Preparation method and application of temperature-sensitive hydrogel membrane with reversibly switched wettability

Through a composite gel of polydimethylsiloxane, titanium dioxide nanoparticles and N-isopropyl acrylamide, a wettability reversible switching hydrogel film with temperature and ultraviolet light response was prepared, which solved the existing hydrogel The poor controllability of controlled release has achieved effective improvements in controlled release and biocompatibility of drugs.

CN118994673APending Publication Date: 2024-11-22CHINA JILIANG UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411106701.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Existing temperature-sensitive hydrogels have problems such as poor controllability and insufficient biocompatibility in controlled drug release, making it difficult to achieve effective temperature response and ultraviolet light response.

Method used

Using a composite gel of polydimethylsiloxane and titanium dioxide nanoparticles combined with N-isopropyl acrylamide, the temperature sensitivity with reversible switching of wetting is prepared by photoinitiator grafting and monomer polymerization grafting steps. Hydrocoagulation film has dual response to temperature and ultraviolet light.

Benefits of technology

It realizes effective controlled release of substances under temperature and ultraviolet light conditions, has stable surface structure and adjustable roughness, simple operation, and gentle and easy to control reaction conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118994673A_ABST
    Figure CN118994673A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and application of a temperature-sensitive hydrogel membrane with reversibly switched wettability, and relates to the technical field of surface modification of biological materials. The temperature-sensitive hydrogel membrane with reversibly switched wettability has the characteristics of temperature response and ultraviolet light response at the same time. The thermo-sensitive composite gel formed by the invention combines the properties of both intelligent gel and nanoparticles, and can realize effective controlled release of substances under ultraviolet light and temperature conditions after loading other substances. The photo-thermal response type composite gel is stable in surface structure and uniform and adjustable in roughness, in addition, the preparation and operation method is simple, and reaction conditions are mild and easy to control. The invention can obtain the preparation method and the application of the temperature-sensitive hydrogel membrane with reversibly switched wettability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of biomaterial surface modification, and in particular to a preparation method and application of a temperature-sensitive hydrogel film with reversible wettability switching. Background Art

[0002] In recent years, with the continuous deepening of nanomaterial research, functionalization and intelligence have gradually become important directions in nanomaterial research, among which organic-inorganic composite materials have attracted widespread attention. TiO2 has many characteristics such as high chemical stability, non-toxicity and small particle size, combined with organic materials with environmental responsiveness, and has broad application prospects in the fields of drug encapsulation and sustained release, biocatalysis, coatings, etc., and has great potential value.

[0003] Temperature response is the most common environmental response. Poly (N-isopropylacrylamide) is the most studied thermosensitive polymer. It has a phase transition temperature around 32°C, which is called the minimum solubility temperature. When poly (N-isopropylacrylamide) is below the minimum solubility temperature, its chain contains a large number of hydrophilic groups, showing hydrophilicity. At the same time, its porous structure and very soft properties can simulate normal tissue very closely and have good biocompatibility. In addition, the low interfacial free energy makes it difficult for bacteria, cells and proteins to adsorb on its surface. When poly (N-isopropylacrylamide) is above the minimum solubility temperature, its chain cannot combine with the hydrogen bonds in the water molecules, showing hydrophobicity, and the surface is no longer antibacterial. At the same time, its excellent biocompatibility is conducive to its adhesion on the cell surface and can be used for the directional release of drugs. However, there are still many problems in the research on drug controlled release of hydrogels, such as high technical difficulty, poor controllability, and poor biocompatibility. Summary of the invention

[0004] The purpose of the present invention is to solve the above technical problems and to provide a preparation method and application of a temperature-sensitive hydrogel film with reversible wettability switching.

[0005] like Figure 1 As shown, a method for preparing a temperature-sensitive hydrogel film with reversible wettability switching is carried out according to the following steps:

[0006] Step S1: preparing a uniform coating of polydimethylsiloxane;

[0007] Put polydimethylsiloxane and curing agent in a centrifugal mixer and mix for 3 to 4 minutes to obtain a mixture; pour the mixture onto the pretreated substrate, then fix the substrate onto a coating machine, start the coating machine, form a PDMS coating on the surface of the substrate, and then place it on a hot plate for curing to obtain a cured PDMS coating-substrate;

[0008] Step S2: Preparation of titanium dioxide nanolayer;

[0009] The titanium dioxide nanoparticle suspension is evenly sprayed onto the PDMS coating-substrate cured in step S1 by a spray gun, and dried to obtain a dried PDMS coating-substrate;

