Carbon-coated aluminum foil water-based adhesive as well as preparation method and application thereof

The aqueous adhesive prepared by copolymerization of monomers such as acrylic acid, 2-propylheptyl acrylate, sodium styrene sulfonate, etc., has solved the high resistivity, low bonding strength and electrolyte corrosion resistance in lithium batteries. The problem of insufficient properties has achieved a comprehensive improvement of low resistivity, high bonding strength and electrolyte corrosion resistance, extending the service life of lithium batteries.

CN118978879AInactive Publication Date: 2024-11-19BLUE OCEAN & BLACK STONE TECH CO LTD (FUJIAN)

Patent Information

Application Number
CN202411107770.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-19
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing water-based adhesives have problems in lithium batteries with high resistivity, low bonding strength and insufficient corrosion resistance of lithium hexafluorophosphate electrolyte, which limits its application in high-performance lithium batteries.

Method used

The three monomers are copolymerized by acrylic acid, 2-propylheptyl acrylate, and sodium styrene sulfonate, and surfactant, protective colloid and initiator are added to prepare low resistivity and high bonding through emulsification and polymerization. Water-based adhesive with strength and good resistance to electrolyte corrosion.

Benefits of technology

A water-based adhesive with low resistivity, high bonding strength and good electrolyte corrosion resistance is achieved, which improves the chemical corrosion resistance of the positive electrode material of lithium battery and extends the service life of lithium battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004991311300000041
    Figure BDA0004991311300000041
Patent Text Reader

Abstract

The invention relates to the technical field of battery electrode adhesives, and particularly discloses a carbon-coated aluminum foil water-based adhesive and a preparation method and application thereof. A preparation method of a water-based adhesive for carbon-coated aluminum foil comprises the following steps: putting acrylic acid, 2-propyl heptyl acrylate and sodium p-styrenesulfonate into water, fully dispersing, then adding a surfactant and a protective colloid, dispersing and emulsifying again, adding a pH buffer agent, adding an initiator, heating to 60-80 DEG C, reacting for 10-30 hours, and cooling to room temperature to obtain the water-based adhesive for carbon-coated aluminum foil. The carbon-coated aluminum foil water-based adhesive is obtained. The three monomers of acrylic acid, 2-propyl heptyl acrylate and sodium p-styrenesulfonate are copolymerized, the sodium p-styrenesulfonate also has an emulsifying effect and protects ordered proceeding of the reaction, and the obtained adhesive has low resistivity, high bonding strength and good lithium hexafluorophosphate electrolyte corrosion resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of lithium battery electrode adhesives, and in particular to a carbon-coated aluminum foil water-based adhesive and a preparation method and application thereof. Background Art

[0002] As a highly efficient energy storage device, lithium batteries have been widely used in various electronic devices. In the production process of lithium batteries, adhesives are needed to fix and connect electrode materials, such as coating and fixing carbon materials on aluminum foil. Traditional adhesives are usually based on organic solvents, which are harmful to the environment and human health. In recent years, water-based adhesives have attracted much attention due to their environmental friendliness and low toxicity. The electrolyte of lithium batteries is generally lithium hexafluorophosphate electrolyte, lithium hexafluorophosphate as the solute, and dimethyl carbonate (DMC) and ethylene carbonate (EC) as the solvents. However, the current water-based adhesives still have certain deficiencies in resistivity, bonding strength and corrosion resistance of lithium hexafluorophosphate electrolyte, which limits their application in high-performance lithium batteries.

[0003] In order to solve the above problems of water-based adhesives, researchers have tried a variety of methods, including changing the formulation of the adhesive, optimizing the preparation process, etc., but they can only improve the individual properties of the water-based adhesive to a certain extent, and it is difficult to achieve a comprehensive improvement in the low resistivity, high bonding strength and good resistance to corrosion in lithium hexafluorophosphate electrolyte of carbon-coated aluminum foil. Therefore, it is of great practical significance and application value to develop a water-based adhesive with low resistivity, high bonding strength and good resistance to corrosion in lithium hexafluorophosphate electrolyte. Summary of the invention

[0004] In view of the above problems, this application proposes the following technical solutions.

