Vacuum oscillation hot-pressing repair method for copper-steel rotor of hydraulic pump

The problem of wear on the copper alloy end face of the copper-steel rotor of the hydraulic pump was solved by the vacuum oscillation hot pressing repair method, achieving efficient repair and low-cost product maintenance.

CN118989858AActive Publication Date: 2024-11-22WUHU STATE-OWNED FACTORY OF MACHINING

Patent Information

Application Number
CN202411049581.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-11-22
Estimated Expiration
2044-08-01

AI Technical Summary

Technical Problem

Existing technologies are insufficient to effectively repair the wear on the copper alloy end face of the copper-steel rotor of a hydraulic pump, resulting in the need to replace high-value-added products and increasing economic costs.

Method used

The vacuum oscillation hot pressing repair method is adopted. By applying pressure in both directions through the upper and lower pressure heads and medium-frequency vibration pressure, a dense connection of copper alloy is formed in a short time at low temperature. X-ray flaw detection is combined to ensure the repair quality.

Benefits of technology

While reducing energy consumption, product quality has been improved, ensuring high-quality repair of high-value-added hydraulic pump rotors and significantly reducing maintenance costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118989858A_ABST
    Figure CN118989858A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of remanufacturing, in particular to a hydraulic pump copper steel rotor vacuum oscillation hot pressing repairing method which comprises the following steps that the corroded and abraded copper alloy end face of a hydraulic pump rotor is polished; processing into a corresponding copper alloy circular ring patch; the hydraulic pump rotor is placed in the lower tool, and the copper alloy end face of the hydraulic pump rotor faces upwards; the copper alloy circular ring patch is fixed to the lower portion of the upper tool through a spring buckle at the bottom of the upper tool; the upper tool, the copper alloy circular ring patch, the hydraulic pump rotor and the lower tool jointly form a to-be-machined connecting assembly; performing oscillation hot-pressing repair; and carrying out nondestructive testing. According to the method, through bidirectional pressurization of the upper pressure head and the lower pressure head and superposition of medium-frequency vibration pressure, compact connection between copper alloys can be formed under the conditions of low temperature and short time, the product quality is improved while energy consumption is reduced, high-quality repair of the high-added-value hydraulic pump rotor is guaranteed, and the product maintenance cost is greatly reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of remanufacturing, and in particular to a vacuum oscillation hot pressing repair method for a hydraulic pump copper-steel rotor. Background Art

[0002] Hydraulic products made of copper and steel bimetallic materials can give full play to the excellent corrosion resistance, wear resistance and lubrication performance of copper alloy, and the high strength performance of steel, which can significantly improve the power-to-weight ratio of hydraulic products. However, hydraulic products, especially rotor products, will inevitably cause certain wear on the copper alloy end face during long-term high-speed operation, thus failing to ensure the reliable operation of the important precision friction pair of the rotor.

[0003] At present, the repair processes for copper alloys include gas welding, brazing, manual arc welding, TIG welding, electron beam welding, etc., but these processes have poor performance after welding and many defects. Therefore, facing the problem of copper alloy end face wear of high value-added hydraulic pump copper steel rotor, no effective repair technology has been proposed. The worn high value-added hydraulic pump rotor can only be replaced, which leads to extremely high economic costs. Summary of the invention

[0004] In order to solve the above technical problems, the present invention proposes a vacuum oscillation hot pressing repair method for a hydraulic pump copper-steel rotor.

[0005] The technical problem to be solved by the present invention is achieved by adopting the following technical solutions:

[0006] A vacuum oscillation hot pressing repair method for a hydraulic pump copper steel rotor comprises the following steps:

[0007] S1. Grind the corroded and worn copper alloy end surface of the hydraulic pump rotor, clean it with ultrasonic wave in acetone, and then blow it dry for later use;

[0008] S2. Use the same material as the copper alloy end face of the hydraulic pump rotor, process it into a corresponding copper alloy ring patch according to the groove form of the copper alloy end face of the hydraulic pump rotor, and polish and clean the surface of the copper alloy ring patch, and then blow dry it for standby use;

[0009] S3. Place the hydraulic pump rotor into the lower tooling with the copper alloy end of the hydraulic pump rotor facing upwards;

[0010] S4. Fix the copper alloy ring patch to the lower part of the upper tooling through the spring buckle at the bottom of the upper tooling;

[0011] S5. Position the upper tooling together with the copper alloy annular patch on the hydraulic pump rotor by positioning the boss at the bottom of the upper tooling and the groove on the hydraulic pump rotor. With the support of the spring buckle, there is a certain distance between the lower end surface of the copper alloy annular patch and the copper alloy end surface of the hydraulic pump rotor. The upper tooling, the copper alloy annular patch, the hydraulic pump rotor and the lower tooling together form a connection component to be processed.