[0010] Step S3: grafting of photoinitiator;

[0011] Under a yellow light environment with a wavelength of 590 nm, the PDMS coating-substrate dried in step S2 is immersed in a benzophenone solution for 10 to 15 minutes, then rinsed and dried to obtain a treated PDMS coating-substrate;

[0012] Step S4: monomer polymerization grafting;

[0013] Under a yellow light environment with a wavelength of 590 nm, N-isopropyl acrylamide and a crosslinking agent N,N'-methylenebisacrylamide are dissolved in deionized water, wherein the mass ratio of the N-isopropyl acrylamide to the crosslinking agent N,N'-methylenebisacrylamide is 100:(1-1.5); then the PDMS coating-substrate treated in step S3 is immersed in deionized water, irradiated with an ultraviolet lamp for 10-20 minutes, then the substrate is rinsed and dried, and finally demolded to obtain a thermosensitive hydrogel film with reversible wettability switching (such as Figure 2 shown);

[0014] The mass ratio of the titanium dioxide nanoparticles to N-isopropylacrylamide in the polydimethylsiloxane and titanium dioxide nanoparticle suspension is (5-12): (0.2-0.25): (2-4).

[0015] An application of a thermosensitive hydrogel film with reversible wettability switching, and an application of the thermosensitive hydrogel film with reversible wettability switching in the preparation of a drug with temperature response and ultraviolet light response.

[0016] Principle of the present invention:

[0017] The present invention spin-coats PDMS on a substrate material, sprays titanium dioxide particles to construct a nano rough layer, and then uses chemical grafting to load a polyisopropylacrylamide hydrogel coating on the surface to achieve a temperature-responsive selective biological effect.

[0018] Beneficial effects of the present invention:

[0019] The present invention discloses a thermosensitive hydrogel film with reversible wettability switching, which has the characteristics of temperature response and ultraviolet light response. The thermosensitive composite gel formed by the present invention combines the performance of both smart gel and nanoparticles, and can realize effective controlled release of substances under ultraviolet light and temperature conditions after loading other substances. The photothermal responsive composite gel of the present invention has a stable surface structure and uniform and adjustable roughness. In addition, the preparation and operation methods are simple, and the reaction conditions are mild and easy to control.

[0020] The present invention can obtain a preparation method and application of a temperature-sensitive hydrogel film with reversible wettability switching. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 A schematic diagram showing the preparation process of a temperature-sensitive hydrogel film with reversible wettability switching according to the present invention;

[0022] Figure 2 A schematic diagram showing the structure of a temperature-sensitive hydrogel membrane with reversible wettability switching according to the present invention;

[0023] Figure 3 A microscopic image showing the surface structure of the temperature-sensitive hydrogel film with reversible wettability switching obtained in Example 1;

[0024] Figure 4 A surface water contact angle diagram of the temperature-sensitive hydrogel film with reversible wettability switching obtained in Example 2 at 20°C;

[0025] Figure 5 A surface water contact angle diagram of the temperature-sensitive hydrogel film with reversible wettability switching obtained in Example 2 at 40°C;

[0026] Figure 6 The graph showing the change of water contact angle on the surface of the hydrogel with temperature when switching back and forth between 20°C and 40°C in Example 3;

[0027] Figure 7 A graph showing how the water contact angle on the hydrogel surface changes with the duration of ultraviolet light irradiation under the combined effects of temperature response and ultraviolet light response. DETAILED DESCRIPTION

[0028] Specific implementation method 1: In this implementation method, a method for preparing a temperature-sensitive hydrogel film with reversible wettability is carried out according to the following steps:

[0029] Step S1: preparing a uniform coating of polydimethylsiloxane;

[0030] Put polydimethylsiloxane and curing agent in a centrifugal mixer and mix for 3 to 4 minutes to obtain a mixture; pour the mixture onto the pretreated substrate, then fix the substrate onto a coating machine, start the coating machine, form a PDMS coating on the surface of the substrate, and then place it on a hot plate for curing to obtain a cured PDMS coating-substrate;

[0031] Step S2: Preparation of titanium dioxide nanolayer;

[0032] The titanium dioxide nanoparticle suspension is evenly sprayed onto the PDMS coating-substrate cured in step S1 by a spray gun, and dried to obtain a dried PDMS coating-substrate;

[0033] Step S3: grafting of photoinitiator;

