Lithium-rich manganese oxide positive electrode material with non-metered Ni / Co / Mn content and preparation method and application of lithium-rich manganese oxide positive electrode material
By adjusting the Ni/Co/Mn content and using one-step spray drying method, the problem of poor circulation stability of lithium-rich manganese positive electrode materials is solved, and the battery performance improvement is achieved with high specific capacity and low cost, which is suitable for large-scale production.
Patent Information
- Application Number
- CN202411085814.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-08
AI Technical Summary
The existing lithium-rich manganese positive electrode materials have poor cycle stability, severe capacity and voltage attenuation, and the processing process of introducing additional doped elements or cladding layers in the modification method is complicated, making it difficult to apply on a large scale commercial basis.
By adjusting the Ni/Co/Mn content, a lithium-rich manganese oxide positive electrode material of Li1.2Ni0.132+xCo0.172+yMn0.492+zO2 is prepared to increase the Ni content or reduce the Co and Mn content, and suppress the attenuation of voltage and capacity. , improve the rate performance of the material, adopt a one-step spray drying method combined with citric acid monohydrate preparation method to simplify the process and reduce costs.
It has achieved a high specific capacity and low cost lithium-rich manganese positive electrode material, with significantly improved voltage and capacity retention, low material cost and simple process, suitable for large-scale industrial production.
Smart Images

Figure CN118970035A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of battery technology, and in particular to a lithium-rich manganese oxide positive electrode material with non-quantitative control of Ni / Co / Mn content, and a preparation method and application thereof. Background Art
[0002] In the existing energy storage battery system, lithium-ion batteries have been widely used in mobile phones, digital cameras, power tools, laptops and other fields due to their advantages such as high energy density, long cycle life, low self-discharge, no memory effect, wide operating temperature range and environmental friendliness, and are gradually expanding to new energy vehicles and energy storage fields.
[0003] Lithium-rich manganese oxide cathode materials are favored by researchers due to their high discharge capacity (>250mAh / g), high average voltage (~3.6V), abundant manganese resources, and low cost, and have become the preferred cathode material for the next generation of lithium-ion batteries. However, lithium-rich manganese-based cathode materials still face the problems of poor cycle stability and severe capacity and voltage attenuation, which seriously affects the commercialization process of lithium-rich manganese oxide cathode materials.
[0004] Element doping and surface coating are currently commonly used modification methods for the cycle stability of lithium-rich manganese positive electrode materials. In the patent specification with publication number CN117317192A, the inventor disclosed a method for preparing La-doped lithium-rich manganese-based positive electrode materials, which slowed down the generation of oxygen vacancies through strong La-O bonds and blocked the migration path of transition metal ions, thereby enhancing the cycle and voltage stability of lithium-rich manganese-based positive electrode materials. In the patent specification with publication number CN117878308A, the inventor disclosed the introduction of a polyurethane material with a strong ligand on the surface of the main material of the lithium-rich manganese-based positive electrode material. During the charge and discharge cycle, the polyurethane material can establish a bond with the oxygen framework on the surface of the main material, thereby stabilizing the lattice oxygen of the main material, inhibiting the irreversible oxygen release during the charge and discharge cycle, and greatly improving the cycle stability of the lithium-rich manganese-based positive electrode material. However, the above schemes all introduce additional doping elements or coating layers, and have the defects of complex processing technology and difficulty in large-scale commercial application, which need to be improved. Summary of the invention
[0005] In order to solve the above technical problems, the purpose of the present invention is to provide a lithium-rich manganese oxide positive electrode material with non-quantitative control of Ni / Co / Mn content and a preparation method and application thereof, so as to solve the problems of introducing additional doping elements or coating layers and complex processing technology in the existing lithium-rich manganese positive electrode material modification method.
[0006] The technical solution of the present invention to solve the above technical problems is as follows:
[0007] A lithium-rich manganese oxide positive electrode material with non-stoichiometric control of Ni / Co / Mn content, the chemical formula of which is Li 1.2 Ni 0.132+x Co 0.172+y Mn 0.492+z O2, where x = 0 ~ ± 0.1, y = 0 ~ ± 0.1, z = 0 ~ ± 0.1.
[0008] The beneficial effects of the present invention are as follows: the present invention provides a lithium-rich manganese-based positive electrode material with high specific capacity, which can effectively reduce the attenuation of voltage and capacity, has low material cost, is not doped with any other elements, and can inhibit the attenuation of voltage and capacity and improve the rate performance of the material by simply increasing the Ni content or reducing the Co and Mn content. In addition, by increasing the Ni content, Ni and Mn are partially reduced, activating the electrochemical activity of more transition metals, providing more capacity, and significantly increasing the median voltage to 3.72V.
