Method for manufacturing electrode body for non-aqueous electrolyte secondary battery, and method for manufacturing non-aqueous electrolyte secondary battery

By adjusting the thickness and weight of the positive electrode plate per unit area, controlling the shaping load of the winding body, the lithium-ion secondary battery electrode body is pressed at room temperature, solving the problems of high cost and low production efficiency of the electrode body heating equipment, and improving production efficiency And suppresses plastic deformation of the septum.

CN118970206APending Publication Date: 2024-11-15TOYOTA BATTERY CO LTD +2
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410569253.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-05-15
Filing Date
2024-05-09
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The prior art requires heating equipment during the pressing process of lithium-ion secondary battery electrodes, resulting in high equipment costs and low production efficiency, and the heating and cooling process affects the production rhythm.

Method used

By adjusting the thickness, weight per unit area and thickness after the pressing of the positive electrode coating process, the wound body shaping load is controlled to be less than 11 MPa to avoid excessive plastic deformation of the spacer, and the electrode body pressing is achieved at room temperature.

Benefits of technology

The electrode body manufacturing process is simplified, equipment costs are reduced, production efficiency is improved, and plastic deformation of the separator is effectively suppressed, avoiding the increase in resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118970206A_ABST
    Figure CN118970206A_ABST
Patent Text Reader

Abstract

The present invention addresses the problem of suppressing excessive plastic deformation of a spacer during pressing of an electrode body by a simple step. In the manufacturing of a lithium ion secondary battery, a wound body pressing step for shaping a wound electrode body into a flat shape, the difference between the thickness of the electrode body when the electrode body is pressed at 1.2 MPa after the wound body pressing step and the thickness of the electrode body when the electrode body is pressed at 0.03 MPa after the wound body pressing step is 0.4 mm or less is set as the wound body shaping load; the thickness [[mu] m] of the positive electrode plate after the positive electrode coating step, the weight [mg / cm < 2 >] of the coated positive electrode material layer, and the thickness [[mu] m] of the positive electrode plate after the positive electrode pressing step are adjusted so that the winding shaping load is 11 [MPa] or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for manufacturing an electrode body for a non-aqueous electrolyte secondary battery and a method for manufacturing a non-aqueous electrolyte secondary battery. More specifically, the present invention relates to a method for manufacturing an electrode body for a non-aqueous electrolyte secondary battery and a method for manufacturing a non-aqueous electrolyte secondary battery, which utilizes a simple process to suppress excessive plastic deformation of a spacer during pressing of the electrode body. Background Art

[0002] Non-aqueous electrolyte secondary batteries such as lithium-ion secondary batteries have high energy density, high voltage and high output, and are therefore carried in vehicles as power sources for driving electric vehicles, hybrid vehicles, and the like. The vehicle-mounted non-aqueous electrolyte secondary battery comprises an electrode body, a non-aqueous electrolyte, and a rectangular parallelepiped battery case for housing them. In order to achieve miniaturization, the electrode body is constructed in a manner in which the positive electrode plate and the negative electrode plate are stacked and wound with a separator. Afterwards, the wound body of the electrode body is shaped into a flat shape corresponding to the internal dimensions of the battery case through a pressing process. The unit cells manufactured in this way are stacked and used in the form of a battery pack. At this time, for the electrode body housed in the battery case, in order to improve the stability and pressure resistance as a battery pack, the electrode body is pressed at a certain pressure or above.

[0003] In the existing method, when the wound body of the electrode body is pressed into a flat shape, if the pressing load for compressing the electrode body is simply increased, the pores of the separator will be flattened, causing an increase in resistance. In order to improve the formability of the electrode body during pressing, the invention described in Patent Document 1 softens the electrode body by heat treating the positive and negative plates. This process improves formability.

[0004] In the invention described in Patent Document 2, the electrode body is heated to stabilize the shape of the electrode body, and then the heated electrode body is pressed. According to such an invention, since the positive electrode plate and the like are softened by heating, the electrode body can be pressed into a flat shape with a very small load, and the pores of the separator are not crushed. Prior art literature Patent Literature

[0005] Patent Document 1: Japanese Patent Application Publication No. 2012-059491 Patent Document 2: Japanese Patent Application Publication No. 2013-206587 Summary of the invention Problems to be solved by the invention

[0006] However, heating the electrode body requires heating equipment, which increases equipment costs. Heating and cooling the electrode body also deteriorates production cycles and reduces production efficiency.

[0007] An object of the present disclosure is to suppress excessive plastic deformation of a spacer during pressing of an electrode assembly using a simple process. Means for solving problems

[0008] The present invention discloses a method for manufacturing an electrode body for a non-aqueous electrolyte secondary battery in one embodiment, wherein the non-aqueous electrolyte secondary battery comprises an electrode body, a non-aqueous electrolyte, and a rectangular parallelepiped battery case for accommodating the electrode body and the non-aqueous electrolyte, characterized in that the manufacturing method comprises the following steps: a positive electrode coating step, in which a positive electrode composite material layer is coated on a positive electrode collector foil of the electrode body to produce a positive electrode plate; a positive electrode pressing step, in which the produced positive electrode plate is pressed; a lamination step, in which the pressed positive electrode plate and a negative electrode plate comprising a negative electrode collector foil and a negative electrode composite material layer are laminated via a separator composed of a porous resin; a winding step, in which the laminated electrode body is wound; and a wound body pressing step, in which the wound electrode body is shaped into a flat shape, and the thickness T1 of the electrode body is reduced. The load of the winding body pressing step in which the difference ΔT between the thickness T2 mm and the thickness T is less than 0.4 mm is set as the winding body shaping load (shaping load) PLMPa, the thickness T1 of the electrode body is the thickness of the electrode body when the electrode body is pressurized at 1.2 MPa after the winding body pressing step, and the thickness T2 of the electrode body is the thickness of the electrode body when the electrode body is pressurized at 0.03 MPa after the winding body pressing step. At this time, the thickness Aμm of the positive electrode plate after the positive electrode coating step, the positive electrode unit area weight B mg / cm2 of the coating of the positive electrode composite material layer in the positive electrode coating step 2 The thickness C μm of the positive electrode plate after the positive electrode pressing step is adjusted so that the winding body shaping load PL MPa is 11 MPa or less.

