Electrolyte and lithium ion battery
By using the combination of LiTDI and Compound A in the lithium-ion battery electrolyte, the problem of electrolyte decomposition of lithium-ion batteries at high voltage and high temperatures is solved, the electrode stability and conductivity are improved, and the circulation and low temperature performance are improved.
Patent Information
- Application Number
- CN202410991378.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-15
AI Technical Summary
The electrolyte decomposition accelerates at high voltage and high temperatures, resulting in unstable solid electrolyte interface film, reducing cycle life and low-temperature discharge performance.
Using an electrolyte containing lithium 2-trifluoromethyl-4,5-dicyanoimidazole (LiTDI) and specific compound A, which has a chain ether and a cyclic ether structure, which improves the stability and conductivity of the SEI layer, and is synergistically LiTDI forms an inorganic and organic interface containing fluorine, nitrogen and oxygen, promoting the dissociation of LiTDI.
Improve electrode stability at high voltage and high temperatures, form a stable SEI layer, significantly improving the circulation performance and low-temperature discharge performance of lithium-ion batteries.
Smart Images

Figure CN118970175A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of lithium ion batteries, and in particular relates to an electrolyte and a lithium ion battery. Background Art
[0002] Lithium-ion batteries are increasingly used in daily life due to their excellent properties, such as low self-discharge rate, long cycle life, high operating voltage and low pollution, covering mobile phones, notebooks and even the new energy vehicle industry, showing great application potential. At the same time, users also put forward requirements for lithium-ion batteries such as high energy density and fast charging. In the lithium-ion battery system, continuously increasing the battery operating voltage and operating temperature will lead to different degrees of electrolyte decomposition, thereby accelerating the degradation and failure of battery performance.
[0003] During the first charge and discharge process, the electrolyte will partially decompose, thus forming a passivation film on the surface of the electrode material, called the solid electrolyte interface (SEI). Therefore, the chemical composition and structure of the SEI film play a key role in improving the battery's operating voltage, operating temperature, and cycle life. At present, the most economical and convenient way to improve battery performance is to optimize the composition of the SEI film by adding a small amount of additives. 2-Trifluoromethyl-4,5-dicyanoimidazole lithium (LiTDI) has good thermal stability, can improve battery life and fast charging, and has attracted widespread attention from researchers. However, the degree of dissociation of LiTDI in conventional non-aqueous organic solvents is low, which means that the number of lithium ions that can move freely in the electrolyte is small, which not only reduces the conductivity of lithium ions, but also is not conducive to the formation of a stable and dense SEI film. The unstable SEI film increases the interfacial impedance between the electrode and the electrolyte, resulting in a decrease in cycle stability and is not conducive to improving low-temperature discharge performance.
[0004] Therefore, how to provide an electrolyte and a lithium-ion battery with good comprehensive performance is a technical problem that needs to be solved urgently. Summary of the invention
[0005] In view of the above problems, an object of the present invention is to provide an electrolyte and a lithium ion battery, wherein the electrolyte can comprehensively improve the cycle performance and low-temperature discharge performance of the lithium ion battery.
[0006] To achieve the above objectives, the first aspect of the present invention provides an electrolyte, comprising a lithium salt, an organic solvent and an additive, wherein the lithium salt comprises 2-trifluoromethyl-4,5-dicyanoimidazole lithium, and the additive comprises a compound A shown in Formula 1:
[0007]
[0008] Wherein R1-R2 are each independently selected from alkyl, alkenyl, alkynyl or acyl.
