Preparation method of europium modified samarium zirconate thermal barrier coating material

Thermal barrier coating was prepared by electron beam physical vapor deposition technology of europium modified samarium zirconate material, which solved the problems of insufficient life of zirconate coating and YSZ temperature limit, and achieved high phase stability and low thermal conductivity, significantly improving Performance of aircraft engine thermal barrier coating.

CN118996332AInactive Publication Date: 2024-11-22AVIC BEIJING INST OF AERONAUTICAL MATERIALS

Patent Information

Application Number
CN202411091997.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing zirconate thermal barrier coatings have insufficient service life at high temperatures and the long-term use temperature of YSZ does not exceed 1200°C, which cannot meet the needs of next-generation high-performance aero engines.

Method used

Thermal barrier coating is prepared by electron beam physical vapor deposition technology using europium modified samarium zirconate material. Thermal barrier coating with a unique columnar crystal structure is formed. Pretreatment steps such as sand blowing, cleaning, dehydration and drying to ensure cleanliness and stability of the coating.

Benefits of technology

The europium-modified zirconic acid saturated barrier coating exhibits high phase stability, low thermal conductivity and good thermal expansion coefficient at high temperatures, extending the service life of the coating, significantly improving the thermal cycle performance, and the thermal life exceeds YSZ. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118996332A_ABST
    Figure CN118996332A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of aero-engine thermal barrier coatings, and relates to a europium modified samarium zirconate thermal barrier coating material and a preparation method thereof. Performing cleaning; dehydrating and drying; the preparation method of the europium-modified samarium zirconate thermal barrier coating comprises the following steps: putting a europium-modified samarium zirconate target material into a deposition chamber of electron beam physical vapor deposition equipment; the molecular formula of the europium modified samarium zirconate target material is Eu-Sm2Zr2O7, and the weight content of Eu is 5%-15%; evaporating the europium modified samarium zirconate target material; selecting deposition process parameters: the vacuum degree lt of a deposition chamber; 5 * 10 <-4 > mbar; the beam intensity of the electron beam is 1.5-1.7 A, the evaporation time is 30-60 min, and the rotation speed is 10-20 RPM; and the evaporation time of the target material is controlled, and finally the europium-modified samarium zirconate thermal barrier coating is obtained on the rotating sample. According to the invention, the characteristics of low thermal conductivity and high service temperature of a single zirconate coating can be ensured, and the practical problems of short service life and low thermal expansion coefficient of the zirconate coating can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of thermal barrier coatings for aviation engines and relates to a method for preparing a europium-modified samarium zirconate thermal barrier coating material. Background Art

[0002] At present, with the continuous improvement of the thrust and working efficiency of gas turbines, the gas intake temperature is getting higher and higher, and the working temperature of the nickel-based high-temperature alloy used in turbine blades and other hot end components has gradually approached its service temperature limit. Thermal barrier coatings (TBCs) are a surface protection technology that utilizes the high temperature resistance, erosion resistance, corrosion resistance and low thermal conductivity of ceramic materials and combines them with metal substrates in the form of coatings to increase the working temperature of metal parts, enhance the high temperature resistance of hot end parts, extend the service life of hot end parts, and improve the working efficiency of the engine. At present, the long-term maximum use temperature of the widely used YSZ (6-8wt.% Y2O3 partially stabilized ZrO2) thermal barrier coating material cannot exceed 1200℃. During the cooling process, the volume expansion occurs due to the phase change to produce a monoclinic phase, which leads to coating failure. However, the long-term use temperature of the next generation of high-performance aircraft engine thermal barrier coating materials must exceed 1200℃. Therefore, the research of new thermal barrier coating materials has become a topic for the development of the next generation of high-performance aircraft engines. Summary of the invention

[0003] The purpose of the present invention is to provide a method for preparing a europium-modified samarium zirconate thermal barrier coating material in view of the above-mentioned deficiencies in the prior art, and the purpose is to solve the problems of insufficient service life of a single zirconate thermal barrier coating and a service temperature of YSZ not exceeding 1200°C by modifying samarium zirconate with rare earth europium.