[0034] Under a yellow light environment with a wavelength of 590 nm, the PDMS coating-substrate dried in step S2 is immersed in a benzophenone solution for 10 to 15 minutes, then rinsed and dried to obtain a treated PDMS coating-substrate;

[0035] Step S4: monomer polymerization grafting;

[0036] Under a yellow light environment with a wavelength of 590 nm, N-isopropyl acrylamide and a cross-linking agent N,N'-methylenebisacrylamide are dissolved in deionized water, wherein the mass ratio of the N-isopropyl acrylamide to the cross-linking agent N,N'-methylenebisacrylamide is 100:(1-1.5); then the PDMS coating-substrate treated in step S3 is immersed in deionized water, irradiated with an ultraviolet lamp for 10-20 minutes, then the substrate is rinsed and dried, and finally demolded to obtain a temperature-sensitive hydrogel film with reversible wettability switching;

[0037] The mass ratio of the titanium dioxide nanoparticles to N-isopropylacrylamide in the polydimethylsiloxane and titanium dioxide nanoparticle suspension is (5-12): (0.2-0.25): (2-4).

[0038] The role of the yellow light environment in steps S3 and S4 is to carry out the grafting of the photoinitiator and to prevent exposure to prevent ultraviolet rays from affecting the photoinitiator.

[0039] Specific embodiment 2: The difference between this embodiment and specific embodiment 1 is that in step S1, polydimethylsiloxane and curing agent are placed in a centrifugal mixer, first rotated forward for 1.5 to 2 minutes, and then reversed for 1.5 to 2 minutes.

[0040] The other steps are the same as those in the first specific implementation.

[0041] Specific implementation method three: This implementation method is different from specific implementation methods one or two in that: the mass ratio of the polydimethylsiloxane to the curing agent in step S1 is (8-10):1, and the curing agent is Dow Corning 184.

[0042] The other steps are the same as those in the first or second embodiment.

[0043] Specific implementation method four: The difference between this implementation method and specific implementation methods one to three is that the pre-treated substrate described in step S1 is processed according to the following steps: the substrate is placed in an ultrasonic cleaning machine for ultrasonic cleaning for 10 to 20 minutes, and after the ultrasonic cleaning, it is rinsed with deionized water for 3 to 5 times, and then blown dry with nitrogen and placed in a vacuum drying oven at 65 to 70°C for 10 to 20 minutes; the substrate is a silicon substrate.

[0044] The other steps are the same as those in Specific Embodiments 1 to 3.

[0045] Specific implementation method five: The difference between this implementation method and specific implementation methods one to four is that: in step S1, the substrate is fixed to the coating machine, and the coating machine is started. It is first pre-rotated at a speed of 500-600 r / min for 10-12s, and then rotated at a speed of 1500-2000 r / min for 50-60s to form a PDMS coating on the surface of the substrate, and then placed on a hot stage for curing at 90-120°C for 20-60min.

[0046] The other steps are the same as those in Specific Embodiments 1 to 4.

[0047] Specific embodiment six: The difference between this embodiment and specific embodiments one to five is that the titanium dioxide nanoparticle suspension described in step S2 is prepared according to the following steps: titanium dioxide nanoparticles with an average particle size of 25nm are added to anhydrous ethanol, and an ultrasonic crusher is used to uniformly disperse them at a power of 300W to obtain a titanium dioxide nanoparticle suspension with a concentration of 5%, and the mass ratio of the titanium dioxide nanoparticles to anhydrous ethanol is (0.2-0.25): (3.8-4.75); the drying temperature in step S2 is 65-70°C.

[0048] The other steps are the same as those in Specific Embodiments 1 to 5.

[0049] Specific embodiment seven: The difference between this embodiment and specific embodiments one to six is ​​that the benzophenone solution described in step S3 is prepared according to the following steps: 2g of benzophenone is added to 18g of anhydrous ethanol, and after mixing evenly, a benzophenone solution with a concentration of 10% is obtained; after rinsing with deionized water in step S3, it is placed in a drying oven at 65-70°C for drying.

[0050] The other steps are the same as those in Specific Embodiments 1 to 6.

[0051] Specific embodiment eight: The difference between this embodiment and specific embodiments one to seven is that in step S4, the mass ratio of N-isopropylacrylamide, cross-linking agent N,N'-methylenebisacrylamide and deionized water is 2: (0.02-0.03): (17.97-17.98).