[0012] S6. Place the connection component to be processed between the upper pressure head and the lower pressure head of the oscillating hot pressing furnace, close the furnace door, evacuate, and then perform oscillating hot pressing repair. The oscillating hot pressing repair process is as follows:

[0013] First, when the vacuum is evacuated to a vacuum degree not higher than 100Pa, a pre-pressure of 0.5-1.0MPa is applied to the connection component to be processed, and heating is started at a heating rate of 10-15℃ / min, and the temperature is heated to 500-580℃ for 2-4H. At the same time, an axial oscillating pressure of 15-35MPa is applied to the connection component to be processed, and the amplitude of the oscillating pressure is 8-10MPa and the frequency of the oscillating pressure is 20-40Hz;

[0014] S7. After cooling down with the furnace, release the pressure, and after reaching room temperature, open the hatch and take out the repaired connection components;

[0015] S8. Take out the repaired hydraulic pump rotor from the tooling and conduct non-destructive testing. If there are no cracks or gaps inside, it is qualified. Machining is carried out according to the requirements of the drawing to remove excess materials, restore the original size of the hydraulic pump rotor, and complete the repair. Otherwise, the copper alloy end face of the hydraulic pump rotor is re-polished and oscillation hot pressing repair is performed again.

[0016] Preferably, in step S1, the grinding depth of the corroded and worn copper alloy end surface of the hydraulic pump rotor is 1 mm.

[0017] Preferably, the thickness of the copper alloy ring patch in step S2 is 2 mm.

[0018] Preferably, in step S3, the lower fixture is in a bowl-shaped structure, and a gap of 2 mm is left between the bottom of the lower fixture and the lowermost surface of the hydraulic pump rotor.

[0019] Preferably, the thickness of the boss in step S4 is 3 mm.

[0020] Preferably, in step S7, the temperature is lowered at a rate of 20°C / min, and the pressure is released when the temperature drops to 200°C.

[0021] Preferably, the nondestructive testing method in step S8 is X-ray testing.

[0022] The beneficial effects of the present invention are:

[0023] The present invention can form a dense connection between copper alloys under conditions of lower temperature and shorter time by applying bidirectional pressurization by upper and lower pressure heads and superimposing medium-frequency vibration pressure, thereby improving product quality while reducing energy consumption, ensuring high-quality repair of high-value-added hydraulic pump rotors, and greatly reducing product maintenance costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] The present invention is further described below in conjunction with the accompanying drawings and embodiments:

[0025] Figure 1 This is a schematic diagram of corrosion and wear on the copper alloy end surface of the hydraulic pump rotor of the present invention;

[0026] Figure 2 This is a schematic diagram of the copper alloy end surface of the hydraulic pump rotor after grinding of the present invention;

[0027] Figure 3 This is a schematic diagram of the structure of the copper alloy ring patch of the present invention;

[0028] Figure 4 This is a schematic diagram of the lower tooling structure of the present invention;

[0029] Figure 5 It is a schematic diagram of the tooling structure of the present invention;

[0030] Figure 6 is a cross-sectional schematic diagram of a connection assembly of the present invention;

[0031] Figure 7 This is a schematic diagram of the copper alloy end surface of the hydraulic pump rotor after repair by the present invention.

[0032] In the figure: 1. hydraulic pump rotor; 2. copper alloy ring patch; 3. lower tooling; 4. upper tooling; 5. spring buckle; 6. boss; 7. groove. DETAILED DESCRIPTION

[0033] In order to make the technical means, creative features, objectives and effects achieved by the present invention easy to understand, the present invention is further described below with reference to the accompanying drawings and embodiments.

[0034] A vacuum oscillation hot pressing repair method for a hydraulic pump copper steel rotor comprises the following steps:

[0035] S1. Grind the corroded and worn copper alloy end surface of the hydraulic pump rotor 1, such as Figure 1 As shown in FIG. 1 , the copper alloy end face of the hydraulic pump rotor 1 that is corroded and worn is shown. The grinding depth is about 1 mm, and then the rotor is ultrasonically cleaned in acetone and then blown dry for later use. Figure 2 shown.

[0036] S2. Use the same material as the copper alloy end face of the hydraulic pump rotor 1. In this embodiment, specifically ZQCu10-2-3 material. Process the corresponding copper alloy ring patch 2 according to the groove 7 of the copper alloy end face of the hydraulic pump rotor 1. The thickness of the copper alloy ring patch 2 is 2 mm, so that there is still a 1 mm processing margin after oscillation hot pressing. Polish and clean the surface of the copper alloy ring patch 2, and then blow dry for use. The structure of the copper alloy ring patch 2 is as follows: Figure 3 shown.