[0009] Another aspect of the present invention is a method for manufacturing an electrode body for a non-aqueous electrolyte secondary battery, wherein the non-aqueous electrolyte secondary battery comprises an electrode body, a non-aqueous electrolyte, and a rectangular parallelepiped battery case for accommodating the electrode body and the non-aqueous electrolyte, characterized in that the manufacturing method comprises the following steps: a positive electrode coating step, in which a positive electrode composite material layer is coated on a positive electrode collector foil of the electrode body to produce a positive electrode plate; a positive electrode pressing step, in which the produced positive electrode plate is pressed; a lamination step, in which the pressed positive electrode plate and a negative electrode plate comprising a negative electrode collector foil and a negative electrode composite material layer are laminated via a separator composed of a porous resin; a winding step, in which the laminated electrode body is wound; and a wound body pressing step, in which the wound electrode body is formed into a flat shape, the thickness of the positive electrode plate after the positive electrode coating step is set to A μm, and the positive electrode unit area weight of the positive electrode composite material layer in the positive electrode coating step is set to B mg / cm 2 , when the thickness of the positive electrode plate after the positive electrode pressing step is set to C μm and the thickness of the positive electrode collector foil is set to D μm, Figure 8 The positive electrode density change ΔPD g / cm is obtained by using the formula (1) shown in 3 When the thickness A μm of the positive electrode plate after the positive electrode coating step and the positive electrode unit area weight B mg / cm 2 , the thickness C μm of the positive electrode plate after the positive electrode pressing step, and the thickness D μm of the positive electrode collector foil are adjusted so that the positive electrode density change ΔPD is 1.0 g / cm 3 the following. In the manufacturing method, the thickness A μm of the positive electrode plate after the positive electrode coating step and the positive electrode unit area weight B mg / cm 2 , the thickness C μm of the positive electrode plate after the positive electrode pressing step, and the thickness D μm of the positive electrode collector foil are adjusted so that the positive electrode density change ΔPD is 0.63 [g / cm 3 ]above.

[0010] In the above production method, in the wound body pressing step, the electrode body may be pressed at room temperature without heating the electrode body. In the above manufacturing method, the above positive electrode composite material layer may include a conductor, and the conductor may be a carbon nanotube.

[0011] In the present disclosure, the method for producing an electrode body for a nonaqueous electrolyte secondary battery may be included as a part of a method for producing a nonaqueous electrolyte secondary battery. Effects of the Invention

[0012] According to the method for producing an electrode body for a nonaqueous electrolyte secondary battery and the method for producing a nonaqueous electrolyte secondary battery of the present disclosure, excessive plastic deformation of the spacer during pressing of the electrode body can be suppressed by a simple process. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] Figure 1 It is a perspective view of the lithium ion secondary battery according to the present embodiment. Figure 2 It is a schematic diagram showing the structure of a laminate of electrode bodies of a lithium ion secondary battery. Figure 3 It is a schematic diagram showing the structure of a wound body of an electrode body of a lithium ion secondary battery. Figure 4 It is a schematic diagram showing the structure of the end portion of the electrode body viewed from the width direction. Figure 5 This is a graph showing the relationship between the wound body shaping load PL [MPa] and the resistance increase rate [%] according to the present embodiment. Figure 6 This is a flowchart showing an example of a method for manufacturing a lithium ion secondary battery according to the present embodiment. Figure 7 1 is a flowchart showing an initial process of the lithium ion secondary battery according to the present embodiment. Figure 8 The positive electrode density change ΔPD [g / cm 3 ] of formula 1. Fig. 9 is the positive electrode density change ΔPD [g / cm 3 ] and the winding body shaping load PL [MPa]. Fig.10 The graph shows the relationship between the winding body shaping load PL [MPa] and the positive electrode density change ΔPD [g / cm 3 ] is a diagram of the relationship between . DETAILED DESCRIPTION

[0014] The following reference Figures 1 to 10 The method for producing an electrode body for a nonaqueous electrolyte secondary battery and the method for producing a nonaqueous electrolyte secondary battery of the present disclosure will be described by way of an embodiment of a method for producing a lithium ion secondary battery 1 .

[0015] <Overview of this Embodiment> Figure 1 It is a perspective view of the lithium ion secondary battery 1 according to the present embodiment. Figure 2 Schematic diagram showing the structure of a laminate of electrode bodies 10 of the lithium ion secondary battery 1 according to the present embodiment. Figure 31 is a schematic diagram showing the structure of a wound body of the electrode body 10 of the lithium ion secondary battery 1 . Figure 4 Schematic diagram showing a winding body pressing process of the electrode body 10 .

[0016] As described in the background art, in the past, in the winding pressing process, when the winding body of the electrode body 10 is pressed into a flat shape, if the pressing load for compressing the electrode body is simply increased, the pores of the separator 120 will be flattened, causing an increase in resistance. To address such a problem, in the inventions described in Patent Documents 1 and 2 of the prior art, heat treatment is performed to soften the electrode body to improve formability.

[0017] However, heating equipment is required to heat the electrode body 10, which leads to a problem of increasing equipment cost. In addition, heating and cooling of the electrode body deteriorate the production cycle and reduce production efficiency.

[0018] In this embodiment, the thickness A [μm] of the positive electrode plate 110 after the positive electrode coating step, the positive electrode unit area weight B [mg / cm ] of the positive electrode composite material layer 112 (positive electrode composite material paste) applied in the positive electrode coating step, and the positive electrode weight per unit area B [mg / cm ] of the positive electrode composite material layer 112 (positive electrode composite material paste) applied in the positive electrode coating step are calculated without such a heat treatment. 2 ], the thickness C [μm] of the positive electrode plate 110 after the positive electrode pressing step is adjusted so that the winding body pressing step is performed without destroying the pores of the separator 120 ( Figure 6 :S4).

[0019] In order to determine the thickness A [μm] of the positive electrode plate 110 after the positive electrode coating step ( S4 ), the positive electrode weight per unit area B [mg / cm ] of the positive electrode composite material layer 112 (positive electrode composite material paste) applied in the positive electrode coating step, 2 ], the thickness C [μm] of the positive electrode plate 110 after the positive electrode pressing step is adjusted to determine the “winding body shaping load PL [MPa]”. The “winding body shaping load PL [MPa]” is set to the winding body pressing step ( S4 ) when the difference ΔT between the thickness T1 [mm] of the electrode body 10 (which is the thickness of the electrode body 10 when the electrode body 10 is pressurized at 1.2 [MPa] after the winding body pressing step) and the thickness T2 [mm] of the electrode body (which is the thickness of the electrode body when the electrode body 10 is pressurized at 0.03 [MPa] after the winding body pressing step) is less than 0.4 [mm]. Figure 6:S4) load. For example, the two electrode bodies 10 after the winding body pressing step (S4) are pressurized at 1.2 [MPa] and 0.03 [MPa], respectively, and these thicknesses T1 [mm] and thickness T2 [mm] are measured, respectively. In other words, when the electrode body 10 is pressed with the winding body shaping load PL [MPa] in the winding body pressing step (S4), the difference ΔT between the thickness T1 [mm] of the electrode body 10 (which is the thickness when the electrode body 10 is pressurized at 1.2 [MPa] after the winding body pressing step (S4)) and the thickness T2 [mm] of the electrode body 10 (which is the thickness when the electrode body 10 is pressurized at 0.03 [MPa] after the winding body pressing step (S4)) is less than 0.4 [mm].

