not corrode metals during the reaction, produces less slag, and most of the hydrophilic carboxyl groups are distributed on the surface of the latex particles and can be quickly neutralized by alkali to form ions.
[0229] Performance Test:
[0230] The gel content of the slightly acidic seed emulsion obtained in step S2 of Examples 1-4 and Comparative Examples 1-3 was tested. The test method was as follows: 15 g of the emulsion was poured on a round flat surface dish with a diameter of 10 cm, and then placed in a blast drying oven at 40°C and a relative humidity of 40% for 48 hours. The dry film was taken out and cut into 1 cm*1 cm square films. About 1 g (recorded as m 0 ), put it into a 500 ml flat bottom glass bottle with 300 g dry tetrahydrofuran solvent, seal it, leave it for 24 hours, filter it, dry the residue at room temperature for 24 hours, put it into a blast drying oven at 40°C and a relative humidity of 40% for 24 hours, weigh it accurately, and record it as m 1 , calculate the gel content according to the following formula:
[0231] Gel content (wt%); (m 0 -m 1 )x 100 / m0.
[0232] The performance of the adhesives obtained in Examples 1-4 and Comparative Example 3 was tested. The test results are shown in Table 5.
[0233] Table 5
[0234]
[0235]
[0236] Table 5 shows that the emulsion prepared by copolymerization of butadiene, styrene, vinylbenzene sulfonate, specific unsaturated carboxylic acid, difunctional acrylate and other monomers by suitable process through polystyrene seed emulsion method or styrene butadiene seed emulsion method has certain acidity (pH value is between 2 and 3, which is more serious than pH 1 of Comparative Example 3) before neutralization, but it will not corrode metals during the reaction, and the amount of slag is small (while the slag in Comparative Example 3 is much), and most of the hydrophilic carboxyl groups are distributed on the surface of latex particles, which can be quickly neutralized by alkali to form ions. After neutralization, the emulsion particle size is small, the average particle size is within 200nm, the dispersibility is good and stable, most of the carboxyl groups are converted into ionic -COOM, and the neutralization degree is more than 90% of the theoretical amount, and it also contains phenyl sulfonate of side chain, which has strong ionicity.
[0237] The present invention uses a proper amount of difunctional acrylate, so that the polymer emulsion dry film has moderate crosslinking, the dry film gel content is above 90wt%, has good skeleton stability, and is not easily damaged by the impact of organic electrolyte.
[0238] In addition, the glass transition temperature of the emulsion of the present invention when dried to form a film is in the range of -10°C to 20°C, and it is easy to construct and shape at room temperature or slightly lower temperature, and has a wide range of applications.
[0239] The above are only embodiments of the present invention, and are not intended to limit the patent scope of the present invention. Any equivalent transformations made using the contents of the present invention specification, or directly or indirectly applied in related technical fields, are also included in the patent protection scope of the present invention.
Claims
1. A binder, characterized in that: The binder contains repeating units produced by copolymerization of unsaturated olefins, sulfonate ionic repeating units such as formula (1), carboxylate ionic repeating units such as formula (2), and difunctional acrylate micro-crosslinking units such as formula (3); Wherein, the structural formula of formula (1) is: Wherein, the structural formula of formula (2) is at least one of (2)-a, (2)-b and (2)-c: Wherein, the structural formula of formula (3) is: Wherein, M1 is one of Li, Na and K; Wherein, M2, M3, M4, M5 and M6 are independently selected from one of Li, Na, K and H, and not all of them are selected from H; Wherein, R is one of C2-C8 alkyl, ethylene oxide, propylene oxide, polyoxyethylene and polyoxypropylene; Wherein, R1 is CH3 or H.
2. The adhesive according to claim 1, characterized in that: The repeating units produced by copolymerization of unsaturated olefins include structures represented by formula (4), formula (5), formula (6) and formula (7); Wherein, formula (4) is: Wherein, the structural formula of formula (5) is one of (5)-a, (5)-b and (5)-c: Wherein, the structural formula of formula (6) is one of (6)-a, (6)-b and (6)-c: Wherein, formula (7) is:
3. The adhesive according to claim 1, characterized in that: The mass ratio of the sulfonate ionic repeating unit of formula (1) to the difunctional acrylate micro-crosslinking unit of formula (3) is 3-13:0.2-1.
4. A method for preparing a binder according to any one of claims 1 to 3, characterized in that: The following steps are involved: S1 mixes styrene, additive 1 and water, and pre-emulsifies to obtain a monomer pre-emulsion; S2. Mix the monomer pre-emulsion, initiator, water and additive 2 in a high pressure or normal pressure reaction device, and heat and react to obtain a slightly acidic seed emulsion; S3: mixing the slightly acidic seed emulsion, additive 3, initiator and water in a high pressure reaction device, and heating and reacting to obtain a slightly acidic emulsion; S4 adjusts the pH value of the slightly acidic emulsion to alkaline, and obtains the binder by heating and reducing pressure.
5. The method according to claim 4, characterized in that: The additive 1 includes at least one of an emulsifier and a polymerizable monomer, and at least includes an emulsifier.
6. The method according to claim 4, characterized in that: The additive 2 includes at least one of bicarbonate, ionization functional monomer, butadiene-containing and mercaptan chain transfer agent, and at least includes bicarbonate and ionization functional monomer.
7. The method according to claim 4, characterized in that: The additive 3 includes an emulsifier, butadiene, styrene, a difunctional acrylate and an ionization functional monomer.
8. The method according to claim 5 or 7, characterized in that: The polymerizable monomer includes at least one of acrylate, methacrylate, maleic acid diester, itaconate diester and unsaturated olefin nitrile.
9. The method according to claim 6 or 7, characterized in that: The ionizing functional monomers include unsaturated carboxylic acids and vinylbenzene sulfonates.
10. A negative electrode for a lithium battery, characterized in that: The invention comprises a binder as claimed in any one of claims 1 to 3.
Citation Information
Patent Citations
Tackifiers for composite articles
CN103118866A
Aqueous binder for lithium ion battery as well as preparation method and application thereof
CN105131875A
Carboxylic butadiene-styrene latex as well as preparation method and application thereof
CN115894798A
Carboxylic butadiene-styrene latex and preparation method thereof
CN116970110A
Styrene-Butadiene-Based Binders and Methods of Preparing and Using Same
US20110214796A1