Electrolyte, secondary battery and electric device
By using additives such as trimethylsilane and triazole ester compounds in the electrolyte, the problem of unstable interface between the positive and negative electrodes of lithium-ion batteries is solved, the cycle performance and high-temperature storage performance of the battery are improved, and the overall battery is enhanced. Stability and safety.
Patent Information
- Application Number
- CN202411018056.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-15
AI Technical Summary
Existing lithium-ion batteries have problems such as lattice oxygen loss, cation mixing, transition metal ion dissolution and electrolyte decomposition in the high nickel positive electrode and silicon negative electrode, resulting in unstable interfaces and affecting battery performance and safety.
Use compounds containing trimethylsilane and triazole ester compounds as additives for electrolytes, combined with components such as lithium difluorophosphate, to regulate the components and stability of the electrolyte interface film, inhibit impedance growth, and improve the interface stability of the positive and negative electrodes. sex.
It significantly improves the room temperature cycle performance, high-temperature storage performance and gas production performance of lithium-ion batteries, and enhances the stability and safety of the batteries.
Smart Images

Figure BDA0004966396370000021 
Figure BDA0004966396370000022 
Figure BDA0004966396370000031
Abstract
Description
Technical Field
[0001] The present application relates to the field of battery technology, and in particular to an electrolyte, a secondary battery and an electrical device. Background Art
[0002] At present, the market is in urgent need of developing secondary batteries with higher energy density. High-nickel ternary positive electrode and silicon negative electrode have become research hotspots due to their higher theoretical capacity. For high-nickel positive electrode, the high-valent Ni formed in a highly delithiated state 4+ Ions are easily reduced to low valence states, such as Ni 3+ and Ni 2+ , which may lead to lattice oxygen loss, cation mixing and transition metal ion dissolution. For silicon negative electrodes, the volume changes greatly during the lithium insertion / delithiation process, the particles inside the electrode will be pulverized by mechanical stress, and the SEI formed by the decomposition of the electrolyte cannot adapt to the volume effect during the cycle and breaks, accelerating aging. In addition, LiPF6 produces acidic compounds after hydrolysis, which accelerates the dissolution of transition metals and the interface deterioration of the Ni-rich positive electrode. The dissolved metal ions migrate and deposit on the surface of the negative electrode, causing the electrolyte to continue to decompose and form Li dendrites on the negative electrode, threatening battery safety. Therefore, improving the stability of the positive and negative electrode / electrolyte interface is particularly important for improving the performance of lithium-ion batteries. From the perspective of cost and practicality, it is more appropriate to add functional electrolyte additives to the electrolyte. The composition and stability of the electrolyte interface film can be regulated by designing the molecular structure of the additive. Summary of the invention
[0003] The purpose of the present application is to provide an electrolyte, a secondary battery and an electrical device to improve the room temperature cycle performance and high temperature storage performance of the secondary battery.
[0004] To achieve the above objectives, in the first aspect of the present application, an electrolyte is provided, which comprises an additive, an organic solvent and an electrolyte salt, wherein the additive comprises a first additive and a second additive, wherein the first additive is a compound containing trimethylsilane, and the second additive is a triazole ester compound.
[0005] As an embodiment of the present application, the additive includes a third additive, and the third additive includes at least one of lithium difluorophosphate, lithium difluorooxalatoborate, lithium fluorosulfonate, and lithium difluorobisoxalatophosphate.
[0006] As an implementation scheme of the present application, based on the total mass of the electrolyte, the mass percentage of the first additive is W1, the mass percentage of the second additive is W2, and the mass percentage of the third additive is W3, wherein W1, W2 and W3 satisfy: 0.05≤(W1+W3) / W2≤4.5.
[0007] As an embodiment of the present application, based on the total mass of the electrolyte, the mass percentage of the first additive is W1, 0.50%≤W1≤1.50%.
[0008] As an embodiment of the present application, based on the total mass of the electrolyte, the mass percentage of the second additive is W2, 0.20%≤W2≤3.00%.
[0009] As an embodiment of the present application, based on the total mass of the electrolyte, the mass percentage of the third additive is W3, 0.10%≤W3≤0.50%.
[0010] As an embodiment of the present application, the trimethylsilane-containing compound comprises at least one of tris(trimethylsilyl)borate, tris(trimethylsilyl)phosphate, and tris(trimethylsilyl)phosphite.