[0020] Figure 5 This is a graph showing the relationship between the wound body shaping load PL [MPa] and the resistance increase rate [%] according to the present embodiment. Figure 5 The horizontal axis is the winding body shaping load PL [MPa], and the vertical axis is the resistance increase rate [%]. The "resistance increase rate [%]" here refers to the resistance increase rate [%] of the internal resistance of the lithium ion secondary battery 1. If the pores of the separator 120 are flattened, the lithium ions Li + It is difficult to pass through the separator 120, so the internal resistance increases. Therefore, if the internal resistance increases, it can be inferred that the winding body pressing process ( Figure 6 :The pores in S4) have been flattened.

[0021] According to this figure, it can be inferred that if the winding body shaping load PL is greater than 11.0 [MPa], the winding body pressing process ( Figure 6 The inventors have found through experiments that, at this time, by making the winding body shaping load PL [MPa] less than 11 [MPa], the winding body pressing process can be performed at room temperature without damaging the pores (S4) of the separator 120.

[0022] Specifically, using Figure 8 The formula (1) shown in FIG. 1 is used to calculate the thickness of the positive electrode plate 110 after the positive electrode coating step, which is A [μm], and the positive electrode weight per unit area is B [mg / cm 2 ], the positive electrode density change ΔPD [g / cm 3 At this time, the thickness A [μm] and the positive electrode unit area weight B [mg / cm 2 ], the thickness C [μm] of the positive electrode plate 110 after the positive electrode pressing process, and the thickness D [μm] of the positive electrode collector foil are adjusted so that the positive electrode density change ΔPD is 1.0 [g / cm3 ] or less. In addition, the thickness A [μm] and the positive electrode unit area weight B [mg / cm 2 ], the thickness C [μm] of the positive electrode plate 110 after the positive electrode pressing process, and the thickness D [μm] of the positive electrode collector foil are adjusted so that the positive electrode density change ΔPD is 0.63 [g / cm 3 By adjusting in this way, the winding body shaping load PL [MPa] can be easily adjusted to 11 [MPa] or less.

[0023] <Lithium Ion Secondary Battery 1 of the Present Embodiment> First, the configuration of the lithium ion secondary battery 1 which is a premise of the present embodiment will be briefly described. Figure 1 1 is a perspective view of a lithium-ion secondary battery 1. Figure 1 As shown, the lithium-ion secondary battery 1 is constructed in the form of a unit cell. The lithium-ion secondary battery 1 includes a rectangular parallelepiped battery case 11 having an opening on the upper side. The battery case 11 includes a cover 12 that seals the opening of the battery case 11. An electrode body (a flat wound electrode body) 10 is accommodated in the battery case 11. The battery case 11 is filled with a non-aqueous electrolyte 17. The battery case 11 and the cover 12 are made of metal such as an aluminum alloy. In the lithium-ion secondary battery 1, a sealed battery cell is formed by installing the cover 12 on the battery case 11. In addition, in the lithium-ion secondary battery 1, the cover 12 includes a negative electrode external terminal 14 and a positive electrode external terminal 16 for charging and discharging electric power. The negative electrode external terminal 14 is connected to the negative electrode connecting portion 103 (see Figure 2 ) is connected to the negative electrode current collector 13 through the cover 12. The positive electrode external terminal 16 is connected to the positive electrode connecting portion 113 (see Figure 2 ) are connected via the cover 12 using the positive electrode collector 15.

[0024] <Electrode Body 10> Figure 2 Schematic diagram showing the structure of a laminate of an electrode body 10 of a lithium-ion secondary battery 1. Figure 2 As shown, the electrode body 10 of the lithium ion secondary battery 1 includes a negative electrode plate 100, a positive electrode plate 110 and a separator 120. The negative electrode plate 100 includes a negative electrode composite material layer 102 on both sides of the negative electrode collector foil 101. The positive electrode plate 110 includes a positive electrode composite material layer 112 on both sides of the positive electrode collector foil 111. The negative electrode plate 100 and the positive electrode plate 110 are overlapped with the separator 120 to form a laminated electrode body (laminated body) 10. The laminate is wound along the length direction Z with the winding axis as the center and shaped into a flat shape to form an electrode body (flat wound electrode body) 10.

[0025] The negative electrode connection portion 103 functions as a current collector for extracting power from the negative electrode mixture layer 102 of the negative electrode plate 100 . The positive electrode connection portion 113 functions as a current collector for extracting power from the positive electrode mixture layer 112 of the positive electrode plate 110 .

[0026] <End Structure of Electrode Body 10> Figure 3 1 is a perspective view showing the end of the negative electrode side in the width direction of the wound electrode body 10. Figure 6 The electrode body 10 which has been layered in the winding step ( Figure 6 : S3) in which the portion of the center Ct is wound around the winding axis. Next, in the winding body pressing step ( Figure 6 : S4), a pair of opposing presses 2 (refer to Figure 4 ) The wound electrode body 10 is shaped so that the end portion viewed in the width direction W becomes a flat shape like a competitive track. Figure 1 As shown, the flat electrode body 10 is housed in the battery case 11, and the negative electrode collector 13 is welded to the negative electrode connection portion 103. The positive electrode collector 15 is welded to the positive electrode connection portion 113. As a welding method for the connection portion and the collector, there are, for example, ultrasonic welding, resistance welding, and electric welding. After that, the negative electrode external terminal 14 is connected to the negative electrode collector 13 through the cover 12, and the positive electrode external terminal 16 is connected to the positive electrode collector 15.

[0027] Here, the direction parallel to the winding axis of the electrode body 10 is referred to as the “width direction W”. In addition, the direction perpendicular to the winding axis of the electrode body 10 and perpendicular to the surface of the flat portion F is referred to as the “thickness direction T”. In addition, the direction perpendicular to the width direction W and the thickness direction T is referred to as the “length direction Z”.

[0028] <Flat portion F and curved portion R> Figure 4 1 is a schematic diagram showing the structure of the end of the electrode body 10 viewed from the width direction W. In the wound body of the electrode body 10, the negative electrode plate 100 and the positive electrode plate 110 are repeatedly stacked with the separator 120 interposed therebetween. The central portion of the electrode body 10 pressed into a flat shape is a straight line, and a planar "flat portion F" (see FIG. 1 ) is formed by the negative electrode plate 100, the positive electrode plate 110 and the separator 120. Figure 3 ).

[0029] In addition, in the flat part F Figure 3 The upper and lower ends shown in FIG. 1 are formed by bending the electrode body 10 composed of the stacked negative electrode plate 100, the positive electrode plate 110, and the separator 120 into a semi-cylindrical shape to form a bent portion R (see FIG. 1 ). Figure 3). The stacked layers of the curved portion R are roughly concentric semicircular when viewed from the width direction W, and the position of the center of these semicircles is referred to as the "center Ct". The center Ct can be assumed to be a straight line continuous along the width direction W.

[0030] <Negative Electrode Plate 100> In the negative electrode plate 100, a negative electrode composite material layer 102 is formed on both sides of a negative electrode collector foil 101. In the embodiment, the negative electrode collector foil 101 is composed of Cu foil. The negative electrode collector foil 101 constitutes the basis of the aggregate of the negative electrode composite material layer 102, and has the function of a collector component that collects electricity from the negative electrode composite material layer 102. In the negative electrode plate 100, the negative electrode composite material layer 102 is formed on the negative electrode collector foil 101 made of metal. In the first embodiment, the negative electrode active material is a material that can absorb and release lithium ions, and a powdered carbon material composed of graphite (black lead) or the like is used.