[0037] S3, put the hydraulic pump rotor 1 into the lower tooling 3, with the copper alloy end of the hydraulic pump rotor 1 facing upward. The structure of the lower tooling 3 is as follows Figure 4 The lower fixture 3 is a bowl-shaped structure, and the lower end of the hydraulic pump rotor 1 can be embedded in its circular groove to ensure vertical and stable placement. Considering that the lower end surface of the hydraulic pump rotor 1 is a precision assembly surface, a 2mm gap is left between it and the lower fixture 3 to prevent the lower end of the hydraulic pump rotor 1 from being compressed and deformed.

[0038] S4, fix the copper alloy ring patch 2 to the lower part of the upper tooling 4 through the spring buckle 5 at the bottom of the upper tooling 4. The structure of the upper tooling 4 is as follows Figure 5 shown.

[0039] S5. Positioning is performed through the boss 6 at the bottom of the upper tooling 4 and the groove 7 on the hydraulic pump rotor 1. The thickness of the boss 6 is 3mm, ensuring that the relative position of the upper tooling, the annular patch and the hydraulic pump rotor is accurate. The upper tooling 4 and the copper alloy annular patch 2 are placed together on the hydraulic pump rotor 1. Under the support of the spring buckle 5, there is a certain distance between the lower end face of the copper alloy annular patch 2 and the copper alloy end face of the hydraulic pump rotor 1. This distance is conducive to the discharge of gas between the lower end face of the copper alloy annular patch 2 and the copper alloy end face of the hydraulic pump rotor 1 during subsequent vacuuming. If the spring buckle 5 is not provided, there will be no distance between the lower end face of the copper alloy annular patch 2 and the copper alloy end face of the hydraulic pump rotor 1, which may cause gas to remain between the lower end face of the copper alloy annular patch 2 and the copper alloy end face of the hydraulic pump rotor during vacuuming, thereby forming an unfused defect due to the residual gas after hot pressing. The upper tooling 4, the copper alloy annular patch 2, the hydraulic pump rotor 1 and the lower tooling 3 together form a connection component to be processed.

[0040] S6. Place the connection component to be processed between the upper pressure head and the lower pressure head of the oscillating hot pressing furnace, close the furnace door, evacuate, and then perform oscillating hot pressing repair. The oscillating hot pressing repair process is as follows:

[0041] First, evacuate to a vacuum degree no higher than 100Pa, apply a pre-pressure of 0.5-1.0MPa to the processing connection component, start heating, the heating rate is 10-15℃ / min, heat to 500-580℃, keep warm for 2-4H, and at the same time apply an axial oscillation pressure of 15-35MPa to the processing connection component, the oscillation pressure amplitude is 8-10MPa, and the oscillation pressure frequency is 20-40Hz.

[0042] Specifically, in this embodiment, the vacuum is evacuated to a vacuum degree of 50Pa, and a pre-pressure of 0.8MPa is applied to the connection assembly to be processed. Under the pressure, the spring buckle is deformed, and the lower end surface of the copper alloy ring patch is tightly fitted with the upper end surface of the hydraulic pump rotor. Heating is started to be heated to 550°C and the temperature is kept for 2 hours. At the same time, an axial oscillation pressure of 20MPa is applied to the connection assembly to be processed, and the amplitude of the oscillation pressure is 10MPa and the frequency of the oscillation pressure is 30Hz. It is ensured that the copper alloys are metallurgically bonded.

[0043] S7. After the oscillation hot pressing of the connection components is completed, the pressure is released and the temperature is lowered at a rate of 20℃ / min. When the temperature drops to 200℃, the pressure between the upper and lower pressure heads is released. After cooling to room temperature, the pressure in the furnace is restored to atmospheric pressure, the hatch is opened, and the repaired connection components are taken out.

[0044] S8. Take out the repaired hydraulic pump rotor 1 from the tooling and perform nondestructive testing by X-ray flaw detection. If there is no crack or gap inside, it is qualified. Machining is performed according to the requirements of the drawing to remove excess material, restore the original size of the hydraulic pump rotor 1, and complete the repair. Otherwise, the copper alloy end face of the hydraulic pump rotor 1 is re-polished and oscillation hot pressing repair is performed again.

[0045] According to the above examples, shear specimens were prepared in the same way and mechanical properties were verified. The results are shown in Table 1.

[0046] Table 1 Comparison of performance between conventional repair and vacuum shock hot pressing repair

[0047] sample Shear strength / MPa Base Material 258 Conventional welding repair 202 Vacuum Oscillation Hot Press Repair 249

[0048] As can be seen from Table 1, the mechanical properties of the products repaired by vacuum oscillation hot pressing sintering are similar to those of the parent material, and are significantly higher than those of the samples repaired by conventional diffusion welding.

[0049] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The above embodiments and descriptions only describe the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention. The scope of protection of the present invention is defined by the attached claims and their equivalents.