[0004] To solve this technical problem, the technical solution of the present invention is:

[0005] A method for preparing a europium-modified samarium zirconate thermal barrier coating material, wherein the method comprises the following steps when preparing the thermal barrier coating:

[0006] Step 1: Load the europium-modified samarium zirconate target into the deposition chamber of the electron beam physical vapor deposition equipment; the europium-modified samarium zirconate target has a molecular formula of Eu-Sm2ZrO7, and the Eu weight content is 5%-15%. Preferably, the Eu weight content is 6%-10%.

[0007] Step 2: Evaporating the europium-modified samarium zirconate target in a deposition chamber to obtain a europium-modified samarium zirconate thermal barrier coating on a rotating sample.

[0008] The sample material is GH3039.

[0009] The deposition process parameters in step 2 are selected as follows:

[0010] The vacuum degree of the deposition chamber is <5×10 -4 mbar; electron beam current intensity 1.5-1.7A; evaporation time 30-60min, rotation speed: 10-20RPM.

[0011] The preparation method also includes a cooling operation after step 2, specifically: cooling the sample to below 200 degrees Celsius to obtain a europium-modified samarium zirconate thermal barrier coating on the rotating sample, and the cooling is natural cooling.

[0012] The preparation method also includes a pretreatment operation before step 1, the steps are as follows:

[0013] 1.1. Sand blasting: treat the surface of the bonding layer of the sample with pollutants. The sand particle size is 120 mesh and the compressed air pressure is 0.1-0.3MPa.

[0014] 1.2. Cleaning: Rinse the sample surface with tap water, and then soak the sample in deionized water;

[0015] 1.3. Dehydration and drying: Soak the sample in an organic solvent, then take it out and put it in an oven to dry.

[0016] In the step 1.1, a water-blown sand method is used, and the sand particles are Al2O3 sand particles or ZrO2 sand particles.

[0017] In order to ensure that the sample surface is clean and free of contamination, the rinsing time in step 1.2 is greater than or equal to 20 minutes; the immersion time is greater than or equal to 20 minutes.

[0018] In order to ensure that the sample surface is clean and free of contamination, the immersion time in step 1.3 is greater than or equal to 20 minutes.

[0019] The organic solvent in step 1.3 is anhydrous ethanol, and the purity is analytical grade or industrial grade.

[0020] The drying operation in step 1.3 is to dry at 80° C. for 30 minutes; if the temperature is too low and the time is too long, or if the temperature is too high, oxidation of the sample surface will occur.

[0021] The present invention has the following advantages and beneficial effects:

[0022] The europium-modified samarium zirconate thermal barrier coating of the present invention, as a new type of thermal barrier coating material, has no phase change after long-term heat treatment at high temperature and has high phase stability. Their thermal expansion coefficient is close to that of YSZ, and has lower thermal conductivity and better thermal expansion coefficient. At the same time, the europium-modified samarium zirconate thermal barrier coating is prepared by electron beam physical vapor deposition technology, which will make the thermal barrier coating have a unique columnar crystal structure, and the coating has better strain tolerance and better thermal cycle performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] In order to more clearly illustrate the technical solutions implemented in the present invention, the following is a brief explanation of the drawings required to be used in the examples of the present invention. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative work.

[0024] Figure 1 It is a schematic diagram of thermal conductivity of Example 1, Example 2, Example 3 and Comparative Example;

[0025] Figure 2 It is a schematic diagram of thermal expansion coefficient of Example 1, Example 2, Example 3 and Comparative Example;

[0026] Figure 3 It is a schematic diagram of thermal life of Example 1, Example 2, Example 3 and the comparative example;

[0027] Figure 4 It is a schematic diagram of the columnar crystal structure of the present invention;

[0028] Figure 5 A schematic diagram of thermal life with different Eu contents was prepared using the method of Example 2. DETAILED DESCRIPTION

[0029] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0030] The features of various aspects of the embodiments of the present invention will be described in detail below. In the following detailed description, many specific details are provided to provide a comprehensive understanding of the present invention. However, it is obvious to a person skilled in the art that the present invention can also be implemented without these specific details. The technical solution of the invention will be further described in detail below in conjunction with the embodiments:

[0031] Embodiment 1:

[0032] ⑴. Sand blasting: The surface of the bonding layer of the sample was treated with water sand blasting method. The particle size of Al2O3 sand was 120 mesh and the compressed air pressure was 0.1MPa. The material of the sample was GH3039.