[0011] As an embodiment of the present application, the triazole ester compound comprises a compound represented by Formula I and / or Formula II:
[0012]
[0013] Among them, R1 and R4 are each independently selected from at least one of hydrogen, an alkyl group with 1 to 6 carbon atoms, an alkenyl group with 2 to 6 carbon atoms, an alkynyl group with 2 to 6 carbon atoms, an alkoxy group with 1 to 6 carbon atoms, an amino group, a halogen atom, a benzene ring, and an aldehyde group; R2 and R3 are each independently selected from at least one of a substituted or unsubstituted alkyl group with 1 to 6 carbon atoms.
[0014] As an embodiment of the present application, the triazole ester compound comprises at least one of the compounds having the structural formulas shown in A1 to A7:
[0015]
[0016]
[0017] As an embodiment of the present application, the electrolyte salt includes one or both of lithium hexafluorophosphate and lithium bis(fluorosulfonyl)imide.
[0018] As an embodiment of the present application, the organic solvent comprises at least two of chain carbonate, cyclic carbonate, carboxylic acid ester, acetonitrile, and sulfolane.
[0019] In the second aspect of the present application, a secondary battery is provided, the secondary battery comprising a positive electrode plate, the positive electrode plate comprising a positive electrode collector and a positive electrode active material layer arranged on at least one surface of the positive electrode collector, the positive electrode active material layer comprising a positive electrode active material; a negative electrode plate, the negative electrode plate comprising a negative electrode collector and a negative electrode active material layer arranged on at least one surface of the negative electrode collector, the negative electrode active material layer comprising a negative electrode active material; a separator; and the electrolyte described in the first aspect of the present application.
[0020] As an embodiment of the present application, the positive electrode active material comprises at least one of lithium nickel cobalt manganese oxide or lithium nickel cobalt aluminum oxide; when the positive electrode active material comprises lithium nickel cobalt manganese oxide, the molar amount of the nickel element is greater than 0.5, based on the molar amount of the nickel element, the cobalt element and the manganese element in the lithium nickel cobalt manganese oxide being 1; when the positive electrode active material comprises lithium nickel cobalt aluminum oxide, the molar amount of the nickel element is greater than 0.5, based on the molar amount of the nickel element, the cobalt element and the aluminum element in the lithium nickel cobalt aluminum oxide being 1.
[0021] As an embodiment of the present application, the negative electrode active material contains silicon.
[0022] According to a third aspect of the present application, an electrical device is provided, wherein the electrical device comprises the secondary battery according to the second aspect of the present application.
[0023] Compared with the prior art, the beneficial effects of this application are:
[0024] The present application provides an electrolyte, the electrolyte comprising an additive, an organic solvent and an electrolyte salt, the additive comprising a first additive and a second additive, the first additive being a compound containing trimethylsilane, and the second additive being a triazole ester compound. The present application suppresses the impedance growth during the cycle of a ternary-silicon dioxide system secondary battery, and improves the normal temperature cycle performance, high temperature storage performance and gas production performance by adding a compound containing trimethylsilane as the first additive and a triazole ester compound as the second additive to the electrolyte. DETAILED DESCRIPTION
[0025] To better illustrate the purpose, technical solutions and advantages of the present application, the present application will be further described below in conjunction with specific examples, but the examples do not limit the present application in any form. Unless otherwise specified, the reagents, methods and equipment used in the present application are conventional reagents, methods and equipment in the art. Unless otherwise specified, the reagents and materials used in the present application are commercially available.
[0026] An embodiment of the present application provides an electrolyte, which includes an additive, an organic solvent and an electrolyte salt, wherein the additive includes a first additive and a second additive, wherein the first additive is a compound containing trimethylsilane, and the second additive is a triazole ester compound.
[0027] In the present application, the -Si(CH3)3-O structure in the compound containing trimethylsilane decomposes and defluorinates with the electrolyte salt (usually fluorinated) to generate a compound that can reduce impedance, thereby improving the stability of the battery. The triazole ester compound used in the electrolyte of the present application can preferentially undergo redox reactions at the positive / negative electrodes to generate stable CEI / SEI, promoting Li + The compound can also moderately inhibit the acidity of the electrolyte and reduce the generation of HF acid, thereby alleviating the corrosion of the positive and negative electrodes. The synergy of the two can take into account the stability of the positive and negative electrode / electrolyte interface and more effectively guarantee the electrochemical performance of the whole battery.