[0009] Furthermore, its chemical formula is Li 1.2 Ni 0.132+x Co 0.172+y Mn 0.492+z O2, wherein x=0, ±0.04 or ±0.1; y=0, ±0.04 or ±0.1; z=0, ±0.06 or ±0.1.
[0010] The method for preparing the above-mentioned lithium-rich manganese oxide positive electrode material with non-quantitative control of Ni / Co / Mn content comprises the following steps:
[0011] (1) Preparation of precursor solution
[0012] Lithium acetate dihydrate, nickel acetate tetrahydrate, cobalt acetate tetrahydrate, manganese acetate tetrahydrate and citric acid monohydrate are mixed and added into water, and stirred to obtain a product;
[0013] (2) Preparation of precursor materials
[0014] The precursor solution obtained in step (1) is spray-dried to obtain;
[0015] (3) Preparation of positive electrode materials
[0016] The precursor material obtained in step (2) is heat treated to obtain the product.
[0017] The beneficial effects of the present invention are as follows: the preparation process of the present invention is simple, environmentally friendly, and has mild preparation conditions, which is conducive to large-scale industrial production and application.
[0018] Furthermore, in step (1), the stoichiometric ratio of lithium acetate dihydrate, nickel acetate tetrahydrate, cobalt acetate tetrahydrate and manganese acetate tetrahydrate is 1.2: (0.032-0.232): (0.072-0.272): (0.392-0.592), and 3% by mass of lithium acetate dihydrate is additionally added to compensate for the lithium loss during the heat treatment process.
[0019] Furthermore, in the precursor solution of step (1), the total concentration of metal acetate is 0.1-0.2 mol / L, and the concentration of citric acid monohydrate is 0.2-0.5 mol / L.
[0020] Furthermore, in step (1), the stirring speed is 300-1000 rpm, the time is 0.5-2 h, and the temperature is 20-30°C.
[0021] Furthermore, in step (2), the inlet temperature of the spray drying is 200-250°C, the outlet temperature is 80-120°C, and the feed rate is 0.5-2L / h.
[0022] The beneficial effect of adopting the above further technical scheme is as follows: the present invention adopts a one-step spray drying method in combination with the use of monohydrated citric acid to atomize the feed liquid through an atomizer to obtain fine droplets, and by controlling the inlet and outlet temperature and pressure of the spray dryer, more than 90 to 95% of the water is rapidly evaporated in an instant during the contact between the small droplets and the hot air, so that the metal acetate and the Li ions react quickly and evenly, thereby improving the preparation efficiency, improving the dispersibility, and further improving the electrochemical performance of the obtained electrode material.
[0023] Furthermore, the heat treatment conditions in step (3) are: in an air atmosphere, heating to 900-1100° C. at a heating rate of 1-5° C. / min, and keeping the temperature for 10-30 min.
[0024] The application of the above-mentioned lithium-rich manganese oxide positive electrode material with non-stoichiometric control of Ni / Co / Mn content in the preparation of lithium-ion batteries.
[0025] The present invention has the following beneficial effects:
[0026] (1) No additional doping elements or coating layers are required. Simply increasing the Ni content or reducing the Co and Mn content inhibits cation mixing, improves structural stability, and thus inhibits voltage and capacity attenuation. At the same time, increasing the Ni content or reducing the Co and Mn content expands the interlayer spacing of the (003) crystal plane and improves the rate performance of the material. In addition, the increase in Ni content causes Ni and Mn to be partially reduced, activating more transition metal electrochemical activity, providing more capacity, and at the same time significantly increasing the median voltage from 3.25V to 3.72V.
[0027] (2) In the lithium-rich manganese-based positive electrode material prepared by the present invention, a one-step spray drying method is used in combination with the use of monohydrated citric acid to atomize the feed liquid through an atomizer to obtain fine droplets. By controlling the inlet and outlet temperature and pressure of the spray dryer, more than 90% to 95% of the water can be rapidly evaporated in an instant during the contact process between the small droplets and the hot air, so that the metal acetate and the lithium salt react evenly and form a lithium-rich manganese precursor material powder with good dispersibility.
[0028] (3) The preparation method of the lithium-rich manganese-based positive electrode material provided by the present invention has a simple synthesis process. The lithium-rich manganese-based positive electrode material with excellent electrochemical performance can be obtained simply by adjusting the content of Ni, Co, and Mn in the material chemical formula, and no other elements are added. It has low cost, is environmentally friendly, and is conducive to large-scale production and application.