[0005] A method for preparing a carbon-coated aluminum foil water-based adhesive, the method comprising: adding acrylic acid, 2-propylheptyl acrylate, and sodium styrene sulfonate into water, fully dispersing, then adding a surfactant and a protective colloid, dispersing and emulsifying again, adding a pH buffer, adding an initiator, heating to 60-80°C and reacting for 10-30 hours to obtain the carbon-coated aluminum foil water-based adhesive.

[0006] By adopting the above technical scheme, three monomers of acrylic acid, 2-propylheptyl acrylate and sodium styrene sulfonate are copolymerized. Sodium styrene sulfonate also has an emulsifying effect to protect the orderly progress of the reaction. The adhesive obtained above has low resistivity, high bonding strength and good corrosion resistance to lithium hexafluorophosphate electrolyte.

[0007] A preferred solution of the preparation method of the carbon-coated aluminum foil water-based adhesive is that the mass ratio of acrylic acid, 2-propylheptyl acrylate and sodium styrene sulfonate is 50:(6-10):(20-30).

[0008] By adopting the above technical solution, the water-based adhesive prepared by the three monomers in this ratio achieves the requirements of low resistivity, high bonding strength and good electrolyte resistance.

[0009] A preferred solution for the preparation method of the carbon-coated aluminum foil water-based adhesive is that the mass ratio of the acrylic acid, the water, the surfactant, the protective colloid, and the initiator is 50:(100-200):(1-5):(1-5):(0.05-0.5).

[0010] By adopting the above technical solution, the polymerization reaction proceeds in an orderly manner and the reaction is sufficient.

[0011] A preferred embodiment of the method for preparing the carbon-coated aluminum foil water-based adhesive is that the surfactant is an anionic surfactant or a non-ionic surfactant.

[0012] By adopting the above technical solution, both the nonionic surfactant and the anionic surfactant can prevent the emulsion droplets from aggregating and stabilize the reaction of the droplets.

[0013] A preferred solution of the method for preparing the carbon-coated aluminum foil water-based adhesive is that the protective colloid is one of hydroxyethyl fiber, gelatin, gum arabic, sodium alginate, and sodium polyacrylate.

[0014] By adopting the above technical solution, this type of protective colloid can prevent the aggregation of colloid particles and improve the stability of the reaction solution.

[0015] A preferred solution of the method for preparing the carbon-coated aluminum foil water-based adhesive is that polyurethane emulsion is also added during the heating reaction process.

[0016] By adopting the above technical solution, the addition of polyurethane can further improve the adhesive's resistance to corrosion by lithium hexafluorophosphate electrolyte while maintaining good low resistivity and high bonding strength.

[0017] A preferred solution of the method for preparing the carbon-coated aluminum foil water-based adhesive is that the mass ratio of the acrylic acid to the polyurethane in the polyurethane emulsion is 50:(4-8).

[0018] By adopting the above technical solution and inputting raw materials in this ratio, the prepared adhesive has good low resistivity, high bonding strength and resistance to corrosion by lithium hexafluorophosphate electrolyte.

[0019] A carbon-coated aluminum foil water-based adhesive is prepared according to the above preparation method.

[0020] By adopting the above technical solution, the water-based adhesive has good bonding effect, low resistivity and resistance to corrosion by lithium hexafluorophosphate electrolyte.

[0021] The invention discloses an application of a carbon-coated aluminum foil water-based adhesive, wherein the carbon-coated aluminum foil water-based adhesive is used to bond carbon and then coated on a positive electrode aluminum foil of a lithium battery.

[0022] By adopting the above technical solution, the aqueous adhesive has good chemical corrosion resistance and can remain stable in the working environment of the lithium battery, thereby improving the electrolyte resistance of the positive electrode material and extending the service life of the lithium battery.

[0023] The low resistivity carbon-coated aluminum foil water-based adhesive of the present application is mainly used in the production process of lithium batteries to fix and connect electrode materials. It can be widely used in various electronic devices, such as smart phones, tablet computers, electric vehicles and other fields that require high-performance lithium batteries. DETAILED DESCRIPTION

[0024] Example 1 Take materials by mass, put 50 parts of acrylic acid, 8 parts of 2-propylheptyl acrylate, and 25 parts of sodium styrene sulfonate into 150 parts of water, fully disperse, then add 3 parts of surfactant and 2 parts of protective colloid, disperse and emulsify again, add 1 part of pH buffer, add 0.2 parts of initiator, heat to 75°C and react for 20 hours to obtain the carbon-coated aluminum foil water-based adhesive.