Claims

1. A vacuum oscillation hot pressing repair method for a hydraulic pump copper steel rotor, characterized in that: The following steps are involved: S1. Grind the corroded and worn copper alloy end surface of the hydraulic pump rotor (1), clean it by ultrasonic cleaning in acetone, and then blow dry it for later use; S2, using the same material as the copper alloy end face of the hydraulic pump rotor (1), processing into a corresponding copper alloy annular patch (2) according to the form of the groove (7) on the copper alloy end face of the hydraulic pump rotor (1), and polishing and cleaning the surface of the copper alloy annular patch (2), and then drying it for standby use; S3, placing the hydraulic pump rotor (1) into the lower tooling (3), with the copper alloy end surface of the hydraulic pump rotor (1) facing upward; S4, fixing the copper alloy annular patch (2) to the lower part of the upper tooling (4) by means of the spring buckle (5) at the bottom of the upper tooling (4); S5. Positioning is performed by using the boss (6) at the bottom of the upper tooling (4) and the groove (7) on the hydraulic pump rotor (1), and the upper tooling (4) and the copper alloy annular patch (2) are placed together on the top of the hydraulic pump rotor (1). With the support of the spring buckle (5), there is a certain distance between the lower end surface of the copper alloy annular patch (2) and the copper alloy end surface of the hydraulic pump rotor (1). The upper tooling (4), the copper alloy annular patch (2), the hydraulic pump rotor (1) and the lower tooling (3) together form a connection component to be processed; S6. Place the connection component to be processed between the upper pressure head and the lower pressure head of the oscillating hot pressing furnace, close the furnace door, evacuate, and then perform oscillating hot pressing repair. The oscillating hot pressing repair process is as follows: First, when the vacuum is evacuated to a vacuum degree not higher than 100Pa, a pre-pressure of 0.5-1.0MPa is applied to the connection component to be processed, and heating is started at a heating rate of 10-15℃ / min, and the temperature is heated to 500-580℃ for 2-4H. At the same time, an axial oscillating pressure of 15-35MPa is applied to the connection component to be processed, and the amplitude of the oscillating pressure is 8-10MPa and the frequency of the oscillating pressure is 20-40Hz; S7. After cooling down with the furnace, release the pressure, and after reaching room temperature, open the hatch and take out the repaired connection components; S8. The repaired hydraulic pump rotor (1) is taken out from the tooling and subjected to nondestructive testing. If there are no cracks or gaps inside, it is qualified. Machining is performed according to the requirements of the drawing to remove excess materials and restore the original size of the hydraulic pump rotor (1). Otherwise, the copper alloy end face of the hydraulic pump rotor (1) is re-polished and oscillation hot pressing is performed again for repair.

2. A vacuum oscillation hot pressing repair method for a hydraulic pump copper steel rotor according to claim 1, characterized in that: In step S1, the grinding depth of the corroded and worn copper alloy end surface of the hydraulic pump rotor (1) is 1 mm.

3. The vacuum oscillation hot pressing repair method for a hydraulic pump copper steel rotor according to claim 1 is characterized in that: The thickness of the copper alloy ring patch (2) in step S2 is 2 mm.

4. A vacuum oscillation hot pressing repair method for a hydraulic pump copper steel rotor according to claim 1, characterized in that: In step S3, the lower fixture (3) is in a bowl-shaped structure, and a gap of 2 mm is left between the bottom of the lower fixture (3) and the lowermost surface of the hydraulic pump rotor (1).

5. The vacuum oscillation hot pressing repair method for a hydraulic pump copper steel rotor according to claim 1 is characterized in that: The thickness of the boss (6) in step S4 is 3 mm.

6. A vacuum oscillation hot pressing repair method for a hydraulic pump copper steel rotor according to claim 1, characterized in that: In step S7, the temperature is lowered at a rate of 20°C / min, and the pressure is released when the temperature drops to 200°C.

7. A vacuum oscillation hot pressing repair method for a hydraulic pump copper steel rotor according to claim 1, characterized in that: The non-destructive testing method in step S8 is X-ray flaw detection.

Citation Information

Patent Citations

  • Vacuum brazing repairing method for cracks of high-temperature alloy thin-wall part

    CN102120292A

  • Vamp wrapping process for carbon fiber prepreg repaired aluminum alloy crack pipe

    CN104175058A

  • Method for repairing metal structure through composite material bonding based on health monitoring technology

    CN117102804A

  • IBR blade repair

    GB202216469D0

  • Splice insert repair for superalloy turbine blades

    US20130115091A1

Cited By

  • Oscillation hot-pressing integrated forming process for L-shaped groove insulation of generator rotor

    CN120956009A

  • A vibration and hot-pressing integrated forming process for L-shaped slot insulation of a generator rotor

    CN120956009B