[0029] (4) The lithium-rich manganese oxide positive electrode material Li 1.2 Ni 0.132+x Co 0.172 Mn 0.492 O2 (x = -0.1 ~ 0.1), the median voltage increased from 3.25V to 3.72V, when x = 0.1, the capacity retention rate of the lithium-rich manganese oxide positive electrode material was as high as 71.90% and the voltage retention rate was as high as 88.17% after 200 cycles at a current density of 200mA / g. 1.2 Ni 0.132 Co 0.172+y Mn 0.492 The lithium-ion battery assembled with the best component sample (y=-0.1) prepared by O2 has a capacity retention rate of up to 86.78% and a voltage retention rate of up to 82.99% after 500 cycles at a current density of 200 mA / g. 1.2 Ni 0.132 Co 0.172 Mn 0.492+z The lithium-ion battery assembled with the best component sample (z=-0.6) prepared by O2 has a capacity retention rate of up to 66.93% and a voltage retention rate of up to 75.79% after 350 cycles at a current density of 1000mA / g. The lithium-rich manganese oxide positive electrode material obtained by regulating the Ni / Co / Mn components in the present invention has electrochemical properties that are superior to most lithium-rich manganese-based positive electrode materials, thereby improving the performance and effect of lithium-ion batteries. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 This is a SEM image of the lithium-rich manganese oxide positive electrode material obtained in Example 1-13 in Experimental Example 1;
[0031] Figure 2 XRD diagram of the lithium-rich manganese oxide positive electrode materials obtained in Examples 1-4 and Example 13 in Experimental Example 2;
[0032] Figure 3 XRD diagram of the lithium-rich manganese oxide positive electrode materials obtained in Examples 5-8 and Example 13 in Experimental Example 2;
[0033] Figure 4 XRD diagram of the lithium-rich manganese oxide positive electrode material obtained in Examples 9-13 in Experimental Example 2;
[0034] Figure 5 TEM images of lithium-rich manganese oxide positive electrode materials obtained in Examples 1, 4 and 13 in Experimental Example 3;
[0035] Figure 6 The XPS O 1s graph of the lithium-rich manganese oxide positive electrode material obtained in Examples 1-4 and Example 13 in Experimental Example 4;
[0036] Figure 7 XPS Ni 2p diagram of the lithium-rich manganese oxide positive electrode materials obtained in Examples 1-4 and Example 13 in Experimental Example 4;
[0037] Figure 8 The XPS Mn 3s diagram of the lithium-rich manganese oxide positive electrode material obtained in Examples 1-4 and Example 13 in Experimental Example 4;
[0038] Fig. 9 The first charge and discharge curves of the lithium-rich manganese oxide positive electrode materials obtained in Examples 1-4 and Example 13 in Experimental Example 5;
[0039] Fig.10 The first charge and discharge curves of the lithium-rich manganese oxide positive electrode materials obtained in Examples 5-8 and Example 13 in Experimental Example 5;
[0040] Fig.11 This is the first charge and discharge curve of the lithium-rich manganese oxide positive electrode material obtained in Examples 9-13 in Experimental Example 5;
[0041] Fig.12 The median voltage decay diagram of the lithium-rich manganese oxide positive electrode material obtained in Example 1-13 in Experimental Example 5;
[0042] Fig.13 The cycle stability diagram of the lithium-rich manganese oxide positive electrode material obtained in Example 1-13 in Experimental Example 5;
[0043] Fig.14 This is a rate performance diagram of the lithium-rich manganese oxide positive electrode material obtained in Example 1-13 in Experimental Example 5. DETAILED DESCRIPTION
[0044] The principles and features of the present invention are described below in conjunction with the accompanying drawings. The examples are only used to explain the present invention and are not used to limit the scope of the present invention. If specific conditions are not specified in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0045] Embodiment 1:
[0046] A lithium-rich manganese oxide positive electrode material with non-stoichiometric control of Ni / Co / Mn content, the chemical formula of which is: Li 1.2 Ni 0.232 Co 0.172 Mn 0.492 O2.
[0047] The preparation method comprises the following steps:
[0048] (1) Preparation of precursor solution
[0049] 18.914 g of lithium acetate dihydrate, 8.660 g of nickel acetate tetrahydrate, 6.426 g of cobalt acetate tetrahydrate and 18.088 g of manganese acetate tetrahydrate were weighed and dissolved in 1 L of deionized water, and 63.042 g of citric acid monohydrate was added, and 3% by mass of lithium acetate dihydrate was additionally added to compensate for the lithium loss during the heat treatment; the mixture was mechanically stirred at 500 rpm for 1 h at room temperature to obtain a precursor solution.