[0031] In manufacturing the negative electrode plate 100, first, for example, a negative electrode active material, a solvent, and a binder (adhesive) are kneaded to prepare a negative electrode composite material paste ( Figure 7 : S21). The prepared negative electrode composite material paste is applied to the negative electrode collector foil 101 ( Figure 7 :S22), drying is performed in a drying process ( Figure 7 : S23). Then, the negative electrode plate 100 is subjected to a negative electrode pressing process ( Figure 7 : S24) is made into specified thickness and density.

[0032] <Positive Electrode Plate 110> The positive electrode plate 110 is formed by forming a positive electrode composite material layer 112 on both sides of the positive electrode collector foil 111. In the embodiment, the positive electrode collector foil 111 is composed of Al foil or Al alloy foil. The positive electrode collector foil 111 constitutes the basis of the aggregate of the positive electrode composite material layer 112 and has the function of a collector that collects electricity from the positive electrode composite material layer 112.

[0033] In the positive electrode plate 110, a positive electrode composite material layer 112 is formed on the surface of the positive electrode collector foil 111. The positive electrode composite material layer 112 has a positive electrode active material. The positive electrode active material is a material that can absorb and release lithium, and for example, lithium cobalt oxide (LiCoO2), lithium manganese oxide (LiMn2O4), lithium nickel oxide (LiNiO2) and the like can be used. In addition, a material obtained by mixing LiCoO2, LiMn2O4, and LiNiO2 in an arbitrary ratio can also be used.

[0034] In addition, the positive electrode composite material layer 112 includes a conductive material. As the conductive material, carbon black such as acetylene black (AB) and Ketjen black, and graphite (black lead) can be used. In this embodiment, in order to reduce the positive electrode unit area weight B [mg / cm2 ], using highly conductive carbon nanotubes, carbon nanofibers, etc. As a result, the amount of addition used to obtain the same degree of conductivity is small, and the solid content rate of the positive electrode composite material paste can be reduced.

[0035] In manufacturing the positive electrode plate 110, first, for example, a positive electrode active material, a conductive material, a solvent, and a binder (adhesive) are kneaded to prepare a positive electrode composite material paste ( Figure 7 : S11). The mixed positive electrode composite material paste is applied to the positive electrode collector foil 111 ( Figure 7 :S12). Then drying is performed ( Figure 7 : S13). Finally, the positive electrode plate 110 is subjected to a positive electrode pressing process ( Figure 7 :S14) made into specified thickness and density.

[0036] <Spacer 120> The separator 120 is a highly insulating nonwoven fabric made of polypropylene or the like, which is a porous resin for retaining the nonaqueous electrolyte 17 between the negative electrode plate 100 and the positive electrode plate 110. In addition, a porous polymer film such as a porous polyethylene film, a porous polyolefin film, and a porous polyvinyl chloride film, or a lithium ion or ion conductive polymer electrolyte film may be used alone or in combination as the separator 120. When the electrode body 10 is immersed in the nonaqueous electrolyte 17, the nonaqueous electrolyte 17 penetrates from the end of the separator 120 toward the center.

[0037] The resin separator 120 has a certain elasticity, even in the winding body pressing process ( Figure 6 :S4) Such temporary extrusion pressure will restore the original thickness as soon as the extrusion pressure disappears. However, if the extrusion pressure exceeds a certain level (11 [MPa] in this embodiment), the material will undergo plastic deformation, the flattened pores will not return to their original size, the porosity [%] will decrease, and the lithium ion Li + The movement of is suppressed. Therefore, the internal resistance increases irreversibly.

[0038] In the method for manufacturing the separator 120 , a porous sheet is stretched in the longitudinal direction and the width direction to adjust the size of the pores, thereby making the porosity a target value. The separator 120 may be a single layer or may be composed of multiple layers. In this embodiment, the core sheet is made of a porous sheet of polyethylene. When heated to high temperatures, the core sheet dissolves and closes the pores, thereby preventing lithium ions Li + In addition, by using polypropylene porous sheets with high mechanical strength, heat resistance and corrosion resistance to form both sides of the core sheet, micro short circuits can be suppressed.

[0039] <Method for Manufacturing Lithium Ion Secondary Battery 1> Figure 6 1 is a flowchart showing an example of a method for manufacturing a lithium-ion secondary battery 1 according to the present embodiment. Regarding the lithium-ion secondary battery 1 as a unit cell, first, in an initial step (S1), a negative electrode plate 100, a positive electrode plate 110, and a separator 120 as power generation elements are respectively manufactured. Regarding the initial step (S1), the following is based on Figure 7 In the initial step (S1), after the negative electrode plate 100, the positive electrode plate 110, and the separator 120 are separately manufactured, the negative electrode plate 100 and the positive electrode plate 110 are overlapped with the separator 120 in the lamination step (S2) to be integrated. In the winding step (S3), as shown in FIG. Figure 2 As shown in FIG. 1 , the laminated body thus prepared is wound along the length direction Z. When winding, Figure 3 When viewed in the width direction W shown in FIG. 1 , the laminate is roughly in the shape of a track for land sports. In the winding step (S3), the wound laminate is roughly in the shape of a plate. In the winding pressing step (S4), as shown in FIG. Figure 4 As shown in FIG. 1 , such a wound body is pressed by a pair of pressing surfaces 2a of a pair of opposing press machines 2 in the thickness direction T indicated by the arrow. In the wound body pressing step (S4), in order to accommodate the electrode body 10 without gaps, Figure 1 In the battery case 11 shown in FIG. 1 , the electrode body 10 is pressed until it reaches a predetermined thickness [mm]. At this time, the winding body shaping load PL [kN] is determined by the positive electrode composite material paste preparation step ( Figure 7 : The positive electrode weight per unit area B [mg / cm 2 ], the thickness A [μm] of the positive electrode plate 110 after the positive electrode coating step (S12), the thickness C [μm] of the positive electrode plate 110 after the positive electrode pressing step (S14), etc.

[0040] In the winding body pressing step (S4), after adjusting the thickness of the electrode body 10, the assembling step (S5) is performed. In the assembling step (S5), Figure 1 As shown, the negative electrode collector 13 and the positive electrode collector 15 are installed on the electrode body 10, and the negative electrode external terminal 14 and the positive electrode external terminal 16 are further installed with the help of the cover body 12. The electrode body 10 is then housed in the battery shell 11. The cover body 12 is then welded to the battery shell 11, thereby sealing the opening. At this stage, the liquid injection port 18 of the cover body 12 is open, so the battery cell is heated by the battery cell drying process (S6) to dry the inside of the battery cell. After the battery cell is dried by the battery cell drying process (S6), the non-aqueous electrolyte 17 is injected by the liquid injection and sealing process (S7), and the liquid injection port 18 is sealed and sealed. The above completes the assembly of the lithium-ion secondary battery 1.