[0025] The surfactant is sodium stearate. The protective colloid is hydroxyethyl cellulose. The pH buffer is sodium bicarbonate. The initiator is sodium persulfate.

[0026] Example 2 Take materials by mass, put 50 parts of acrylic acid, 8 parts of 2-propylheptyl acrylate, and 25 parts of sodium styrene sulfonate into 150 parts of water, and fully disperse them. Then add 3 parts of surfactant and 2 parts of protective colloid, disperse and emulsify again, add 1 part of pH buffer, add 0.2 parts of initiator, heat to 75°C and react for 10 hours, add 10 parts of polyurethane emulsion with a mass concentration of 60%, and continue to react at 75°C for 10 hours to obtain the carbon-coated aluminum foil water-based adhesive.

[0027] The surfactant is sodium stearate. The protective colloid is hydroxyethyl cellulose. The pH buffer is sodium bicarbonate. The initiator is sodium persulfate.

[0028] Test Example 1 Take materials by mass, take 3.5 parts of adhesive and 50 parts of water, mix them, stir evenly, then add 1 part of conductive carbon black, 0.5 parts of carbon nanotubes and 45 parts of other positive electrode materials, stir evenly to obtain slurry, adjust the viscosity of the slurry at 25°C between 3000 and 4000 mPa·s by adjusting the water content, apply the slurry on aluminum foil with the same coating thickness, dry, cut into squares of the same size, and obtain carbon-coated aluminum foil. The two types of carbon-coated aluminum foil prepared in this test example are the same except that the types of adhesives are different and the viscosity of the slurry is different within the range. The types of adhesives are shown in Table 1.

[0029] The carbon coated aluminum foil was tested as follows.

[0030] Resistivity test: The carbon-coated aluminum foil was tested using a pole piece resistance meter, model BER1300 (IEST Yuanneng Technology).

[0031] Peel force test: Place the cut carbon-coated aluminum foil in a 35% RH constant temperature room for 30 minutes. Place the two carbon-coated aluminum foils together with the coating facing outward and the copper foil facing inward, and place them in an electric roller press to roll the carbon-coated aluminum foil to a compaction density of 0.95g / cm 3 , and then place it for 30 minutes after rolling. During this period, five 12.5cm×5cm stainless steel plates were selected, and double-sided tapes of corresponding specifications were pasted on the stainless steel plates. Then, the carbon-coated aluminum foil was pasted on the double-sided tape with the coating facing down, and then a 2.5cm wide masking tape was pasted on the copper foil. The carbon-coated aluminum foil steel plate was rolled back and forth by an electric rolling roller with a certain pressure (1kgf) for one week, and then an electronic stripping machine was used to test the adhesion of the carbon-coated aluminum foil; the same method as above was used, but only the carbon-coated aluminum foil was pasted on the double-sided tape with the coating facing up to test the cohesion of the carbon-coated aluminum foil.

[0032] Electrolyte resistance test: The electrolyte is 1 mol / L LiPF6, and the solvent is dimethyl carbonate (DMC) and ethylene carbonate (EC) in a volume ratio of 1:1. The carbon-coated aluminum foil is immersed in the electrolyte for 28 days, and the resistivity of the carbon-coated aluminum foil before and after immersion is tested. The adhesion and cohesion of the carbon-coated aluminum foil after immersion are tested according to the peeling force test method.

[0033] The test results of the above test items are shown in Table 1.

[0034] Table 1 Performance test of carbon-coated aluminum foil prepared by four adhesives In Table 1, PVDF5130 is polyvinylidene fluoride supplied by Shanghai Youcheng International Trading Co., Ltd.