[0050] (2) Preparation of precursor materials
[0051] The precursor solution obtained in step (1) is sent to a spray dryer by a peristaltic pump. The inlet temperature of the spray dryer is set to 230°C, the outlet temperature is set to 100°C, and the feed rate is set to 1L / h. The precursor material is obtained by spray drying under high temperature and high pressure.
[0052] (3) Preparation of positive electrode materials
[0053] The precursor material obtained in step (2) is placed in an alumina crucible, wherein the alumina crucible has a length of 120 mm, a width of 120 mm, and a height of 50 mm. The alumina crucible is placed in a box furnace, heated at a heating rate of 3°C / min in an air atmosphere, and heat treated at 1000°C for 20 min to obtain Li 1.2 Ni 0.232 Co 0.172 Mn 0.492 O2 positive electrode material, named Ni232.
[0054] Embodiment 2:
[0055] A lithium-rich manganese oxide positive electrode material with non-stoichiometric control of Ni / Co / Mn content, the chemical formula of which is: Li1.2 Ni 0.172 Co 0.172 Mn 0.492 O2.
[0056] The preparation method is the same as that in Example 1, except that, when preparing the precursor solution, 18.914 g of lithium acetate dihydrate, 6.420 g of nickel acetate tetrahydrate, 6.426 g of cobalt acetate tetrahydrate and 18.088 g of manganese acetate tetrahydrate are weighed and dissolved in 1 L of deionized water, and 63.042 g of citric acid monohydrate is added, and 3% by mass of lithium acetate dihydrate is additionally added to compensate for the lithium loss during the heat treatment process; the precursor solution is obtained by mechanical stirring at 500 rpm at room temperature for 1 hour, and the remaining steps are the same as those in Example 1. The obtained positive electrode material is named Ni172.
[0057] Embodiment 3:
[0058] A lithium-rich manganese oxide positive electrode material with non-stoichiometric control of Ni / Co / Mn content, the chemical formula of which is: Li 1.2 Ni 0.092 Co 0.172 Mn 0.492 O2.
[0059] The preparation method is the same as that in Example 1, except that, when the precursor solution is prepared, 18.914 g of lithium acetate dihydrate, 3.434 g of nickel acetate tetrahydrate, 6.426 g of cobalt acetate tetrahydrate and 18.088 g of manganese acetate tetrahydrate are weighed and dissolved in 1 L of deionized water, and 63.042 g of citric acid monohydrate is added, and 3% by mass of lithium acetate dihydrate is additionally added to compensate for the lithium loss during the heat treatment process; the precursor solution is obtained by mechanical stirring at 500 rpm at room temperature for 1 hour, and the remaining steps are the same as those in Example 1. The obtained positive electrode material is named Ni092.
[0060] Embodiment 4:
[0061] A lithium-rich manganese oxide positive electrode material with non-stoichiometric control of Ni / Co / Mn content, the chemical formula of which is: Li 1.2 Ni 0.032 Co 0.172 Mn 0.492 O2.
[0062] The preparation method is the same as that in Example 1, except that, when the precursor solution is prepared, 18.914 g of lithium acetate dihydrate, 1.194 g of nickel acetate tetrahydrate, 6.426 g of cobalt acetate tetrahydrate and 18.088 g of manganese acetate tetrahydrate are weighed and dissolved in 1 L of deionized water, and 63.042 g of citric acid monohydrate is added, and 3% of lithium acetate dihydrate is additionally added by mass to compensate for the lithium loss during the heat treatment process; the precursor solution is obtained by mechanical stirring at 500 rpm at room temperature for 1 hour, and the remaining steps are the same as those in Example 1. The obtained positive electrode material is named Ni032.
[0063] Embodiment 5:
[0064] A lithium-rich manganese oxide positive electrode material with non-stoichiometric control of Ni / Co / Mn content, the chemical formula of which is: Li 1.2 Ni 0.132 Co 0.272 Mn 0.492 O2.
[0065] The preparation method is the same as that in Example 1, except that, when preparing the precursor solution, 18.914 g of lithium acetate dihydrate, 4.927 g of nickel acetate tetrahydrate, 10.162 g of cobalt acetate tetrahydrate and 18.088 g of manganese acetate tetrahydrate are weighed and dissolved in 1 L of deionized water, and 63.042 g of citric acid monohydrate is added, and 3% by mass of lithium acetate dihydrate is additionally added to compensate for the lithium loss during the heat treatment process; the precursor solution is obtained by mechanical stirring at 500 rpm at room temperature for 1 hour, and the remaining steps are the same as those in Example 1. The obtained positive electrode material is named Co272.