[0041] Thereafter, the SEI film is formed by the initial charge of the lithium ion secondary battery 1 in the activation step (S8). In the aging step, the lithium ion secondary battery 1 is stored at a high temperature for a long period of time to eliminate micro short circuits. After the activation step ( S8 ) is completed, the battery capacity, internal resistance, self-discharge, OCV, etc. of the lithium ion secondary battery 1 are inspected in the inspection step ( S9 ), and qualified lithium ion secondary batteries 1 are shipped as products.

[0042] <Initial Step (S1)> Figure 7 1 is a flowchart showing an initial step ( S1 ) of the lithium ion secondary battery 1 according to the present embodiment.

[0043] The initial step ( S1 ) is a step of manufacturing the negative electrode plate 100 , the positive electrode plate 110 , and the separator 120 , which are power generation elements. In the positive electrode composite material paste preparation step ( S11 ), a positive electrode active material, a conductive material, a solvent, and a binder (binder) are kneaded to prepare a positive electrode composite material paste.

[0044] In this embodiment, the thickness A [μm] and the positive electrode unit area weight B [mg / cm ] of the positive electrode plate 110 after the positive electrode coating step ( S12 ) are adjusted according to the formulation in the positive electrode composite material paste preparation step ( S11 ). 2 ], the thickness C [μm] of the positive electrode plate 110 after positive electrode pressing, etc. are adjusted, thereby changing the winding body shaping load PL [kN].

[0045] Regarding the adjustment of the thickness A [μm] of the positive electrode plate 110 after the positive electrode coating step (S12), the thickness A [μm] can be increased by, for example, increasing the amount of solvent mixed. In addition, from the perspective of the relationship between the positive electrode active material and the battery capacity of the positive electrode, it is necessary to make the positive electrode unit area weight B [mg / cm 2 ] is a certain amount. Therefore, if the conductive material is, for example, carbon nanotubes, its mass can be smaller than that of carbon particles due to its shape and conductivity. Therefore, the solid content rate of the positive electrode composite material paste can be reduced, and the positive electrode unit area weight B [mg / cm 2 ].

[0046] In the positive electrode coating step ( S12 ), by adjusting the formulation of the positive electrode composite material paste in this manner, the thickness A [μm] of the positive electrode plate 110 after the positive electrode coating step ( S12 ) is adjusted. After the positive electrode coating step (S12), the positive electrode composite material layer 112 is dried in a drying step (S13) to volatilize volatile components such as the solvent, thereby solidifying the positive electrode composite material layer 112. The positive electrode plate 110 dried in the drying step (S13) is shaped and pressed in a positive electrode pressing step (S14) to a predetermined thickness.

[0047] In the initial step (S1), the negative electrode plate 100 is manufactured in parallel with the manufacture of the positive electrode plate 110. Although not described in detail here, the negative electrode plate 100 is manufactured through a negative electrode composite material paste preparation step (S21), a negative electrode coating step (S22), a drying step (S23), and a negative electrode pressing step (S24).

[0048] Although detailed description is omitted, the separator 120 is manufactured in parallel with the manufacture of the positive electrode plate 110 through the separator manufacturing step ( S31 ). In the above initial process ( Figure 6 : In S1), the negative electrode plate 100, the positive electrode plate 110, and the separator 120, which are power generation elements of the lithium ion secondary battery 1, are manufactured respectively.

[0049] <Lamination Step (S2)> The negative electrode plate 100, the positive electrode plate 110, and the separator 120 manufactured in the initial step (S1) as described above are Figure 2 , Figure 4 As shown, the negative electrode plate 100, the separator 120, the positive electrode plate 110, and the separator 120 are stacked in this order.

[0050] <Winding Step (S3)> The negative electrode plate 100, the positive electrode plate 110, and the separator 120 which have been laminated in the lamination step (S2) are as follows: Figure 2 , Figure 3 Winding is performed as shown.

[0051] <Wound body pressing step (S4)> In the winding body pressing step (S4), as Figure 4 As shown, the wound body of the electrode body 10 is pressed in the thickness direction T by the pressing surface 2 a of the press machine 2 .

[0052] Here, the load of the winding pressing step (S4) when the difference ΔT between the thickness T1 [mm] of the electrode body 10 (which is the thickness of the electrode body 10 when the electrode body 10 is pressurized at 1.2 [MPa] after the winding pressing step (S4)) and the thickness T2 [mm] of the electrode body 10 (which is the thickness of the electrode body 10 when the electrode body 10 is pressurized at 0.03 [MPa] after the winding pressing step (S4)) is less than 0.4 [mm] is set as the winding shaping load PL [MPa].

[0053] The thickness A [μm] and the positive electrode unit area weight B [mg / cm 2 ] and the thickness C [μm] of the positive electrode plate 110 after the positive electrode pressing step is adjusted so that the winding body shaping load PL [MPa] is less than 11 [MPa].

[0054] Here, in the present embodiment, the thickness of the positive electrode plate 110 after the positive electrode coating step ( S12 ) is denoted as A [μm], and the positive electrode unit area weight is denoted as B [mg / cm 2 ], the thickness of the positive electrode plate 110 after the positive electrode pressing step is set to C [μm], and the thickness of the positive electrode collector foil is set to D [μm]. Figure 8 The positive electrode density change ΔPD [g / cm 3 ], the thickness A [μm] and the positive electrode unit area weight B [mg / cm 2 ], the thickness C [μm] of the positive electrode plate 110 after the positive electrode pressing process, and the thickness D [μm] of the positive electrode collector foil are adjusted so that the positive electrode density change ΔPD is 1.0 [g / cm 3 By adjusting in this way, in the winding body pressing step (S4), the winding body shaping load PL [MPa] can be made 11 [MPa] or less.

[0055] It should be noted that the thickness A [μm] and the positive electrode unit area weight B [mg / cm 2 ], the thickness C [μm] of the positive electrode plate 110 after the positive electrode pressing process, and the thickness D [μm] of the positive electrode collector foil are adjusted so that the positive electrode density change ΔPD is 0.63 [g / cm 3 This is because, by adjusting in this way, the particles of the positive electrode active material and the conductive material are closely attached to each other, and the contact resistance between them can be reduced.

[0056] (Function of this embodiment) like Figure 4As shown, in the winding body pressing process ( Figure 6 :S4) When the winding body of the electrode body 10 is pressed by a pair of pressing surfaces 2a, 2a of the press machine 2, the reaction force characteristics of the positive electrode plate 110 dominate the formability. The separator 120 is made of porous polyolefins such as polyethylene (PE) and polypropylene (PP) and has a certain elasticity. However, if it is subjected to a greater pressure exceeding a certain pressure, it will irreversibly undergo plastic deformation. Once plastic deformation occurs, the pores are flattened, the water permeability is deteriorated, and the lithium ion Li + Therefore, it has an adverse effect on battery performance.