[0009] Compared with the prior art, the electrolyte of the present invention includes 2-trifluoromethyl-4,5-dicyanoimidazole lithium (LiTDI). LiTDI is not easy to hydrolyze and can produce a large amount of LiF under high voltage and high temperature, thereby improving the stability of the electrode electrolyte. However, the solubility of LiF in carbonates (such as ethylene carbonate, etc.) is relatively high, which means that the formed LiF is easily redissolved back into the electrolyte instead of being completely retained on the electrode surface to form a continuous and dense SEI layer, which will lead to an insufficient stability of the SEI layer. At the same time, the degree of dissociation of LiTDI in conventional carbonates is relatively low, which also has a significant negative impact on the conductivity of the electrolyte. Based on this, the present invention also introduces compound A shown in formula 1 as an additive. Formula 1 includes two structures, chain ether and cyclic ether, which makes formula 1 have relatively high stability and can maintain the stability of the SEI layer under high temperature and high pressure; at the same time, formula 1 can also cooperate with LiTDI to form an inorganic double interface containing fluorine, nitrogen, and oxygen and an organic double interface containing oxygen, which is not easily dissolved in carbonates, thereby further improving the stability of the SEI layer; in addition, the cyclic ether structure in compound A gives compound A low viscosity and low melting point characteristics, which means that the dissociation process of LiTDI in the electrolyte will be greatly promoted, thereby improving the conductivity of the electrolyte. In summary, the electrolyte of the present invention can improve the electrode stability at high voltage and high temperature by combining LiTDI with compound A shown in formula 1, promote the formation of a stable SEI layer, and significantly improve the conductivity of the electrolyte, thereby comprehensively improving the cycle performance and low-temperature discharge performance of lithium-ion batteries.
[0010] Further, R1-R2 of the present invention are each independently selected from C1-C6 alkyl, C2-C6 alkenyl, C2-C6 alkynyl or C1-C6 acyl. For example, C1-C6 alkyl may be but not limited to at least one of methyl, ethyl, propyl, isopropyl, butyl, sec-butyl, tert-butyl, pentyl and cyclohexyl; C2-C6 alkenyl may be but not limited to at least one of vinyl, propenyl, butenyl, pentenyl and hexenyl, preferably, C2-C6 alkenyl may be vinyl or allyl; C2-C6 alkynyl may be but not limited to at least one of ethynyl, propynyl, butynyl, pentynyl and hexynyl; C1-C6 acyl may be C1-C6 alkanoyl, such as C1-C6 acyl may be but not limited to formyl, acetyl, propionyl, butyryl, etc.
[0011] Furthermore, the group of R1 in the present invention is the same as the group of R2.
[0012] Furthermore, the compound A of the present invention is at least one selected from compounds 1 to 6:
[0013]
[0014] Furthermore, the mass of the additive of the present invention accounts for 0.1-5.0% of the total mass of the electrolyte. Specifically, the mass of the additive may be, but is not limited to, 0.1%, 0.5%, 0.8%, 1.0%, 1.3%, 1.8%, 2.2%, 2.6%, 2.9%, 3.2%, 3.5%, 3.8%, 4.1%, 4.5%, 5.0% of the total mass of the electrolyte.
[0015] Further, the lithium salt of the present invention also includes at least one of lithium hexafluorophosphate (LiPF6), lithium perchlorate (LiClO4), lithium tetrafluoroborate (LiBF4), lithium bis(trifluoromethylsulfonyl imide) (LiFSI), lithium bis(trifluoromethylsulfonyl imide) (LiTFSI), lithium methanesulfonate (LiCH3SO3), lithium trifluoromethylsulfonate (LiCF3SO3), lithium fluorosulfonate (LiSO2F), lithium bis(oxalate borate) (LiBC4O8), lithium difluorooxalate borate (LiBF2C2O4), lithium difluorophosphate (LiPO2F2), lithium difluorobis(oxalate phosphate) (LiDFBP), lithium diphosphate (LiPO2F2), lithium bis(trifluoromethylsulfonyl imide) (LiTFSI) and lower aliphatic lithium carboxylates. Further, lower aliphatic lithium carboxylates include but are not limited to lithium chloroborane, lithium tetraphenylborate, lithium imide salts, etc.
[0016] Further, the mass of the lithium salt of the present invention accounts for 5-25% of the total mass of the electrolyte. Further, the mass of the lithium salt accounts for 6-20% of the total mass of the electrolyte, preferably, the mass of the lithium salt accounts for 8-18% of the total mass of the electrolyte. As an example, the mass of the lithium salt accounts for 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18% of the total mass of the electrolyte, but is not limited to the listed values, and other values not listed in the numerical range are also applicable.