[0066] Embodiment 6:
[0067] A lithium-rich manganese oxide positive electrode material with non-stoichiometric control of Ni / Co / Mn content, the chemical formula of which is: Li 1.2 Ni 0.132 Co 0.212 Mn 0.492 O2.
[0068] The preparation method is the same as that in Example 1, except that, when the precursor solution is prepared, 18.914 g of lithium acetate dihydrate, 4.927 g of nickel acetate tetrahydrate, 7.920 g of cobalt acetate tetrahydrate and 18.088 g of manganese acetate tetrahydrate are weighed and dissolved in 1 L of deionized water, and 63.042 g of citric acid monohydrate is added, and 3% of lithium acetate dihydrate is additionally added by mass to compensate for the lithium loss during the heat treatment process; the precursor solution is obtained by mechanical stirring at 500 rpm at room temperature for 1 hour, and the remaining steps are the same as those in Example 1. The obtained positive electrode material is named Co212.
[0069] Embodiment 7:
[0070] A lithium-rich manganese oxide positive electrode material with non-stoichiometric control of Ni / Co / Mn content, the chemical formula of which is: Li 1.2 Ni 0.132 Co 0.132 Mn 0.492 O2.
[0071] The preparation method is the same as that in Example 1, except that, when preparing the precursor solution, 18.914 g of lithium acetate dihydrate, 4.927 g of nickel acetate tetrahydrate, 4.932 g of cobalt acetate tetrahydrate and 18.088 g of manganese acetate tetrahydrate are weighed and dissolved in 1 L of deionized water, and 63.042 g of citric acid monohydrate is added, and 3% by mass of lithium acetate dihydrate is additionally added to compensate for the lithium loss during the heat treatment process; the precursor solution is obtained by mechanical stirring at 500 rpm at room temperature for 1 hour, and the remaining steps are the same as those in Example 1. The obtained positive electrode material is named Co132.
[0072] Embodiment 8:
[0073] A lithium-rich manganese oxide positive electrode material with non-stoichiometric control of Ni / Co / Mn content, the chemical formula of which is: Li 1.2 Ni 0.132 Co 0.072 Mn 0.492 O2.
[0074] The preparation method is the same as that in Example 1, except that, when the precursor solution is prepared, 18.914 g of lithium acetate dihydrate, 4.927 g of nickel acetate tetrahydrate, 2.69 g of cobalt acetate tetrahydrate and 18.088 g of manganese acetate tetrahydrate are weighed and dissolved in 1 L of deionized water, and 63.042 g of citric acid monohydrate is added, and 3% by mass of lithium acetate dihydrate is additionally added to compensate for the lithium loss during the heat treatment process; the precursor solution is obtained by mechanical stirring at 500 rpm at room temperature for 1 hour, and the remaining steps are the same as those in Example 1. The obtained positive electrode material is named Co072.
[0075] Embodiment 9:
[0076] A lithium-rich manganese oxide positive electrode material with non-stoichiometric control of Ni / Co / Mn content, the chemical formula of which is: Li 1.2 Ni 0.132 Co 0.172 Mn 0.592 O2.
[0077] The preparation method is the same as that in Example 1, except that, when preparing the precursor solution, 18.914 g of lithium acetate dihydrate, 4.927 g of nickel acetate tetrahydrate, 6.426 g of cobalt acetate tetrahydrate and 21.764 g of manganese acetate tetrahydrate are weighed and dissolved in 1 L of deionized water, and 63.042 g of citric acid monohydrate is added, and 3% by mass of lithium acetate dihydrate is additionally added to compensate for the lithium loss during the heat treatment process; the precursor solution is obtained by mechanical stirring at 500 rpm at room temperature for 1 hour, and the remaining steps are the same as those in Example 1. The obtained positive electrode material is named Mn592.
[0078] Embodiment 10:
[0079] A lithium-rich manganese oxide positive electrode material with non-stoichiometric control of Ni / Co / Mn content, the chemical formula of which is: Li 1.2 Ni 0.132 Co 0.172 Mn 0.552 O2.