[0028] In some embodiments, the additive includes a third additive, and the third additive includes at least one of lithium difluorophosphate, lithium difluorooxalatoborate, lithium fluorosulfonate, and lithium difluorobisoxalatophosphate. The third additive can regulate the SEI component of the silicon negative electrode / electrolyte interface, increase the inorganic component in the SEI, and thus improve the Li + Improve the interface conduction capacity and reduce the interface impedance, improve the stability of SEI structure, and inhibit the generation of side reactions.
[0029] In some embodiments, based on the total mass of the electrolyte, the mass percentage of the first additive is W1, the mass percentage of the second additive is W2, and the mass percentage of the third additive is W3, wherein W1, W2 and W3 satisfy: 0.05≤(W1+W3) / W2≤4.5. For example, (W1+W3) / W2 can be any one of 0.05, 0.1, 0.5, 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5 or a range between any two values. When W1, W2 and W3 meet the above ranges, the normal temperature cycle performance, high temperature storage and gas production performance of the secondary battery can be further improved.
[0030] In some embodiments, based on the total mass of the electrolyte, the mass percentage of the first additive is W1, 0.30% ≤ W1 ≤ 2.00%. For example, W1 can be any one of 0.30%, 0.50%, 1.00%, 1.20%, 1.50%, 1.80%, 2.00%, or a range between any two values. In some embodiments, based on the total mass of the electrolyte, the mass percentage of the first additive is W1, 0.50% ≤ W1 ≤ 1.50%. When W1 is within the above range, the normal temperature cycle performance, high temperature storage and gas production performance of the secondary battery can be further improved.
[0031] In some embodiments, based on the total mass of the electrolyte, the mass percentage of the second additive is W2, 0.20%≤W2≤3.00%. For example, W2 can be any one of 0.20%, 0.50%, 1.00%, 1.50%, 2.00%, 2.50%, 3.00%, or a range between any two values. When W2 is within the above range, the normal temperature cycle performance, high temperature storage and gas production performance of the secondary battery can be further improved.
[0032] In some embodiments, based on the total mass of the electrolyte, the mass percentage of the third additive is W3, 0.10%≤W3≤0.50%. For example, W3 can be any one of 0.10%, 0.15%, 0.20%, 0.25%, 0.30%, 0.35%, 0.40%, 0.45%, 0.50%, or a range between any two values. When W3 is within the above range, the normal temperature cycle performance, high temperature storage and gas production performance of the secondary battery can be further improved.
[0033] In some embodiments, the trimethylsilane-containing compound comprises at least one of tris(trimethylsilyl)borate, tris(trimethylsilyl)phosphate, and tris(trimethylsilyl)phosphite.
[0034] In some embodiments, the triazole ester compound comprises a compound represented by Formula I and / or Formula II:
[0035]
[0036] Among them, R1 and R4 are each independently selected from at least one of hydrogen, an alkyl group with 1 to 6 carbon atoms, an alkenyl group with 2 to 6 carbon atoms, an alkynyl group with 2 to 6 carbon atoms, an alkoxy group with 1 to 6 carbon atoms, an amino group, a halogen atom, a benzene ring, and an aldehyde group; R2 and R3 are each independently selected from at least one of a substituted or unsubstituted alkyl group with 1 to 6 carbon atoms.
[0037] In some embodiments, the triazole ester compound comprises at least one of the compounds having the structural formulas A1 to A7:
[0038]
[0039] The CAS numbers of the compounds represented by A1 to A7 in the present application are 149104-88-1, 1255651-14-9, 850567-98-5, 913836-00-7, 613660-87-0, 21733-05-1, and 3641-14-3, respectively.
[0040] In some embodiments, the electrolyte salt comprises one or both of lithium hexafluorophosphate and lithium bis(fluorosulfonyl)imide.
[0041] In some embodiments, the concentration of the electrolyte salt in the electrolyte is 0.8 M to 1.3 M. For example, the concentration of the electrolyte salt can be any value among 0.8 M, 0.9 M, 1.0 M, 1.1 M, 1.2 M, 1.3 M or the range between any two values. When the concentration of the electrolyte salt is within the above range, the conductivity of the electrolyte can be ensured to be within a suitable range.