[0017] Furthermore, the organic solvent of the present invention includes at least one of carbonate, carboxylate and ether compounds. Specifically, carbonates include but are not limited to ethylene carbonate (EC), propylene carbonate, butylene carbonate (BC), pentyl carbonate, dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), and propylene carbonate (PC); carboxylates include but are not limited to γ-butyrolactone, γ-valerolactone, δ-valerolactone, methyl acetate (MA), ethyl acetate (EA), propyl acetate (EP), butyl acetate, propyl propionate (PP), and butyl propionate; ether compounds include but are not limited to 1,3-dioxolane (DOL), 1,4-dioxane (DX), crown ethers, tetrahydrofuran (THF), 2-methyltetrahydrofuran (2-CH3-THF), 2-trifluoromethyltetrahydrofuran (2-CF3-THF), dimethoxymethane, diethoxymethane, ethoxymethoxymethane, ethylene glycol di-n-propyl ether, ethylene glycol di-n-butyl ether, and diethylene glycol dimethyl ether.
[0018] Furthermore, the electrolyte of the present invention also includes an auxiliary agent, which is selected from vinylene carbonate (VC), vinylene carbonate, fluoroethylene carbonate (FEC), vinyl sulfite, 1,3-propane sultone (PS), 1,3-propylene sultone, 1,4-butane sultone, vinyl sulfate, succinic anhydride, maleic anhydride, 2-methylmaleic anhydride, methyl carbonate-2-propynyl ester, tetravinylsilane, triallyl isocyanurate, hexamethylene diisocyanate, o-phenanthroline At least one of quinone, p-phenylene diisocyanate, 2,4-toluene diisocyanate, N-phenylbis(trifluoromethanesulfonyl)imide, vinyl bissulfate, phenyl methanesulfonate, vinyl bissulfate, bis-spiro propylene sulfate, hydroquinone difluorosulfonate, triallyl phosphate, tripropargyl phosphate, 2,4-butane sultone, isocyanoethyl methacrylate, methylene disulfonate, tris(trimethylsilyl)borate, tris(trimethylsilyl)phosphate, and tris(vinyldimethylsilyl)phosphate.
[0019] Further, the mass of the auxiliary agent of the present invention accounts for 0.1-5% of the total mass of the electrolyte, specifically, the mass of the auxiliary agent may account for 0.2-2% of the total mass of the electrolyte. As an example, the mass of the auxiliary agent accounts for 0.1%, 0.2%, 0.5%, 0.8%, 1%, 1.5%, 2%, 2.2%, 2.5%, 3%, 3.2%, 3.5%, 3.8%, 4%, 4.2%, 4.5%, 4.8%, 5% of the total mass of the electrolyte, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0020] Correspondingly, the second aspect of the present invention also provides a lithium ion battery, comprising a positive electrode and a negative electrode, and also comprising the above-mentioned electrolyte. The lithium ion battery adopts the above-mentioned electrolyte, and the lithium ion battery has good high temperature cycle performance, room temperature fast charge cycle performance, and also has good low temperature performance, especially at -20°C.
[0021] Furthermore, the active material of the positive electrode of the present invention is selected from lithium cobalt oxide (such as LiCoO2), lithium nickel oxide (such as LiNiO2), lithium manganese oxide (such as LiMnO2, LiMn2O4), lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide structure (such as LiNi x Co y Mn 1-x-y M z O2, wherein 0.6≤x<0.9, x+y<1, 0≤z<0.08, M is at least one of Al, Mg, Zr and Ti), lithium iron phosphate (such as LiFePO4 (also referred to as LFP)), a composite material of lithium iron phosphate and carbon, lithium manganese phosphate (such as LiMnPO4), a composite material of lithium manganese phosphate and carbon, lithium iron manganese phosphate and a composite material of lithium iron manganese phosphate and carbon. In a preferred embodiment, the positive electrode is made of a nickel cobalt manganese oxide material, and the nickel cobalt manganese oxide material is LiNi x Co y Mn 1-x-y M z O2, wherein 0.6≤x<0.9, x+y<1, 0≤z<0.08, M is at least one of Al, Mg, Zr and Ti. As an example, x=0.8, y=0.1, M is Zr, and z=0.03.