[0080] The preparation method is the same as that in Example 1, except that, when preparing the precursor solution, 18.914 g of lithium acetate dihydrate, 4.927 g of nickel acetate tetrahydrate, 6.426 g of cobalt acetate tetrahydrate and 20.293 g of manganese acetate tetrahydrate are weighed and dissolved in 1 L of deionized water, and 63.042 g of citric acid monohydrate is added, and 3% by mass of lithium acetate dihydrate is additionally added to compensate for the lithium loss during the heat treatment process; the precursor solution is obtained by mechanical stirring at 500 rpm at room temperature for 1 hour, and the remaining steps are the same as those in Example 1. The obtained positive electrode material is named Mn552.
[0081] Embodiment 11:
[0082] A lithium-rich manganese oxide positive electrode material with non-stoichiometric control of Ni / Co / Mn content, the chemical formula of which is: Li 1.2 Ni 0.132 Co 0.172 Mn 0.432 O2.
[0083] The preparation method is the same as that in Example 1, except that, when preparing the precursor solution, 18.914 g of lithium acetate dihydrate, 4.927 g of nickel acetate tetrahydrate, 6.426 g of cobalt acetate tetrahydrate and 15.882 g of manganese acetate tetrahydrate are weighed and dissolved in 1 L of deionized water, and 63.042 g of citric acid monohydrate is added, and 3% by mass of lithium acetate dihydrate is additionally added to compensate for the lithium loss during the heat treatment process; the precursor solution is obtained by mechanical stirring at 500 rpm at room temperature for 1 hour, and the remaining steps are the same as those in Example 1. The obtained positive electrode material is named Mn432.
[0084] Embodiment 12:
[0085] A lithium-rich manganese oxide positive electrode material with non-stoichiometric control of Ni / Co / Mn content, the chemical formula of which is: Li 1.2 Ni 0.132 Co 0.172 Mn 0.392 O2.
[0086] The preparation method is the same as that in Example 1, except that, when the precursor solution is prepared, 18.914 g of lithium acetate dihydrate, 4.927 g of nickel acetate tetrahydrate, 6.426 g of cobalt acetate tetrahydrate and 14.411 g of manganese acetate tetrahydrate are weighed and dissolved in 1 L of deionized water, and 63.042 g of citric acid monohydrate is added, and 3% by mass of lithium acetate dihydrate is additionally added to compensate for the lithium loss during the heat treatment process; the precursor solution is obtained by mechanical stirring at 500 rpm at room temperature for 1 hour, and the remaining steps are the same as those in Example 1. The obtained positive electrode material is named Mn392.
[0087] Embodiment 13:
[0088] A lithium-rich manganese oxide positive electrode material with non-stoichiometric control of Ni / Co / Mn content, the chemical formula of which is: Li 1.2 Ni 0.132 Co 0.172 Mn 0.492 O2.
[0089] The preparation method is the same as that in Example 1, except that, when the precursor solution is prepared, 18.914 g of lithium acetate dihydrate, 4.927 g of nickel acetate tetrahydrate, 6.426 g of cobalt acetate tetrahydrate and 18.088 g of manganese acetate tetrahydrate are weighed and dissolved in 1 L of deionized water, and 63.042 g of citric acid monohydrate is added, and 3% of lithium acetate dihydrate is additionally added by mass to compensate for the lithium loss during the heat treatment process; the precursor solution is obtained by mechanical stirring at 500 rpm at room temperature for 1 hour, and the remaining steps are the same as those in Example 1. The obtained positive electrode material is named Ni132 or Co172 or Mn492.
[0090] Test example 1: SEM test
[0091] The lithium-rich manganese-based positive electrode materials prepared in Examples 1-13 were subjected to SEM testing to observe the morphology and size of the lithium-rich manganese-based positive electrode materials.
[0092] The experimental results are as follows Figure 1 As shown, it can be seen that the lithium-rich manganese-based positive electrode materials prepared in the embodiments of the present invention are all spherical in shape, with a smooth surface and a size of about 400-700 nm.
[0093] Test Example 2: XRD test
[0094] XRD test was performed on the lithium-rich manganese-based positive electrode materials prepared in Examples 1-13 to test the average structure of the lithium-rich manganese-based positive electrode materials.
[0095] The experimental results are as follows Figure 2-Figure 4 As shown. It can be seen that increasing the Ni content or reducing the Co and Mn contents increases I(003) / I(104) and reduces the cation mixing. In addition, reducing the Ni content or reducing the Co and Mn content causes the spinel phase to appear in the lithium-rich manganese-based positive electrode material.
[0096] Test Example 3: TEM test
[0097] The lithium-rich manganese-based positive electrode materials prepared in Examples 1, 4 and 13 were subjected to TEM testing to test the local structure of the lithium-rich manganese-based positive electrode materials.