[0042] In some embodiments, the organic solvent comprises at least two of linear carbonates, cyclic carbonates, carboxylic acid esters, acetonitrile, and sulfolane. In some embodiments, the linear carbonate comprises at least one of ethyl methyl carbonate, dimethyl carbonate, methyl propyl carbonate, and diethyl carbonate. In some embodiments, the cyclic carbonate comprises at least one of ethylene carbonate, propylene carbonate, butylene carbonate, and fluoroethylene carbonate. In some embodiments, the carboxylic acid ester comprises at least one of ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, and methyl butyrate.
[0043] In some embodiments, the organic solvent accounts for 5 to 20 wt% of the total weight of the electrolyte. For example, the organic solvent may account for the total weight of the electrolyte as any value among 5 wt%, 8 wt%, 12 wt%, 15 wt%, 18 wt%, 20 wt% or the range between any two values.
[0044] In some embodiments, the secondary battery includes a positive electrode plate, the positive electrode plate includes a positive electrode current collector and a positive electrode active material layer provided on at least one surface of the positive electrode current collector, and the positive electrode active material layer contains a positive electrode active material.
[0045] In some embodiments, the chemical formula of the positive electrode active material includes Li a Ni x Co y Mn z M b O2, where 0.95 ≤ a ≤ 1.1, 0.5 ≤ x ≤ 1.0, 0 < y ≤ 0.3, 0 < z ≤ 0.2, 0 < b < 0.1, and x + y + z + b = 1.0, and M is at least one of Al, Zr, Ti, V, Mg, Fe, B, and Mo.
[0046] In some embodiments, the positive electrode active material comprises at least one of lithium nickel cobalt manganese oxide or lithium nickel cobalt aluminum oxide; when the positive electrode active material comprises lithium nickel cobalt manganese oxide, the molar amount of the nickel element is greater than 0.5, based on the molar amount of the nickel element, the cobalt element, and the manganese element in the lithium nickel cobalt manganese oxide being 1; when the positive electrode active material comprises lithium nickel cobalt aluminum oxide, the molar amount of the nickel element is greater than 0.5, based on the molar amount of the nickel element, the cobalt element, and the aluminum element in the lithium nickel cobalt aluminum oxide being 1.
[0047] In some embodiments, the positive electrode active material layer can be one or more layers. Each layer of the multi-layer positive electrode active material can contain the same or different positive electrode active materials. The positive electrode active material is any substance that can reversibly intercalate and deintercalate active ions.
[0048] In some embodiments, the positive electrode active material comprises a doping element and / or a coating element. There is no particular requirement for the doping element and / or the coating element, as long as the positive electrode active material can be made more stable.
[0049] In addition, the positive electrode active material layer further includes a positive electrode conductor and a positive electrode binder.
[0050] In some embodiments, the type of positive electrode conductive agent is not limited, and any known conductive agent can be used. Examples of positive electrode conductive agents may include but are not limited to acetylene black, carbon black, carbon nanotubes, graphene, etc. The above positive electrode conductive agents can be used alone or in any combination.
[0051] In some embodiments, the type of solvent used to form the positive electrode slurry is not limited, as long as it is a solvent that can dissolve or disperse the positive electrode active material, the positive electrode conductor, and the positive electrode binder. Examples of solvents used to form positive electrode slurries may include any of aqueous solvents and organic solvents. Examples of aqueous media may include, but are not limited to, water and mixed media of alcohol and water. Examples of organic media may include, but are not limited to, aliphatic hydrocarbons such as hexane; aromatic hydrocarbons such as benzene, toluene, xylene, and methylnaphthalene; heterocyclic compounds such as quinoline and pyridine; ketones such as acetone, methyl ethyl ketone, and cyclohexanone; esters such as methyl acetate and methyl acrylate; amines such as diethylenetriamine and N,N-dimethylaminopropylamine; ethers such as diethyl ether, propylene oxide, and tetrahydrofuran (THF); amides such as N-methylpyrrolidone (NMP), dimethylformamide, and dimethylacetamide; aprotic polar solvents such as hexamethylphosphoramide and dimethyl sulfoxide, etc.