[0022] Furthermore, the active material of the negative electrode of the present invention includes at least one of a carbon-based negative electrode, a silicon-based negative electrode, a tin-based negative electrode, and a lithium negative electrode. The carbon-based negative electrode may include graphite, hard carbon, soft carbon, graphene, mesophase carbon microspheres, etc.; the silicon-based negative electrode may include silicon materials, silicon oxides, silicon-carbon composite materials, and silicon alloy materials, etc.; the tin-based negative electrode may include tin, tin carbon, tin oxygen, and tin metal compounds; the lithium negative electrode may include metallic lithium or a lithium alloy. The lithium alloy may specifically be at least one of a lithium silicon alloy, a lithium sodium alloy, a lithium potassium alloy, a lithium aluminum alloy, a lithium tin alloy, and a lithium indium alloy. DETAILED DESCRIPTION
[0023] In order to further illustrate the purpose, technical scheme and beneficial effects of the present invention, the present invention will be further described below in conjunction with specific examples. It should be noted that, if specific conditions are not specified in the examples and comparative examples, they can be carried out according to conventional conditions or conditions recommended by the manufacturer, and if the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be obtained commercially.
[0024] Example 1
[0025] Preparation of electrolyte:
[0026] In a glove box filled with nitrogen (O2 <1ppm, H2O <1ppm), ethylene carbonate (EC), butylene carbonate (BC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) were mixed in a mass ratio of 5:1:1:1 to obtain 87g of a mixed solvent as an organic solvent, and 1g of compound 1 was added to obtain a mixed solution. The mixed solution was sealed and packaged and placed in a quick freezer (-4°C) for 2h and then taken out. In a glove box filled with nitrogen (O2 <1ppm, H2O <1ppm), 8g of 2-trifluoromethyl-4,5-dicyanoimidazole lithium (LiTDI) and 4g of lithium hexafluorophosphate (LiPF6) were slowly added to the mixed solution, and the electrolyte was prepared after mixing evenly.
[0027] Preparation of positive electrode:
[0028] The ternary material LiNi 0.8 Co 0.1 Mn 0.1 Zr 0.03 O2, conductive agent SuperP, adhesive PVDF and carbon nanotubes (CNT) are mixed evenly in a mass ratio of 96.5:1.5:1:1 to form a lithium-ion battery positive electrode slurry with a certain viscosity, which is coated on the aluminum foil for current collector. The coating amount is 324g / m 2 , dried at 85°C and then cold pressed; then trimmed, cut into pieces, and slit, and after slitting, dried at 85°C for 4 hours under vacuum conditions, and the tabs were welded to make positive electrodes that meet the requirements.
[0029] Preparation of negative electrode:
[0030] Artificial graphite and silicon are mixed in a mass ratio of 90:10, and then mixed with conductive agent SuperP, thickener CMC, and adhesive SBR (styrene-butadiene rubber latex) in a mass ratio of 95:1.5:1.0:2.5 to make a slurry, mix evenly, apply the mixed slurry on both sides of the copper foil, dry and roll to obtain a negative electrode sheet, and make a negative electrode sheet that meets the requirements.
[0031] Preparation of lithium-ion batteries:
[0032] The positive electrode sheet, negative electrode sheet and separator prepared according to the above process are laminated to form a lithium-ion battery with a thickness of 4.7mm, a width of 55mm and a length of 60mm. The battery is vacuum-baked at 75°C for 10h and the above electrolyte is injected. After standing for 24h, the battery is charged to 4.4V with a constant current of 0.1C (180mA), and then charged at a constant voltage of 4.4V until the current drops to 0.05C (90mA); then discharged to 3.0V with 0.2C (180mA), and the charge and discharge are repeated twice. Finally, the battery is charged to 3.8V with 0.2C (180mA) to complete the production of the lithium-ion battery.
[0033] The components and contents of the electrolytes of Examples 1 to 15 and Comparative Examples 1 to 3 are shown in Table 1, wherein the preparation processes of the electrolytes, positive electrode sheets, negative electrode sheets, and lithium-ion batteries of Examples 2 to 15 and Comparative Examples 1 to 3 are the same as those of Example 1.
[0034] Table 1 Compositions of the electrolytes of the embodiments and comparative examples
[0035]
[0036]
[0037] The above compound 7 is ethylene glycol dimethyl ether (cas: 110-71-4), and its structure is shown below:
[0038]
[0039] The lithium ion batteries prepared in Examples 1 to 15 and Comparative Examples 1 to 3 were subjected to high temperature storage performance test, high temperature cycle performance test, room temperature lithium ion cycle performance test, and low temperature performance test under the following conditions. The results are shown in Table 2.