[0098] The experimental results are as follows Figure 5 It can be seen that as the Ni content of the lithium-rich manganese-based positive electrode material prepared in the embodiment of the present invention increases, the (003) crystal plane spacing increases continuously, which can improve the Li + Deintercalation kinetics during charge and discharge.
[0099] Test Example 4: XPS Test
[0100] The lithium-rich manganese-based positive electrode materials prepared in Examples 1-4 and Example 13 were subjected to TEM test to test the valence states of the elements in the lithium-rich manganese-based positive electrode materials.
[0101] The experimental results are as follows Figure 6-Figure 8 It can be seen that as the Ni content of the lithium-rich manganese-based positive electrode material provided in this embodiment increases, the oxygen vacancy content gradually decreases. 2+ The content gradually increases and the Mn valence gradually decreases.
[0102] Test Example 5: Electrochemical Performance Test
[0103] (1) Preparation of positive electrode sheet
[0104] The lithium-rich manganese-based positive electrode material and Super P prepared in Example 1-13 were weighed in a mass ratio of 8:1 and placed in a ball mill, tungsten carbide ball milling beads were added, the ball-to-material mass ratio in the ball mill was 100:1, and alcohol was added as a dispersant. After ball milling for 6 hours, the mixture was dried in a drying oven to obtain a mixture A;
[0105] Weigh 285 mg of mixture A and 1250 mg of 1.2% CMC solution, stir at room temperature for 2 h, ultrasonicate for 2 h, stir again for 2 h, coat on aluminum foil with a 0.1 μm scraper, dry in a vacuum drying oven at 110 ° C for 20 h, cut into electrodes with a diameter of 10 mm, and then transfer the cut electrodes to a vacuum oven at 115 ° C for 10 h for use.
[0106] (2) Assemble CR2025 stainless steel button battery
[0107] Using a metal lithium sheet as the negative electrode, 200 μL of LBC-3045I(G) commercial electrolyte was dripped into it, and the CR2025 stainless steel button battery was assembled in a glove box filled with argon gas and with a moisture content of less than 0.01 ppm. After standing at 45°C for 40 hours, its charge and discharge performance was tested.
[0108] CR2025 stainless steel button battery electrochemical performance test:
[0109] The cycle performance of the batteries prepared in Examples 1-13 was tested by constant current charge and discharge. The test temperature was 25°C, the voltage window was 2.0-4.8V, and the current densities tested were 0.1C, 0.2C, 0.5C, 1C, 2C, 5C and 10C, respectively, where 1C = 200mA / g.
[0110] like Figure 9-11 As shown in FIG. 1 , as the Ni content increases, the specific capacity contributed by the transition metal cations gradually increases, which is mainly because the increase in the Ni content causes the transition metal cations Mn and Ni to be partially reduced. 1.2 Ni 0.112 Co 0.172 Mn 0.492 The lithium-ion battery prepared by O2 has a maximum first discharge specific capacity of 279.41 mAh / g at a current density of 20 mA / g.
[0111] like Fig.12 and Fig.13 As shown, the lithium-rich manganese oxide positive electrode material Li 1.2 Ni 0.232 Co 0.172 Mn 0.492 After 200 cycles at a current density of 200 mA / g, the capacity retention rate of the lithium-ion battery prepared by O2 is as high as 71.90%, and the voltage retention rate is as high as 88.17%. This is mainly because the increased non-stoichiometric Ni will pre-occupy the Li sites in the Li layer after entering the lattice, and these interlayer Ni atoms coordinate with the adjacent O, thereby improving the stability of the lattice oxygen. 1.2 Ni 0.132 Co 0.072 Mn 0.492 After 500 cycles at a current density of 200 mA / g, the capacity retention rate of the lithium-ion battery prepared by O2 is as high as 86.78%, and the voltage retention rate is as high as 82.99%. 1.2 Ni0.132 Co 0.172 Mn 0.432 After 350 cycles at a current density of 1000mA / g, the capacity retention rate of the lithium-ion battery prepared by O2 was as high as 66.93%, and the voltage retention rate was as high as 75.79%.
[0112] like Fig.14 As shown, the increase in Ni content expands the interlayer spacing of the (003) crystal plane, making the lithium-rich manganese oxide positive electrode material Li 1.2 Ni 0.232 Co 0.172 Mn 0.492 The lithium-ion battery prepared by O2 still provides 81.44mAh / g capacity at a current density of 2000mA / g. 1.2 Ni 0.132 Co 0.072 Mn 0.492 The lithium-ion battery prepared by O2 still provides 103mAh / g capacity at a current density of 2000mA / g. 1.2 Ni 0.132 Co 0.172 Mn 0.432 The lithium-ion battery prepared by O2 still provides a capacity of 90mAh / g at a current density of 2000mA / g.