[0052] The other steps are the same as those in Specific Embodiments 1 to 7.

[0053] Specific embodiment nine: The difference between this embodiment and specific embodiments one to eight is that the wavelength of the ultraviolet lamp in step S4 is 340-365nm, and the power is 300-500W; after the ultraviolet lamp irradiation in step S4, it is first rinsed alternately with anhydrous ethanol and deionized water 3-4 times, and then placed in a drying oven at 65-70°C to dry.

[0054] The other steps are the same as those in Specific Embodiments 1 to 8.

[0055] Specific embodiment 10: This embodiment provides an application of a thermosensitive hydrogel film with reversible wettability switching, and the application of the thermosensitive hydrogel film with reversible wettability switching in the preparation of drugs with temperature response and ultraviolet light response.

[0056] The following examples are used to verify the beneficial effects of the present invention:

[0057] Example 1: A method for preparing a temperature-sensitive hydrogel film with reversible wettability switching, comprising the following steps:

[0058] Step S1: preparing a uniform coating of polydimethylsiloxane;

[0059] A 4-inch substrate was placed in an ultrasonic cleaning machine for ultrasonic cleaning for 10 minutes, and after the ultrasonic cleaning, it was rinsed with deionized water for 3 times, and then dried with nitrogen and placed in a vacuum drying oven for 10 minutes to obtain a pre-treated substrate, wherein the substrate is a silicon substrate;

[0060] 12 g of polydimethylsiloxane (PDMS) prepolymer and 1.2 g of curing agent (Dow Corning 184) were placed in a centrifugal mixer, first rotated forward for 1.5 min, and then reversed for 1.5 min to obtain a mixture; the mixture was poured onto the pretreated substrate, and then the substrate was fixed to a coating machine, and the coating machine was started, first pre-rotated at a speed of 500 r / min for 10 s, and then rotated at a speed of 1500 r / min for 60 s to form a PDMS coating with a thickness of about 50 μm on the surface of the substrate, and then placed on a hot stage for curing at 120° C. for 30 min to obtain a cured PDMS coating-substrate;

[0061] Step S2: Preparation of titanium dioxide nanolayer;

[0062] Add the titanium dioxide nanoparticle suspension to the liquid storage cavity of a gas brush spray gun with a diameter of 0.2 mm, apply a gas pressure of 20 kPa, start the spray gun at a distance of 15 cm above the substrate, spray the titanium dioxide nanoparticle suspension evenly onto the substrate, and place it in a drying oven at 65 ° C for drying to obtain a dried PDMS coating-substrate;

[0063] The titanium dioxide nanoparticle suspension described in step S2 is prepared according to the following steps: 0.25 g of titanium dioxide nanoparticles with an average particle size of 25 nm is added to 4.75 g of anhydrous ethanol, and an ultrasonic crusher is used to uniformly disperse the particles at a power of 300 W to obtain a titanium dioxide nanoparticle suspension with a concentration of 5%;

[0064] Step S3: grafting of photoinitiator;

[0065] Under a yellow light environment with a wavelength of 590 nm, the PDMS coating-substrate dried in step S2 is immersed in a benzophenone solution. After soaking for 10 minutes, the surface is rinsed with deionized water to remove the benzophenone not fixed on the surface, and then the surface water stains are blown away with nitrogen gas, and then placed in a drying oven at 65° C. to dry, to obtain a treated PDMS coating-substrate;

[0066] The benzophenone solution in step S3 is prepared by the following steps: 2 g of benzophenone is added to 18 g of anhydrous ethanol, and after mixing evenly, a benzophenone solution with a concentration of 10% is obtained;

[0067] Step S4: monomer polymerization grafting;

[0068] Under a yellow light environment with a wavelength of 590 nm, 4 g of monomer N-isopropylacrylamide (NIPAm) and 0.04 g of cross-linking agent N,N'-methylenebisacrylamide were dissolved in 35.96 g of deionized water; then the PDMS coating-substrate treated in step S3 was immersed in deionized water, and an ultraviolet lamp (wavelength of 365 nm, power of 500 W) was used to irradiate 15 cm above the silicon substrate for 10 minutes, and then anhydrous ethanol and deionized water were used to rinse alternately for 3 times, and then dried in a drying oven at 65°C, and finally demolded to obtain a thermosensitive hydrogel film with reversible wettability switching (such as Figure 3 shown).