[0052] There is no particular limitation on the type of positive electrode current collector, which can be any known material suitable for use as a positive electrode current collector. Examples of positive electrode current collectors may include, but are not limited to, metal materials such as aluminum, stainless steel, nickel plating, titanium, and tantalum; carbon materials such as carbon cloth and carbon paper; and composite materials formed by polymers and metal layers. In some embodiments, the positive electrode current collector is a metal material. In some embodiments, the positive electrode current collector is aluminum.
[0053] In some embodiments, the secondary battery includes a negative electrode plate, the negative electrode plate includes a negative electrode collector and a negative electrode active material layer arranged on at least one surface of the negative electrode collector, the negative electrode active material contains a negative electrode active material, and the negative electrode active material includes at least one of a graphite material and a silicon-based material.
[0054] In some embodiments, the negative electrode active material contains silicon.
[0055] The type of negative electrode current collector is not particularly limited and can be selected according to actual needs. Preferably, aluminum foil or carbon-coated aluminum foil can be used.
[0056] In order to prevent short circuit, a separator is usually provided between the positive electrode and the negative electrode. The type of separator is not particularly limited and can be selected according to actual needs. The separator can be a polypropylene film, a polyethylene film, a polyvinylidene fluoride film, a spandex film, an aramid film, or a multilayer composite film modified by a coating.
[0057] In some embodiments, the present application provides an electrical device, which includes the above-mentioned secondary battery. The electrical device can be an application device such as a vehicle, a mobile phone, a portable device, a laptop computer, a ship, a spacecraft, an electric toy, and an electric tool. The vehicle can be a new energy vehicle, and the new energy vehicle can be a pure electric vehicle, a hybrid vehicle, or an extended-range vehicle, etc.; the spacecraft includes an airplane, a rocket, a space shuttle, and a spacecraft, etc.; the electric toy includes a fixed or mobile electric toy, for example, a game console, an electric car toy, an electric ship toy, and an electric airplane toy, etc.; the electric tool includes a metal cutting electric tool, a grinding electric tool, an assembly electric tool, and an electric tool for railways, for example, an electric drill, an electric grinder, an electric wrench, an electric screwdriver, an electric hammer, an impact drill, a concrete vibrator, and an electric planer, etc. The embodiments of the present application do not impose any special restrictions on the above-mentioned devices.
[0058] The following are specific embodiments of the present application, and the technical scheme of the present application is further described in conjunction with the embodiments, but the present application is not limited to these embodiments. The reagents, methods and equipment used in the present application, unless otherwise specified, are conventional reagents, methods and equipment in the art.
[0059] Example 1
[0060] Embodiment 1 provides a lithium ion battery, and the preparation method thereof comprises the following steps:
[0061] (1) Preparation of positive electrode sheet
[0062] The positive electrode active material LiNi 0.6 Mn 0.2 Co 0.2 O2 (NMC622), conductive agent acetylene black (Super P) and binder polyvinylidene fluoride (PVDF) are mixed evenly in a mass ratio of NMC622:Super P:PVDF=94:3:3, and evenly dispersed in 1-methyl-2-pyrrolidone (NMP) to form a uniform black slurry. The mixed slurry is coated on both sides of the aluminum foil, and then baked, rolled and cut into pieces to obtain the positive electrode sheet.
[0063] (2) Preparation of negative electrode sheet
[0064] The negative electrode active materials are artificial graphite (AG), silicon dioxide (SiO x ), conductive agent acetylene black (Super P) and binder SBR according to the mass ratio of AG:SiO x :Super P:SBR=91:3:3:3 are mixed evenly and dispersed evenly in deionized water to form a uniform black slurry. The mixed slurry is coated on both sides of the copper foil, and then baked, rolled and cut into pieces to obtain the negative electrode sheet.
[0065] (3) Preparation of electrolyte
[0066] At room temperature, in a glove box filled with argon (H2O <1ppm, O2 <1ppm), EC, EMC and DEC were mixed in a mass ratio of 3:5:2 and The molecular sieve is used to remove water, and LiPF6 and LiFSI are added to the obtained mixed solvent. The mixture is stirred continuously and cooled down to ensure that the temperature of the electrolyte does not rise by more than 2°C. Lithium salt is then added to finally obtain a colorless transparent liquid. Tris(trimethylsilyl) phosphate equivalent to 1% of the total mass of the electrolyte, 0.5% of A7, and 0.05% of lithium difluorooxalatoborate are added, and the mixture is stirred evenly to obtain an electrolyte in which the concentrations of LiPF6 and LiFSI are 1M and 0.2M, respectively.