[0035] It can be concluded from Table 1 that the water-based adhesive prepared in Example 1 and Example 2 is used in carbon-coated aluminum foil. Compared with polyacrylate and PVDF5130, the resistivity, bonding strength and corrosion resistance of the carbon-coated aluminum foil prepared in Example 1 and Example 2 are significantly better than those of polyacrylate and PVDF5130. The above shows that the water-based adhesive copolymerized with three monomers of acrylic acid, 2-propylheptyl acrylate and sodium styrene sulfonate in this application has low resistivity, which improves the conductive properties of the carbon-coated aluminum foil; has high bonding strength and can firmly connect the electrode material; has high corrosion resistance to lithium hexafluorophosphate electrolyte, and can be used in lithium batteries to extend the service life of lithium batteries.

[0036] In Table 1, by comparing the carbon-coated aluminum foils prepared by the water-based adhesives prepared in Example 1 and Example 2, it can be seen that the carbon-coated aluminum foil prepared by adding a small amount of polyurethane emulsion during the polymerization process of the water-based adhesive in Example 2 has a smaller increase in resistivity and a smaller decrease in bonding strength after long-term use.

[0037] The low-resistivity carbon-coated aluminum foil water-based adhesive of the present application is mainly used in the production process of lithium batteries to fix and connect electrode materials, and can be widely used in various electronic devices such as smart phones, tablet computers, electric vehicles and other fields that require high-performance lithium batteries.

[0038] The above are only some embodiments of the present application, and the protection scope of the present application is not limited to the above embodiments. For ordinary technicians in this technical field, some improvements and modifications without departing from the creative design of the present application should also fall within the protection scope of the present application.

Claims

1. A method for preparing a carbon-coated aluminum foil water-based adhesive, characterized in that: The preparation method comprises: putting acrylic acid, 2-propylheptyl acrylate and sodium styrene sulfonate into water, fully dispersing them, then adding surfactant and protective colloid, dispersing and emulsifying them again, adding pH buffer, adding initiator, heating to 60-80°C and reacting for 10-30h to obtain the carbon-coated aluminum foil water-based adhesive.

2. The method for preparing the carbon-coated aluminum foil water-based adhesive according to claim 1, characterized in that: The mass ratio of acrylic acid, 2-propylheptyl acrylate and sodium styrene sulfonate is 50:(6-10):(20-30).

3. The method for preparing the carbon-coated aluminum foil water-based adhesive according to claim 1, characterized in that: The mass ratio of the acrylic acid, the water, the surfactant, the protective colloid and the initiator is 50:(100-200):(1-5):(1-5):(0.05-0.5).

4. The method for preparing the carbon-coated aluminum foil water-based adhesive according to claim 1, characterized in that: The surfactant is an anionic surfactant or a nonionic surfactant.

5. The method for preparing the carbon-coated aluminum foil water-based adhesive according to claim 1, characterized in that: The protective colloid is one of hydroxyethyl cellulose, gelatin, gum arabic, sodium alginate and sodium polyacrylate.

6. The method for preparing the carbon-coated aluminum foil water-based adhesive according to claim 1, characterized in that: During the heating reaction process, polyurethane emulsion is also added.

7. The method for preparing the carbon-coated aluminum foil water-based adhesive according to claim 6, characterized in that: The mass ratio of the acrylic acid to the polyurethane in the polyurethane emulsion is 50:(4-8).

8. A carbon-coated aluminum foil water-based adhesive, characterized in that: Prepared according to the preparation method according to any one of claims 1 to 7.

9. An application of the carbon-coated aluminum foil water-based adhesive as claimed in claim 8, characterized in that: The carbon-coated aluminum foil water-based adhesive is used to bind carbon and then coated on the positive electrode aluminum foil of the lithium battery.

Citation Information

Patent Citations

  • Bonding glue used for glass mosaics and preparation method thereof

    CN103059794A

  • Lithium ion battery positive electrode aqueous adhesive and preparation method thereof

    CN106833448A

  • Aqueous adhesive for heatproof layer of lithium ion battery diaphragm, and preparation method and applications thereof

    CN107384261A

  • Composite emulsion type lithium battery ceramic diaphragm adhesive as well as preparation method and application thereof

    CN115785860A

  • Conductive composite aqueous binder as well as preparation method and application thereof

    CN116948573A

Cited By

  • Negative electrode binder, negative electrode plate and battery

    CN119371911A