[0069] Example 2: A method for preparing a temperature-sensitive hydrogel film with reversible wettability switching, comprising the following steps:

[0070] Step S1: preparing a uniform coating of polydimethylsiloxane;

[0071] A 2-inch substrate was placed in an ultrasonic cleaning machine for ultrasonic cleaning for 10 minutes, and after the ultrasonic cleaning, it was rinsed with deionized water for 3 times, and then dried with nitrogen and placed in a vacuum drying oven for 10 minutes to obtain a pre-treated substrate, wherein the substrate is a silicon substrate;

[0072] 6 g of polydimethylsiloxane (PDMS) prepolymer and 0.667 g of curing agent (Dow Corning 184) were placed in a centrifugal mixer, first rotated forward for 1.5 minutes, and then reversed for 1.5 minutes to obtain a mixture; the mixture was poured onto the pretreated substrate, and then the substrate was fixed to a coating machine, and the coating machine was started, first pre-rotated at a speed of 500 r / min for 10 seconds, and then rotated at a speed of 1500 r / min for 60 seconds to form a PDMS coating with a thickness of about 50 μm on the surface of the substrate, and then placed on a hot stage for curing at 120° C. for 30 minutes to obtain a cured PDMS coating-substrate;

[0073] Step S2: Preparation of titanium dioxide nanolayer;

[0074] Add the titanium dioxide nanoparticle suspension to the liquid storage cavity of a gas brush spray gun with a diameter of 0.2 mm, apply a gas pressure of 20 kPa, start the spray gun at a distance of 15 cm above the substrate, spray the titanium dioxide nanoparticle suspension evenly onto the substrate, and place it in a drying oven at 65 ° C for drying to obtain a dried PDMS coating-substrate;

[0075] The titanium dioxide nanoparticle suspension described in step S2 is prepared according to the following steps: 0.25 g of titanium dioxide nanoparticles with an average particle size of 25 nm is added to 4.75 g of anhydrous ethanol, and an ultrasonic crusher is used to uniformly disperse the particles at a power of 300 W to obtain a titanium dioxide nanoparticle suspension with a concentration of 5%;

[0076] Step S3: grafting of photoinitiator;

[0077] Under a yellow light environment with a wavelength of 590 nm, the PDMS coating-substrate dried in step S2 is immersed in a benzophenone solution. After soaking for 10 minutes, the surface is rinsed with deionized water to remove the benzophenone not fixed on the surface, and then the surface water stains are blown away with nitrogen gas, and then placed in a drying oven at 65° C. to dry, to obtain a treated PDMS coating-substrate;

[0078] The benzophenone solution in step S3 is prepared by the following steps: 2 g of benzophenone is added to 18 g of anhydrous ethanol, and after mixing evenly, a benzophenone solution with a concentration of 10% is obtained;

[0079] Step S4: monomer polymerization grafting;

[0080] Under a yellow light environment with a wavelength of 590 nm, 2 g of monomer N-isopropylacrylamide (NIPAm) and 0.03 g of cross-linking agent N,N'-methylenebisacrylamide were dissolved in 17.97 g of deionized water; then the PDMS coating-substrate treated in step S3 was immersed in deionized water, and an ultraviolet lamp (wavelength of 365 nm, power of 500 W) was used to irradiate 15 cm above the silicon substrate for 10 minutes, and then it was first rinsed alternately with anhydrous ethanol and deionized water for 3 times, and then placed in a drying oven at 65°C for drying, and finally demolded to obtain a thermosensitive hydrogel film with reversible wettability switching.

[0081] Example 3: A method for preparing a temperature-sensitive hydrogel film with reversible wettability switching, comprising the following steps:

[0082] Step S1: preparing a uniform coating of polydimethylsiloxane;

[0083] A 4-inch substrate was placed in an ultrasonic cleaning machine for ultrasonic cleaning for 20 minutes, and after the ultrasonic cleaning, it was rinsed with deionized water for 3 times, and then dried with nitrogen and placed in a vacuum drying oven for 20 minutes to obtain a pre-treated substrate, wherein the substrate is a silicon substrate;

[0084] 12 g of polydimethylsiloxane (PDMS) prepolymer and 1.5 g of curing agent (Dow Corning 184) were placed in a centrifugal mixer, first rotated forward for 2 minutes, and then reversed for 2 minutes to obtain a mixture; the mixture was poured onto the pretreated substrate, and then the substrate was fixed to a coating machine, and the coating machine was started, first pre-rotated at a speed of 500 r / min for 10 seconds, and then rotated at a speed of 1500 r / min for 60 seconds to form a PDMS coating with a thickness of about 50 μm on the surface of the substrate, and then placed on a hot stage for curing at 90° C. for 60 minutes to obtain a cured PDMS coating-substrate;