[0067] (4) Preparation of lithium-ion batteries
[0068] The prepared positive electrode sheet, separator (polyethylene), and negative electrode sheet are stacked in order, with the separator placed between the positive and negative electrode sheets. The bare battery cell is obtained by winding, hot pressing and welding the tabs. The bare battery cell is placed in an outer packaging aluminum-plastic film and baked in an oven at 85±10℃ for 24h. The prepared electrolyte is injected into the dried battery, allowed to stand, formed, and divided to complete the preparation of the lithium-ion soft-pack battery.
[0069] The difference between Examples 2 to 17 and Comparative Examples 1 to 6 and Example 1 is that the types and contents of the additives are different, as shown in Table 1 for details.
[0070] Table 1
[0071]
[0072]
[0073] The performance of the secondary batteries obtained in the above examples and comparative examples was tested, and the specific test items, test methods and results are as follows:
[0074] Room temperature DCR test: At 25±2°C, the batteries obtained in Examples 1 to 17 and Comparative Examples 1 to 6 were charged to 4.25V at 1C, then discharged at 1C capacity for 30 min, adjusted to 50% SOC, 5C constant current pulse discharged for 10s and then charged for 10s, and DCR was calculated as (voltage before pulse discharge - voltage after pulse discharge) / discharge current. After 30 days of high temperature storage at 60°C, when the battery was completely cooled to 25±2°C, the DCR was tested again, and the internal resistance change rate = (DCR after 30 days - DCR before 30 days) / DCR before 30 days * 100%. The recorded results are shown in Table 2.
[0075] Normal temperature cycle performance test: At 25±2°C, the batteries obtained in Examples 1 to 17 and Comparative Examples 1 to 6 were subjected to charge and discharge cycle tests at a charge and discharge rate of 1C / 1C in the range of 2.5 to 4.25V, and the first week discharge capacity and the discharge capacity after 1000 cycles of the battery were recorded. The capacity retention rate of 1000 cycles = 1000 weeks discharge capacity / first week discharge capacity*100%, and the recorded data are shown in Table 2.
[0076] High temperature storage performance: The soft-pack batteries obtained in Examples 1 to 17 and Comparative Examples 1 to 6 were placed at 60±2°C, and the charge and discharge test was performed at a charge and discharge rate of 1C / 1C in the range of 2.8 to 4.4V, and the first week discharge capacity of the battery was recorded. After that, the battery was stored at 60±2°C for 120 days, and the charge and discharge test was performed again and the discharge capacity was recorded. High temperature storage capacity retention rate = discharge capacity after 120 days / first week discharge capacity*100%, and the recorded data is shown in Table 2.
[0077] High temperature gas production test: The soft-pack batteries obtained in Examples 1 to 17 and Comparative Examples 1 to 6 were charged to 4.25V at a constant current rate of 1C at 25±2°C, and then charged at a constant voltage of 4.25V until the current was less than 0.05C, so that they were in a fully charged state of 4.25V. The volume of the fully charged battery before storage was tested and recorded as V0; the fully charged battery was then placed in a 60±2°C oven. After 70 days, the battery was taken out and its volume after storage was immediately tested and recorded as V1. Volume expansion rate = (V1–V0) / V0*100%, and the results are shown in Table 2.
[0078] Table 2 Performance test results of secondary batteries prepared in Examples and Comparative Examples
[0079]
[0080]
[0081] Comparing Examples 2, 11 to 16 with Comparative Example 6, the results show that the comprehensive performance of the battery containing triazole ester-based additives is better than that of the battery containing triazole, indicating that adding an ester group to the structure of triazole can impart a higher effect.
[0082] By comparing Examples 2, 11 to 16, it can be seen that when the third additive triazole ester compound is A7, the overall performance of the battery is optimal. This may be because -NH2 has a stronger structural effect with nitrogen azole than other functional groups such as phenyl and halogen elements, and the N-containing interface film can achieve structural protection for the electrode active material; in addition, -NH2 has a stronger effect on H + It also has a certain cleaning effect, which can improve the stability of the interfacial film and inhibit the generation of side reactions.
[0083] By comparing Example 2 and Example 17, it can be seen that further containing the third additive can further optimize the room temperature cycle performance, high temperature storage performance and gas production performance of the battery.