[0040] High temperature storage performance test :
[0041] At room temperature (25°C), the lithium-ion battery was charged and discharged at 0.5C / 0.5C (the battery discharge capacity was recorded as C0), with an upper limit voltage of 4.4V, and then the battery was charged to 4.4V under 0.5C constant current and constant voltage conditions, and the battery thickness was measured (the thickness was recorded as D0); the battery was placed in a 60°C oven for 30 days, taken out and the battery thickness was measured (the thickness was recorded as D1); the battery was placed in a 25°C environment and discharged at 0.5C (the discharge capacity was recorded as C1); the lithium-ion battery was continued to be charged and discharged at room temperature (25°C) at 0.5C / 0.5C (the battery discharge capacity was recorded as C2), with an upper limit voltage of 4.4V, and the capacity retention rate, capacity recovery rate and thickness expansion rate were calculated.
[0042] Capacity retention rate = (C1 / C0)*100%
[0043] Capacity recovery rate = (C2 / C0)*100%
[0044] Thickness expansion rate = (D1 / D0)*100%
[0045] Room temperature fast charging cycle performance test :
[0046] At room temperature (25°C), the lithium-ion battery is charged and discharged at 1.0C / 1.0C once (the battery discharge capacity is C0) with an upper voltage of 4.4V, and then charged and discharged at 4.0C / 1.0C for 500 cycles at room temperature (the battery discharge capacity is C1), and the capacity retention rate is calculated.
[0047] Capacity retention rate = (C1 / C0)*100%
[0048] High temperature cycle test :
[0049] Under high temperature (45°C) conditions, the lithium-ion battery is charged and discharged at 1.0C / 1.0C once (the battery discharge capacity is C0) with an upper voltage of 4.4V, and then charged and discharged at 1.0C / 1.0C for 400 cycles at room temperature (the battery discharge capacity is C1), and the capacity retention rate is calculated.
[0050] Capacity retention rate = (C1 / C0)*100%
[0051] Low temperature performance test :
[0052] At room temperature (25°C), the lithium-ion battery is charged and discharged at 0.5C / 0.5 (battery cut-off voltage is 3.0V, discharge capacity is C0), and the upper limit voltage is 4.4V (cut-off current 0.05C). Then the battery is fully charged to 4.4V (cut-off current 0.05C) at 0.5C at room temperature (25°C), and then the battery is transferred to -20°C and left for 4 hours, and discharged to 3.0V at 0.5C, and the discharge capacity is C1. The capacity retention rate is calculated.
[0053] Capacity retention rate = (C1 / C0)*100%
[0054] Table 2 Lithium-ion battery performance test results
[0055]
[0056]
[0057] As can be seen from Table 2, compared with Comparative Example 1, Examples 1 to 6 use the additive shown in Formula 1 of the present invention in their electrolytes, and the lithium-ion batteries not only have good high-temperature storage and high-temperature cycle performance, but also have good low-temperature performance at -20°C. This is because Formula 1 of the present invention includes two structures, chain ether and cyclic ether, which makes Formula 1 have relatively high stability and can maintain the stability of the SEI layer at high temperature and high pressure; at the same time, Formula 1 can also cooperate with LiTDI to form an inorganic and oxygen-containing double interface containing fluorine, nitrogen, and oxygen, which is not easily dissolved in carbonates, thereby further improving the stability of the SEI layer; in addition, the cyclic ether structure in Compound A gives it low viscosity and low melting point characteristics, which means that the dissociation process of LiTDI will be greatly promoted, thereby improving the conductivity of the electrolyte. In summary, the electrolyte of the present invention can improve the electrode stability at high voltage and high temperature by combining LiTDI with Compound A shown in Formula 1, promote the formation of a stable SEI layer, and significantly improve the conductivity of the electrolyte, thereby comprehensively improving the cycle performance and low-temperature discharge performance of the lithium-ion battery.
[0058] By comparing Example 1 with Example 10, it can be seen that the lithium salt using only LiTDI can also make the lithium-ion battery have good cycle performance and low-temperature discharge performance. This is because the cyclic ether structure in compound A gives it low viscosity and low melting point characteristics, which means that the dissociation process of LiTDI will be greatly promoted, thereby improving the conductivity of the electrolyte, that is, the LiTDI of the present invention does not need to be used in combination with a lithium salt with high conductivity (such as lithium hexafluorophosphate, lithium hexafluoroarsenate, lithium tetrafluoroborate, lithium perchlorate, etc.).