[0085] Step S2: Preparation of titanium dioxide nanolayer;

[0086] Add the titanium dioxide nanoparticle suspension to the liquid storage cavity of a gas brush spray gun with a diameter of 0.2 mm, apply a gas pressure of 20 kPa, start the spray gun at a distance of 15 cm above the substrate, spray the titanium dioxide nanoparticle suspension evenly onto the substrate, and place it in a drying oven at 65 ° C for drying to obtain a dried PDMS coating-substrate;

[0087] The titanium dioxide nanoparticle suspension described in step S2 is prepared according to the following steps: 0.2 g of titanium dioxide nanoparticles with an average particle size of 25 nm are added to 3.8 g of anhydrous ethanol, and an ultrasonic crusher is used to uniformly disperse the particles at a power of 300 W to obtain a titanium dioxide nanoparticle suspension with a concentration of 5%;

[0088] Step S3: grafting of photoinitiator;

[0089] Under a yellow light environment with a wavelength of 590 nm, the PDMS coating-substrate dried in step S2 is immersed in a benzophenone solution. After soaking for 10 minutes, the surface is rinsed with deionized water to remove the benzophenone not fixed on the surface, and then the surface water stains are blown away with nitrogen gas, and then placed in a drying oven at 65° C. to dry, to obtain a treated PDMS coating-substrate;

[0090] The benzophenone solution described in step S3 is prepared by the following steps: 4 g of benzophenone is added to 36 g of anhydrous ethanol, and after mixing evenly, a benzophenone solution with a concentration of 10% is obtained;

[0091] Step S4: monomer polymerization grafting;

[0092] Under a yellow light environment with a wavelength of 590 nm, 4 g of monomer N-isopropylacrylamide (NIPAm) and 0.04 g of cross-linking agent N,N'-methylenebisacrylamide were dissolved in 35.96 g of deionized water; then the PDMS coating-substrate treated in step S3 was immersed in deionized water, and an ultraviolet lamp (wavelength of 365 nm, power of 500 W) was used to irradiate 15 cm above the silicon substrate for 10 minutes, and then it was first rinsed alternately with anhydrous ethanol and deionized water for 3 times, and then placed in a drying oven at 65°C for drying, and finally demolded to obtain a thermosensitive hydrogel film with reversible wettability switching.

[0093] Example 4: A method for preparing a temperature-sensitive hydrogel film with reversible wettability switching, comprising the following steps:

[0094] Step S1: preparing a uniform coating of polydimethylsiloxane;

[0095] A substrate with a size of 75 mm×26 mm×1 mm was placed in an ultrasonic cleaning machine for ultrasonic cleaning for 20 minutes, and then rinsed with deionized water for 3 times after the ultrasonic cleaning, and then dried with nitrogen and placed in a vacuum drying oven for 20 minutes to obtain a pretreated substrate, wherein the substrate is a silicon substrate;

[0096] 5 g of polydimethylsiloxane (PDMS) prepolymer and 0.5 g of curing agent (Dow Corning 184) were placed in a centrifugal mixer, first rotated forward for 2 minutes, and then reversed for 2 minutes to obtain a mixture; the mixture was poured onto the pretreated substrate, and then the substrate was fixed to a coating machine, and the coating machine was started, first pre-rotated at a speed of 600 r / min for 12 seconds, and then rotated at a speed of 2000 r / min for 50 seconds to form a PDMS coating with a thickness of about 36 μm on the surface of the substrate, and then placed on a hot stage for curing at 90° C. for 60 minutes to obtain a cured PDMS coating-substrate;

[0097] Step S2: Preparation of titanium dioxide nanolayer;

[0098] Add the titanium dioxide nanoparticle suspension to the liquid storage cavity of a gas brush spray gun with a diameter of 0.2 mm, apply a gas pressure of 20 kPa, start the spray gun at a distance of 15 cm above the substrate, spray the titanium dioxide nanoparticle suspension evenly onto the substrate, and place it in a drying oven at 65 ° C for drying to obtain a dried PDMS coating-substrate;