[0084] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present application rather than to limit the scope of protection of the present application. Although the present application has been described in detail with reference to the preferred embodiments, ordinary technicians in this field should understand that the technical solution of the present application can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present application.
Claims
1. An electrolyte, characterized in that: The electrolyte solution comprises an additive, an organic solvent and an electrolyte salt, wherein the additive comprises a first additive and a second additive, wherein the first additive is a compound containing trimethylsilane, and the second additive is a triazole ester compound.
2. The electrolyte according to claim 1, characterized in that: The additive includes a third additive, and the third additive includes at least one of lithium difluorophosphate, lithium difluorooxalatoborate, lithium fluorosulfonate, and lithium difluorobisoxalatophosphate.
3. The electrolyte according to claim 2, characterized in that: Based on the total mass of the electrolyte, the mass percentage of the first additive is W1, the mass percentage of the second additive is W2, and the mass percentage of the third additive is W3, wherein W1, W2 and W3 satisfy: 0.05≤(W1+W3) / W2≤4.
5.
4. The electrolyte according to claim 2, characterized in that: Based on the total mass of the electrolyte, at least one of the following characteristics is met: (a) the mass percentage content of the first additive is W1, 0.50%≤W1≤1.50%; (b) the mass percentage content of the second additive is W2, 0.20%≤W2≤3.00%; (c) The mass percentage content of the third additive is W3, 0.10%≤W3≤0.50%.
5. The electrolyte according to claim 1, characterized in that: The trimethylsilane-containing compound comprises at least one of tri(trimethylsilyl)borate, tri(trimethylsilyl)phosphate, and tri(trimethylsilyl)phosphite.
6. The electrolyte according to claim 1, characterized in that: The triazole ester compound comprises a compound represented by Formula I and / or Formula II: Among them, R1 and R4 are each independently selected from at least one of hydrogen, an alkyl group with 1 to 6 carbon atoms, an alkenyl group with 2 to 6 carbon atoms, an alkynyl group with 2 to 6 carbon atoms, an alkoxy group with 1 to 6 carbon atoms, an amino group, a halogen atom, a benzene ring, and an aldehyde group; R2 and R3 are each independently selected from at least one of a substituted or unsubstituted alkyl group with 1 to 6 carbon atoms.
7. The electrolyte according to claim 6, characterized in that: The triazole ester compound comprises at least one of the compounds having the structural formulas A1 to A7:
8. A secondary battery, characterized in that: Include: A positive electrode sheet, the positive electrode sheet comprising a positive electrode current collector and a positive electrode active material layer disposed on at least one surface of the positive electrode current collector, the positive electrode active material layer comprising a positive electrode active material; A negative electrode sheet, the negative electrode sheet comprising a negative electrode current collector and a negative electrode active material layer disposed on at least one surface of the negative electrode current collector, the negative electrode active material layer comprising a negative electrode active material; Diaphragm; And the electrolyte according to any one of claims 1 to 7.
9. The secondary battery according to claim 8, characterized in that: The positive electrode active material comprises at least one of lithium nickel cobalt manganese oxide or lithium nickel cobalt aluminum oxide; when the positive electrode active material comprises lithium nickel cobalt manganese oxide, the molar amount of the nickel element is greater than 0.5, based on the molar amount of the nickel element, the cobalt element and the manganese element in the lithium nickel cobalt manganese oxide being 1; when the positive electrode active material comprises lithium nickel cobalt aluminum oxide, the molar amount of the nickel element is greater than 0.5, based on the molar amount of the nickel element, the cobalt element and the aluminum element in the lithium nickel cobalt aluminum oxide being 1.
10. The secondary battery according to claim 8, characterized in that: The negative electrode active material contains silicon.
11. An electrical device, characterized in that: A secondary battery comprising the secondary battery according to any one of claims 8 to 10.
Citation Information
Patent Citations
Additive for electrolyte of lithium battery, electrolyte for lithium battery including same, and lithium battery employing same electrolyte
CN109565080A
Electrolyte, electrochemical device, and electronic device
CN111313091A
Electrolyte and secondary battery
CN115966765A
Electrolyte, lithium secondary battery, and electric device
CN117352844A
Electrolyte additive, electrolyte for lithium ion battery and lithium ion battery
CN117613389A