[0113] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A lithium-rich manganese oxide positive electrode material with non-stoichiometric control of Ni / Co / Mn content, characterized in that: Its chemical formula is Li 1.2 Ni 0.132+x Co 0.172+y Mn 0.492+z O2, where x = 0 ~ ± 0.1, y = 0 ~ ± 0.1, z = 0 ~ ± 0.
1.
2. The lithium-rich manganese oxide positive electrode material with non-stoichiometric control of Ni / Co / Mn content according to claim 1, characterized in that: Its chemical formula is Li 1.2 Ni 0.132+x Co 0.172+y Mn 0.492+z O2, wherein x=0, ±0.04 or ±0.1; y=0, ±0.04 or ±0.1; z=0, ±0.06 or ±0.
1.
3. The method for preparing the lithium-rich manganese oxide positive electrode material with non-stoichiometric control of Ni / Co / Mn content according to claim 1 or 2, characterized in that: The following steps are involved: (1) Preparation of precursor solution Lithium acetate dihydrate, nickel acetate tetrahydrate, cobalt acetate tetrahydrate, manganese acetate tetrahydrate and citric acid monohydrate are mixed and added into water, and stirred to obtain a product; (2) Preparation of precursor materials The precursor solution obtained in step (1) is spray-dried to obtain; (3) Preparation of positive electrode materials The precursor material obtained in step (2) is heat treated to obtain the product.
4. The method for preparing a lithium-rich manganese oxide positive electrode material with non-stoichiometric control of Ni / Co / Mn content according to claim 3, characterized in that: In the step (1), the stoichiometric ratio of lithium acetate dihydrate, nickel acetate tetrahydrate, cobalt acetate tetrahydrate and manganese acetate tetrahydrate is 1.2: (0.032-0.232): (0.072-0.272): (0.392-0.592), and 3% by mass of lithium acetate dihydrate is additionally added to compensate for the lithium loss during the heat treatment process.
5. The method for preparing a lithium-rich manganese oxide positive electrode material with non-stoichiometric control of Ni / Co / Mn content according to claim 3, characterized in that: In the step (1), the total concentration of metal acetate in the precursor solution is 0.1-0.2 mol / L, and the concentration of citric acid monohydrate is 0.2-0.5 mol / L.
6. The method for preparing a lithium-rich manganese oxide positive electrode material with non-stoichiometric control of Ni / Co / Mn content according to claim 3, characterized in that: The stirring speed in step (1) is 300-1000 rpm, the stirring time is 0.5-2 h, and the temperature is 20-30°C.
7. The method for preparing a lithium-rich manganese oxide positive electrode material with non-stoichiometric control of Ni / Co / Mn content according to claim 3, characterized in that: In the step (2), the inlet temperature of the spray drying is 200-250°C, the outlet temperature is 80-120°C, and the feed rate is 0.5-2L / h.
8. The method for preparing a lithium-rich manganese oxide positive electrode material with non-stoichiometric control of Ni / Co / Mn content according to claim 3, characterized in that: The heat treatment conditions in step (3) are: in an air atmosphere, heating to 900-1100° C. at a heating rate of 1-5° C. / min, and keeping the temperature for 10-30 minutes.
9. Use of the lithium-rich manganese oxide positive electrode material with non-stoichiometrically regulated Ni / Co / Mn content according to claim 1 or 2 in the preparation of lithium-ion batteries.
Citation Information
Patent Citations
Preparation method of lanthanum-doped O2 type lithium-rich manganese-based positive electrode material
CN117317192A
Lithium-rich manganese-based positive electrode material, preparation method thereof, positive plate and lithium ion battery
CN117878308A
Lithium-rich manganese oxide positive electrode material and preparation method thereof, positive electrode sheet and lithium ion battery
CN111710858A
Lithium-rich manganese-based positive electrode material with low voltage drop performance as well as preparation method and application of lithium-rich manganese-based positive electrode material
CN114566625A
Lithium-rich manganese-based precursor, positive electrode material, lithium ion battery and preparation method of lithium-rich manganese-based precursor
CN116040699A
Cited By
Lithium-rich manganese oxide positive electrode material with excellent comprehensive performance, preparation method and application
CN120527380A
A high-performance lithium-rich manganese oxide cathode material, its preparation method and application.
CN120527380B