[0057] Therefore, the present inventors have found through experiments that by setting the roll shaping load PL [MPa] to 11 [MPa] or less, the roll pressing step can be performed at room temperature without damaging the pores of the separator 120 .

[0058] The inventors have found that in order to reduce the winding body shaping load PL [MPa] to 11 [MPa] or less, the positive electrode density change ΔPD [g / cm 3 ] is 1.0[g / cm 3 ] to achieve this.

[0059] Therefore, it is necessary to prove that the positive electrode density change ΔPD [g / cm 3 ] is 1.0[g / cm 3 ] or less. Therefore, the thickness A [μm] of the positive electrode plate 110 after positive electrode coating, the positive electrode unit area weight B [mg / cm 2 ], the thickness C [μm] of the positive electrode plate 110 after the positive electrode pressing process, the thickness D [μm] of the positive electrode collector foil, and the change in positive electrode density ΔPD [g / cm 3 ] to carry out the following experiment.

[0060] <Experimental example> Here, an experimental example of this embodiment is shown. Fig. 9 This is a table showing the test results of Examples and Comparative Examples of the present embodiment. In the experiment, the following items were measured for the "Comparative Example" and "Examples 1 to 4".

[0061] First, the thickness D [μm] of the positive electrode current collector foil 111 was measured in advance. It should be noted that a common positive electrode current collector foil was used for the positive electrode current collector foil 111, and the thickness D was 12.00 [μm]. Next, a positive electrode composite material paste preparation step (S11) is used to prepare a positive electrode composite material paste of a predetermined formula. Next, a positive electrode coating step (S12) is used to coat the positive electrode composite material paste with a predetermined positive electrode unit area weight B [mg / cm 2] is applied to the positive electrode collector foil 111. Here, the thickness A [μm] of the positive electrode plate 110 after the positive electrode coating is measured. Thereafter, the positive electrode composite material layer 112 is dried, and a positive electrode pressing step (S14) is performed. Thereafter, the thickness C [μm] of the positive electrode plate 110 after the positive electrode pressing is measured.

[0062] Here, the thickness of the positive electrode plate 110 after the positive electrode coating step ( S12 ) is represented by A [μm]. The positive electrode unit area weight is represented by B [mg / cm 2 ]. The thickness of the positive electrode plate 110 after the positive electrode pressing step (S14) is denoted as C [μm]. The thickness of the positive electrode collector foil 111 is denoted as D [μm]. Figure 8 The positive electrode density change ΔPD [g / cm 3 Here, the numerator on the right is multiplied by 10 to make the units consistent.

[0063] Then, the "Comparative Example" and "Examples 1 to 5" were compared. <Experimental conditions> Comparative Example: The thickness A of the positive electrode plate 110 after positive electrode coating is 86.1 [μm], and the positive electrode unit area weight B is 11.33 [mg / cm 2 ], the thickness C of the positive electrode plate 110 after the positive electrode pressing process is 53.5 [μm], and the thickness D of the positive electrode collector foil is 12.00 [μm]. When the positive electrode density change ΔPD is calculated by the above (Formula 1), the change ΔPD is 1.20 [g / cm 3 ]. In addition, the winding body shaping load PL at this time was 13.0 [MPa].

[0064] Embodiment 1: The thickness A of the positive electrode plate 110 after positive electrode coating is 79.1 [μm], and the positive electrode unit area weight B is 11.15 [mg / cm 2 ], the thickness C of the positive electrode plate 110 after the positive electrode pressing process is 55.5 [μm], and the thickness D of the positive electrode collector foil is 12.00 [μm]. When the positive electrode density change ΔPD is calculated by the above (Formula 1), the change ΔPD is 0.90 [g / cm 3 ]. In addition, the winding body shaping load PL at this time was 9.7 [MPa].

[0065] Embodiment 2: The thickness A of the positive electrode plate 110 after positive electrode coating is 75.5 [μm], and the positive electrode unit area weight B is 11.11 [mg / cm 2], the thickness C of the positive electrode plate 110 after the positive electrode pressing process is 58.0 [μm], and the thickness D of the positive electrode collector foil is 12.00 [μm]. When the positive electrode density change ΔPD is calculated by the above (Formula 1), the change ΔPD is 0.67 [g / cm 3 ]. In addition, the winding body shaping load PL at this time was 7.7 [MPa].

[0066] Embodiment 3: The thickness A of the positive electrode plate 110 after positive electrode coating is 82.6 [μm], and the positive electrode unit area weight B is 11.10 [mg / cm 2 ], the thickness C of the positive electrode plate 110 after the positive electrode pressing process is 55.4 [μm], and the thickness D of the positive electrode collector foil is 12.00 [μm]. When the positive electrode density change ΔPD is calculated by the above (Formula 1), the change ΔPD is 1.00 [g / cm 3 ]. In addition, the winding body shaping load PL at this time was 11.0 [MPa].

[0067] Embodiment 4: The thickness A of the positive electrode plate 110 after positive electrode coating is 74.4 [μm], and the positive electrode unit area weight B is 11.03 [mg / cm 2 ], the thickness C of the positive electrode plate 110 after the positive electrode pressing process is 58.0 [μm], and the thickness D of the positive electrode collector foil is 12.00 [μm]. When the positive electrode density change ΔPD is calculated by the above (Formula 1), the change ΔPD is 0.63 [g / cm 3 ]. In addition, the winding body shaping load PL at this time was 6.9 [MPa].

[0068] <Experimental Summary> like Figure 4 As shown, in the winding body pressing process ( Figure 6 :S4) When the pair of pressing surfaces 2a, 2a of the press machine 2 are used to press the winding body of the electrode body 10, the reaction force characteristics of the positive electrode plate 110 dominate the formability. The separator 120 is made of porous polyolefins such as polyethylene (PE) and polypropylene (PP) and has a certain elasticity. However, if it is subjected to a certain pressure, it will undergo plastic deformation. Once plastic deformation occurs, the pores are flattened, the water permeability is deteriorated, and the lithium ion Li + The circulation of lithium ions is deteriorated. Therefore, it has an adverse effect on battery performance. The inventors have confirmed through experiments that if the winding body shaping load PL [MPa] is set to 11 [MPa] or less, the plastic deformation of the separator 120 can be avoided, the pores will not be flattened, and the lithium ion Li can be smoothly transferred. + exchange.

[0069] Therefore, the inventors set 11 [MPa] as the reference threshold PLth, and set the winding body shaping load PL [MPa] to be 11 [MPa] or less of the threshold PLth [MPa]. Based on this analysis, it was found that the winding body pressing process can be performed at room temperature in a manner that does not damage the pores of the separator 120 ( Figure 6 :S4) conditions.

[0070] <Experimental Results> According to the experimental results, in the "Comparative Example", the winding body shaping load PL is 13.0 [MPa], which exceeds the threshold PLth [MPa], so it can be seen that the plastic deformation of the separator 120 cannot be avoided. On the other hand, in "Example 1" to "Example 4", the winding body shaping load PL is 6.9 to 11.0 [MPa], which does not exceed the threshold PLth [MPa], so it can be seen that the plastic deformation of the separator 120 can be avoided.