[0099] The titanium dioxide nanoparticle suspension described in step S2 is prepared according to the following steps: 0.25 g of titanium dioxide nanoparticles with an average particle size of 25 nm is added to 4.75 g of anhydrous ethanol, and an ultrasonic crusher is used to uniformly disperse the particles at a power of 300 W to obtain a titanium dioxide nanoparticle suspension with a concentration of 5%;

[0100] Step S3: grafting of photoinitiator;

[0101] Under a yellow light environment with a wavelength of 590 nm, the PDMS coating-substrate dried in step S2 is immersed in a benzophenone solution. After soaking for 10 minutes, the surface is rinsed with deionized water to remove the benzophenone not fixed on the surface, and then the surface water stains are blown away with nitrogen gas, and then placed in a drying oven at 65° C. to dry, to obtain a treated PDMS coating-substrate;

[0102] The benzophenone solution in step S3 is prepared by the following steps: 2 g of benzophenone is added to 18 g of anhydrous ethanol, and after mixing evenly, a benzophenone solution with a concentration of 10% is obtained;

[0103] Step S4: monomer polymerization grafting;

[0104] Under a yellow light environment with a wavelength of 590 nm, 2 g of monomer N-isopropylacrylamide (NIPAm) and 0.02 g of cross-linking agent N,N'-methylenebisacrylamide were dissolved in 17.98 g of deionized water; then the PDMS coating-substrate treated in step S3 was immersed in deionized water, and an ultraviolet lamp (wavelength of 365 nm, power of 500 W) was used to irradiate 15 cm above the silicon substrate for 10 minutes, and then it was first rinsed alternately with anhydrous ethanol and deionized water for 3 times, and then placed in a drying oven at 70°C for drying, and finally demolded to obtain a thermosensitive hydrogel film with reversible wettability switching.

[0105] By comparing the above four examples, it is found that the mass ratio of polydimethylsiloxane, titanium dioxide nanoparticles and N-isopropylacrylamide shows different effects under different conditions. As the amount of titanium dioxide nanoparticles increases, the surface roughness of the substrate increases, and the wettability effect formed on the surface of the hydrogel film will be enhanced; as the area of ​​the substrate decreases, the amount of N-isopropylacrylamide acting on the substrate increases, and the wettability effect formed on the surface of the hydrogel film is also enhanced.

[0106] Figure 7 It represents the change of water contact angle on the hydrogel surface with the duration of ultraviolet light irradiation under the combined effect of temperature response and ultraviolet light response; Figure 7 As shown in the figure, the wettability transition is achieved by controlling the temperature to be below or above the lowest eutectic temperature (LCST≈32℃) of the thermosensitive hydrogel film. For example, at 20℃, the water contact angle on the surface of the hydrogel film is 18.6°, which is in a hydrophilic state; when the temperature is adjusted to 40℃, the water contact angle is 135°, which is in a hydrophobic state. At the same time, applying ultraviolet light irradiation of different durations can also regulate the wettability at the same time. This is because under the irradiation of ultraviolet light, the long-chain alkyl modified on the surface of TiO2 is decomposed and the surface energy is increased; and because TiO2 is a photosensitive material, photogenerated holes will be generated under the irradiation of ultraviolet light. The photogenerated holes react with lattice oxygen to generate oxygen vacancies on the surface of TiO2, and the oxygen vacancies can react with water molecules. Therefore, the hydrogel film containing TiO2 changes from hydrophobic to hydrophilic, and this transformation effect is enhanced with the increase of time.

Claims

1. A method for preparing a thermosensitive hydrogel film with reversible wettability switching, characterized in that The preparation method is carried out according to the following steps: Step S1: preparing a uniform coating of polydimethylsiloxane; Put polydimethylsiloxane and curing agent in a centrifugal mixer and mix for 3 to 4 minutes to obtain a mixture; pour the mixture onto the pretreated substrate, then fix the substrate onto a coating machine, start the coating machine, form a PDMS coating on the surface of the substrate, and then place it on a hot plate for curing to obtain a cured PDMS coating-substrate; Step S2: Preparation of titanium dioxide nanolayer; The titanium dioxide nanoparticle suspension is evenly sprayed onto the PDMS coating-substrate cured in step S1 by a spray gun, and dried to obtain a dried PDMS coating-substrate; Step S3: grafting of photoinitiator; Under a yellow light environment with a wavelength of 590 nm, the PDMS coating-substrate dried in step S2 is immersed in a benzophenone solution for 10 to 15 minutes, then rinsed and dried to obtain a treated PDMS coating-substrate; Step S4: monomer polymerization grafting; Under a yellow light environment with a wavelength of 590 nm, N-isopropyl acrylamide and a cross-linking agent N,N'-methylenebisacrylamide are dissolved in deionized water, wherein the mass ratio of the N-isopropyl acrylamide to the cross-linking agent N,N'-methylenebisacrylamide is 100:(1-1.5); then the PDMS coating-substrate treated in step S3 is immersed in deionized water, irradiated with an ultraviolet lamp for 10-20 minutes, then the substrate is rinsed and dried, and finally demolded to obtain a temperature-sensitive hydrogel film with reversible wettability switching; The mass ratio of the titanium dioxide nanoparticles to N-isopropylacrylamide in the polydimethylsiloxane and titanium dioxide nanoparticle suspension is (5-12): (0.2-0.25): (2-4).