[0059] By comparing Example 1 with Examples 11 to 12, it can be seen that adding an auxiliary agent on the basis of the additive of the present invention can further improve the cycle performance and low-temperature discharge performance of the lithium-ion battery.
[0060] Comparing Examples 11 to 12 with Examples 13 to 15, it can be seen that when VC / FEC mixed additives are used in the electrolyte, the high temperature performance and low temperature performance of the lithium ion battery are greatly improved, and the expansion rate is further improved.
[0061] By comparing Example 1 and Comparative Example 3, it can be seen that the cycle performance and low-temperature discharge performance of the lithium-ion battery of Comparative Example 3 are worse than those of Example 1. This is because Compound 7 only has chain ether, which has a low oxidation potential, which easily causes the battery to produce gas at high voltage and temperature, thereby deteriorating the battery performance.
[0062] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention is described in detail with reference to the preferred embodiments, it is not limited to those listed in the embodiments. Those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. An electrolyte, characterized in that: The invention comprises a lithium salt, an organic solvent and an additive, wherein the lithium salt comprises 2-trifluoromethyl-4,5-dicyanoimidazole lithium, and the additive comprises a compound A shown in Formula 1: Wherein R1-R2 are each independently selected from alkyl, alkenyl, alkynyl or acyl.
2. The electrolyte according to claim 1, characterized in that R1-R2 are each independently selected from C1-C6 alkyl, C2-C6 alkenyl, C2-C6 alkynyl or C1-C6 acyl.
3. The electrolyte according to claim 1, characterized in that The group of R1 is the same as the group of R2.
4. The electrolyte according to claim 1, characterized in that The compound A is selected from at least one of compounds 1 to 6:
5. The electrolyte according to claim 1, characterized in that The mass of the additive accounts for 0.1-5.0% of the total mass of the electrolyte.
6. The electrolyte according to claim 1, characterized in that The lithium salt also includes at least one of lithium hexafluorophosphate, lithium perchlorate, lithium tetrafluoroborate, lithium bis(fluorosulfonyl imide), lithium bis(trifluoromethylsulfonyl imide), lithium methane sulfonate, lithium trifluoromethyl sulfonate, lithium fluorosulfonate, lithium bis(oxalatoborate), lithium difluorooxalatoborate, lithium difluorophosphate, lithium difluorobis(oxalatophosphate), lithium bis(fluorosulfonyl imide), lithium diphosphate and lithium lower aliphatic carboxylate.
7. The electrolyte according to claim 1, characterized in that The organic solvent includes at least one of carbonate, carboxylate and ether compounds.
8. The electrolyte according to claim 1, characterized in that It also includes an auxiliary agent, which is selected from vinylene carbonate, vinylene carbonate, fluoroethylene carbonate, vinyl sulfite, 1,3-propane sultone, 1,3-propylene sultone, 1,4-butane sultone, vinyl sulfate, succinic anhydride, maleic anhydride, 2-methylmaleic anhydride, methyl carbonate-2-propynyl ester, tetravinylsilane, triallyl isocyanurate, hexamethylene diisocyanate, o-phenanthroline, p-phenylene diisocyanate, 2, At least one of 4-toluene diisocyanate, N-phenylbis(trifluoromethanesulfonyl)imide, vinyl bissulfate, phenyl methanesulfonate, vinyl bissulfate, bis-spiro-propylene sulfate, hydroquinone difluorosulfonate, triallyl phosphate, tripropargyl phosphate, 2,4-butane sultone, isocyanoethyl methacrylate, methylene disulfonate, tris(trimethylsilyl)borate, tris(trimethylsilyl)phosphate, and tris(vinyldimethylsilyl)phosphate.
9. A lithium ion battery comprising a positive electrode and a negative electrode, characterized in that: Also includes the electrolyte according to any one of claims 1 to 8.
10. The lithium ion battery according to claim 9, characterized in that The active material of the positive electrode is selected from lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide 、 At least one of lithium iron phosphate, a composite material of lithium iron phosphate and carbon, lithium manganese phosphate, a composite material of lithium manganese phosphate and carbon, lithium iron manganese phosphate, and a composite material of lithium iron manganese phosphate and carbon.