[0071] As the conditions, the positive electrode density change ΔPD of the "Comparative Example" is 1.20, and the positive electrode density change ΔPD of "Example 1" to "Example 4" is 0.63 to 1.00 [g / cm 3 ]. The results show that by setting the positive electrode density change ΔPD to 1.00 [g / cm 3 ] or less, the winding body shaping load PL [MPa] can be made less than 11 [MPa] which is the reference threshold value PLth.

[0072] That is, the thickness A [μm] of the positive electrode after coating and the positive electrode unit area weight B [mg / cm 2 ], the value of the thickness C [μm] after the positive electrode pressing process makes the positive electrode density change ΔPD 1.00 [g / cm 3 Based on this, the winding body shaping load PL [MPa] can be easily made less than 11 [MPa] of the threshold value PLth [MPa].

[0073] In addition, the thickness of the positive electrode after coating A [μm], the positive electrode unit area weight B [mg / cm 2 ] The specific value of the thickness C [μm] after the positive electrode pressing process is as follows. It was found that by setting the thickness A of the positive electrode after coating to 74.4 to 82.6 [μm], the winding body shaping load PL [MPa] can be set to 11 [MPa] or less, which is the reference threshold value PLth.

[0074] It was also found that by setting the positive electrode unit area weight B to 11.03 to 11.15 [mg / cm 2 ], the winding body shaping load PL [MPa] can be reduced to 11 [MPa] or less, which is the reference threshold value PLth.

[0075] It was also found that by setting the thickness C of the positive electrode after the pressing step to 55.4 to 58.0 [μm], the winding body shaping load PL [MPa] can be set to 11 [MPa] or less, which is the reference threshold value PLth.

[0076] <Function of this embodiment> Fig.10 is the positive electrode density change ΔPD [g / cm 3 ] and the winding body shaping load PL [MPa]. The horizontal axis is the positive electrode density change ΔPD [g / cm 3 ], the vertical axis uses the winding body shaping load PL [MPa], and the experimental results are plotted into a graph to show their relationship. From this graph, it can be seen that the positive electrode density change ΔPD [g / cm 3 ] has a strong positive correlation with the winding body shaping load PL [MPa]. Therefore, it can be confirmed that in order to make the winding body shaping load PL [MPa] less than 11 [MPa] as the plastic deformation load of the separator 120, the positive electrode density change ΔPD is 1.0 [g / cm 3 ] and the following will do.

[0077] (Effects of this embodiment) (1) According to the method for manufacturing the lithium ion secondary battery 1 of the present embodiment, there is an effect of being able to suppress excessive plastic deformation of the spacer 120 during pressing of the electrode body 10 by a simple process.

[0078] (2) After the winding body pressing step (S4), the thickness A [μm] and the positive electrode unit area weight B [mg / cm 2 ], the thickness C [μm] of the positive electrode plate 110 after the positive electrode pressing process is adjusted so that the winding body shaping load PL [MPa] is less than 11 [MPa]. Therefore, in the winding body pressing process, the lithium ion Li + The effect of mobile resistance.

[0079] (3) The thickness of the positive electrode plate 110 after the positive electrode coating step (S12) is denoted as A [μm], and the positive electrode unit area weight is denoted as B [mg / cm 2 ], the thickness of the positive electrode plate 110 after the positive electrode pressing step (S14) is set to C [μm], and the thickness of the positive electrode collector foil 111 is set to D [μm]. Figure 8 The positive electrode density change ΔPD [g / cm 3 In this case, the values ​​A[μm], B[mg / cm2 ], C[μm], and D[μm] were adjusted so that the positive electrode density change ΔPD was 1.0[g / cm 3 ] or less. This has the effect of being able to easily adjust the winding body shaping load PL [MPa] to be 11 [MPa] or less.

[0080] (4) In addition, the positive electrode density change ΔPD was adjusted to 0.63 [g / cm 3 By adjusting in this way, the particles of the positive electrode active material and the conductive material are closely attached to each other, and the contact resistance between them can be reduced.

[0081] (5) In the present embodiment, the winding body shaping load PL [MPa] can be set to 11 [MPa] or less at room temperature without heating. Therefore, there is an effect that it can be implemented with simple equipment.

[0082] (6) Furthermore, since the time required for heating is not required, the production cycle time can be shortened and the production efficiency can be improved. (7) The positive electrode composite material layer 112 of this embodiment includes a conductor, which is a carbon nanotube. Carbon nanotubes have high conductivity and are fibrous in shape, so the amount of conductive material added as a conductive material forming a conductive network can be small, which can reduce the density of the positive electrode composite material layer 112. Therefore, it is easy to mix the positive electrode composite material paste.

[0083] (8) The production method of the present embodiment has the effect of being able to be appropriately implemented in the lithium ion secondary battery 1 . (Variation Example) The above embodiment is an example of the present invention, and can be implemented in the following modified forms.

[0084] In the present embodiment, the lithium ion secondary battery 1 as a plate-shaped unit cell for vehicle use is exemplified as an example of the nonaqueous electrolyte secondary battery, but the present invention is not limited thereto and can be implemented in other applications such as stationary use.

[0085] The drawings are used for explaining the present embodiment, and numerical values ​​may be omitted or dimensional balance may be exaggerated for easy understanding, and the drawings are not limited to these.

[0086] · Figure 6 , Figure 7 The flowchart shown is an example of the present invention, and the present invention can be implemented by adding, deleting, changing the order, or replacing the steps. Various numerical values ​​and ranges are merely examples and can be implemented by those skilled in the art through optimization.