2. The method for preparing a temperature-sensitive hydrogel film with reversible wettability switching according to claim 1, characterized in that In step S1, polydimethylsiloxane and a curing agent are placed in a centrifugal mixer, first rotated forward for 1.5 to 2 minutes, and then reversed for 1.5 to 2 minutes.

3. The method for preparing a temperature-sensitive hydrogel film with reversible wettability switching according to claim 1 or 2, characterized in that The mass ratio of the polydimethylsiloxane to the curing agent in step S1 is (8-10):1, and the curing agent is Dow Corning 184.

4. The method for preparing a temperature-sensitive hydrogel film with reversible wettability switching according to claim 1, characterized in that The pretreated substrate described in step S1 is processed according to the following steps: the substrate is placed in an ultrasonic cleaning machine for ultrasonic cleaning for 10 to 20 minutes, rinsed with deionized water 3 to 5 times after the ultrasonic cleaning, and then dried with nitrogen and placed in a vacuum drying oven at 65 to 70° C. for 10 to 20 minutes; the substrate is a silicon substrate.

5. The method for preparing a temperature-sensitive hydrogel film with reversible wettability switching according to claim 1, characterized in that In step S1, the substrate is fixed to the coating machine, and the coating machine is started. It is first pre-rotated at a speed of 500-600 r / min for 10-12 seconds, and then rotated at a speed of 1500-2000 r / min for 50-60 seconds to form a PDMS coating on the surface of the substrate, and then placed on a hot stage to cure at 90-120° C. for 20-60 minutes.

6. The method for preparing a temperature-sensitive hydrogel film with reversible wettability switching according to claim 1, characterized in that The titanium dioxide nanoparticle suspension described in step S2 is prepared according to the following steps: titanium dioxide nanoparticles with an average particle size of 25 nm are added to anhydrous ethanol, and are evenly dispersed using an ultrasonic crusher at a power of 300 W to obtain a titanium dioxide nanoparticle suspension with a concentration of 5%, wherein the mass ratio of the titanium dioxide nanoparticles to anhydrous ethanol is (0.2-0.25): (3.8-4.75); the drying temperature in step S2 is 65-70°C.

7. The method for preparing a temperature-sensitive hydrogel film with reversible wettability switching according to claim 1, characterized in that The benzophenone solution described in step S3 is prepared according to the following steps: 2 g of benzophenone is added to 18 g of anhydrous ethanol, and mixed evenly to obtain a benzophenone solution with a concentration of 10%; after rinsing with deionized water in step S3, it is placed in a drying oven at 65-70°C for drying.

8. The method for preparing a temperature-sensitive hydrogel film with reversible wettability switching according to claim 1, characterized in that In step S4, the mass ratio of N-isopropylacrylamide, cross-linking agent N,N'-methylenebisacrylamide and deionized water is 2:(0.02-0.03):(17.97-17.98).

9. The method for preparing a temperature-sensitive hydrogel film with reversible wettability switching according to claim 1, characterized in that The wavelength of the ultraviolet lamp in step S4 is 340-365nm, and the power is 300-500W; after the ultraviolet lamp irradiation in step S4, first use anhydrous ethanol and deionized water to rinse alternately 3-4 times, and then place it in a drying oven at 65-70°C to dry.

10. Use of a thermosensitive hydrogel film with reversible wettability prepared by the method according to any one of claims 1 to 9, characterized in that The application of the reversibly switchable thermosensitive hydrogel film in the preparation of drugs with temperature response and ultraviolet light response.

Citation Information

Cited By

  • Surface-modified silicone rubber composite film and preparation method thereof

    CN120157941A