[0087] The composition of the positive electrode composite material paste, the properties of the material, etc. are merely examples of the present invention and can be optimized and implemented by those skilled in the art. The present embodiment is one embodiment of the present invention and is not limited to the embodiment unless it deviates from the claims. It is obvious that the present invention can be implemented by adding, deleting or changing the configuration thereof by a person skilled in the art. The present disclosure includes the following embodiments. It should be noted that reference numerals representing components of the above-described embodiments are used simply to facilitate understanding and not to limit the present disclosure. [Note 1] A method for producing a flat wound electrode body (10) for a non-aqueous electrolyte secondary battery (1), comprising: Applying a positive electrode composite material layer (112) to a positive electrode collector foil (111) to produce a positive electrode plate (110); Pressing the manufactured positive electrode plate; The pressed positive electrode plate and the negative electrode plate (100) comprising a negative electrode current collector foil (101) and a negative electrode composite material layer (102) are stacked via a separator (120) made of a porous resin to produce a laminate; Winding the produced laminate to produce a wound electrode body; and The produced wound electrode body is pressed to shape the wound electrode body into a flat shape. When the load for pressing the wound electrode body is defined as the wound body shaping load PL MPa, the thickness of the positive electrode plate A μm, the positive electrode unit area weight B mg / cm2 of the positive electrode composite layer applied, and the positive electrode weight B mg / cm3 of the positive electrode composite layer applied are calculated. 2 , the thickness Cμm of the pressed positive electrode plate is adjusted so that the winding body shaping load PL MPa is less than 11MPa, and in the wound electrode body, the difference ΔT between the thickness T1 mm of the flat wound electrode body when the flat wound electrode body is shaped and pressurized at 1.2MPa and the thickness T2 mm of the flat wound electrode body when the flat wound electrode body is shaped and pressurized at 0.03MPa is less than 0.4mm. [Note 2] A method for producing a flat wound electrode body (10) for a non-aqueous electrolyte secondary battery (1), comprising: Applying a positive electrode composite material layer (112) to a positive electrode collector foil (111) to produce a positive electrode plate (110); Pressing the manufactured positive electrode plate; The pressed positive electrode plate and the negative electrode plate (100) comprising a negative electrode current collector foil (101) and a negative electrode composite material layer (102) are stacked via a separator (120) made of a porous resin to produce a laminate; Winding the produced laminate to produce a wound electrode body; and The produced wound electrode body is pressed to shape the wound electrode body into a flat shape. The thickness of the positive electrode plate is denoted by A μm, and the positive electrode weight per unit area of ​​the positive electrode composite material layer is denoted by B mg / cm 2 , when the thickness of the pressed positive electrode plate is C μm and the thickness of the positive electrode collector foil is D μm, Figure 8 The positive electrode density change ΔPD g / cm is obtained by using the formula (1) shown in 3 hour, The thickness of the positive electrode plate A μm, the weight per unit area of ​​the positive electrode B mg / cm 2 , the thickness C μm of the pressed positive electrode plate, and the thickness D μm of the positive electrode collector foil are adjusted so that the positive electrode density change ΔPD is 1.0 g / cm 3 the following.

Claims

1. A method for manufacturing an electrode body for a non-aqueous electrolyte secondary battery, the non-aqueous electrolyte secondary battery comprising an electrode body, a non-aqueous electrolyte, and a rectangular parallelepiped battery case for accommodating the electrode body and the non-aqueous electrolyte, characterized in that: The above manufacturing method comprises the following steps: A positive electrode coating step, coating the positive electrode composite material layer onto the positive electrode collector foil of the electrode body to produce a positive electrode plate; A positive electrode pressing step, pressing the manufactured positive electrode plate; A lamination step of laminating the pressed positive electrode plate and the negative electrode plate comprising a negative electrode collector foil and a negative electrode composite material layer via a separator made of a porous resin; a winding step of winding the stacked electrode body; and The winding body pressing step is to shape the wound electrode body into a flat shape. The load of the winding body pressing step in which the difference ΔT between the thickness T1 mm and the thickness T2 mm of the electrode body is 0.4 mm or less is set as the winding body shaping load PL MPa, the thickness T1 of the electrode body is the thickness of the electrode body when the electrode body is pressurized at 1.2 MPa after the winding body pressing step, and the thickness T2 of the electrode body is the thickness of the electrode body when the electrode body is pressurized at 0.03 MPa after the winding body pressing step. At this time, The thickness A μm of the positive electrode plate after the positive electrode coating step, the positive electrode unit area weight B mg / cm2 of the positive electrode composite material layer in the positive electrode coating step, 2 The thickness C μm of the positive electrode plate after the positive electrode pressing step is adjusted so that the winding body shaping load PL MPa is 11 MPa or less.

2. The method for producing an electrode body for a non-aqueous electrolyte secondary battery according to claim 1, wherein: In the wound body pressing step, the electrode body is pressed at room temperature without heating the electrode body.

3. The method for producing an electrode body for a non-aqueous electrolyte secondary battery according to claim 1 or 2, characterized in that: The positive electrode composite material layer contains a conductor, and the conductor is a carbon nanotube.

4. The method for producing an electrode body for a non-aqueous electrolyte secondary battery according to claim 1 or 2, wherein: The non-aqueous electrolyte secondary battery is a lithium ion secondary battery. 5 . A method for producing a non-aqueous electrolyte secondary battery, comprising the method for producing an electrode body for a non-aqueous electrolyte secondary battery according to claim 1 .

6. A method for manufacturing an electrode body for a non-aqueous electrolyte secondary battery, the non-aqueous electrolyte secondary battery comprising an electrode body, a non-aqueous electrolyte, and a rectangular parallelepiped battery case for accommodating the electrode body and the non-aqueous electrolyte, characterized in that: The above manufacturing method comprises the following steps: A positive electrode coating step, coating the positive electrode composite material layer onto the positive electrode collector foil of the electrode body to produce a positive electrode plate; A positive electrode pressing step, pressing the manufactured positive electrode plate; A lamination step of laminating the pressed positive electrode plate and the negative electrode plate comprising a negative electrode collector foil and a negative electrode composite material layer via a separator made of a porous resin; a winding step of winding the stacked electrode body; and The winding body pressing step is to shape the wound electrode body into a flat shape. The thickness of the positive electrode plate after the positive electrode coating step is denoted by A μm, and the positive electrode unit area weight of the positive electrode composite material layer in the positive electrode coating step is denoted by B mg / cm 2 , when the thickness of the positive electrode plate after the positive electrode pressing step is set to C μm and the thickness of the positive electrode collector foil is set to D μm, Calculate the change in positive electrode density ΔPD g / cm 3 hour, The thickness A μm and the positive electrode weight B mg / cm 2 , the thickness C μm of the positive electrode plate after the positive electrode pressing step, and the thickness D μm of the positive electrode collector foil are adjusted so that the positive electrode density change ΔPD is 1.0 g / cm 3 the following.

7. The method for producing an electrode body for a non-aqueous electrolyte secondary battery according to claim 6, wherein: The thickness A μm and the positive electrode weight B mg / cm 2 , the thickness C μm of the positive electrode plate after the positive electrode pressing step, and the thickness D μm of the positive electrode collector foil are adjusted so that the positive electrode density change ΔPD is 0.63 g / cm 3 above.

8. The method for producing an electrode body for a non-aqueous electrolyte secondary battery according to claim 6 or 7, characterized in that: In the wound body pressing step, the electrode body is pressed at room temperature without heating the electrode body.

9. The method for producing an electrode body for a non-aqueous electrolyte secondary battery according to claim 6 or 7, characterized in that: The positive electrode composite material layer contains a conductor, and the conductor is a carbon nanotube.

10. The method for producing an electrode body for a non-aqueous electrolyte secondary battery according to claim 6 or 7, characterized in that: The non-aqueous electrolyte secondary battery is a lithium ion secondary battery. 11 . A method for producing a non-aqueous electrolyte secondary battery, comprising the method for producing an electrode body for a non-aqueous electrolyte secondary battery according to claim 6 or 7 .

Citation Information

Patent Citations

  • Electrode group for flat-type secondary battery and flat-type secondary battery using the same

    JP2012059491A

  • Method for manufacturing battery with flat electrode body

    JP2013206587A