[0033] ⑵. Cleaning: Rinse the sample surface with tap water for 30 minutes, and soak the sample in deionized water for 30 minutes;

[0034] ⑶, Dehydration and drying: Soak the sample in an organic solvent for 30 minutes, then take it out and put it in an oven, and dry it at 80℃ for 30 minutes. The organic solvent is anhydrous ethanol with analytical purity;

[0035] ⑷. Preparation of thermal barrier coating: Load the europium-modified samarium zirconate target into the deposition chamber of the electron beam physical vapor deposition equipment, where the Eu weight content is 5%. Obtain the Eu-Sm2ZrO7 thermal barrier coating on the rotating sample, the rotation speed is 10RPM; the deposition process parameters are: vacuum degree 3.5×10 -4 mbar, beam intensity 1.5A, evaporation time 40min, after cooling to below 200°C, the loading chamber was opened to obtain the Eu-Sm2ZrO7 thermal barrier coating.

[0036] Embodiment 2:

[0037] ⑴. Sand blasting: The surface of the bonding layer of the sample was treated with water sand blasting method. The particle size of Al2O3 sand was 120 mesh and the compressed air pressure was 0.1MPa. The material of the sample was GH3039.

[0038] ⑵. Cleaning: Rinse the sample surface with tap water for 30 minutes, and soak the sample in deionized water for 30 minutes;

[0039] ⑶, Dehydration and drying: Soak the sample in an organic solvent for 30 minutes, then take it out and put it in an oven, and dry it at 80℃ for 30 minutes. The organic solvent is anhydrous ethanol with analytical purity;

[0040] ⑷. Preparation of thermal barrier coating: Load the europium-modified samarium zirconate target into the deposition chamber of the electron beam physical vapor deposition equipment, where the Eu weight content is 10%. Obtain the Eu-Sm2ZrO7 thermal barrier coating on the rotating sample, the rotation speed is 15RPM; the deposition process parameters are: vacuum degree 2.5×10 -4 mbar, beam intensity 1.6A, evaporation time 40min, after cooling to below 200°C, the loading chamber was opened to obtain the Eu-Sm2Zr2O7 thermal barrier coating.

[0041] Embodiment 3:

[0042] ⑴. Sand blasting: The surface of the bonding layer of the sample was treated with water sand blasting method. The particle size of Al2O3 sand was 120 mesh and the compressed air pressure was 0.1MPa. The material of the sample was GH3039.

[0043] ⑵. Cleaning: Rinse the sample surface with tap water for 30 minutes, and soak the sample in deionized water for 30 minutes;

[0044] ⑶, Dehydration and drying: Soak the sample in an organic solvent for 30 minutes, then take it out and put it in an oven, and dry it at 80℃ for 30 minutes. The organic solvent is anhydrous ethanol with analytical purity;

[0045] ⑷. Preparation of thermal barrier coating: Load the europium-modified samarium zirconate target into the deposition chamber of the electron beam physical vapor deposition equipment, where the Eu weight content is 15%. Obtain the Eu-Sm2ZrO7 thermal barrier coating on the rotating sample, the rotation speed is 20RPM; the deposition process parameters are: vacuum degree 2.5×10 -4 mbar, beam intensity 1.7A, evaporation time 40min, after cooling to below 200°C, the loading chamber was opened to obtain the Eu-Sm2Zr2O7 thermal barrier coating.

[0046] Comparative Example:

[0047] ⑴. Sand blasting: The surface of the bonding layer of the sample was treated with water sand blasting method. The particle size of Al2O3 sand was 120 mesh and the compressed air pressure was 0.1MPa. The material of the sample was GH3039.

[0048] ⑵. Cleaning: Rinse the sample surface with tap water for 30 minutes, and soak the sample in deionized water for 30 minutes;

[0049] ⑶, Dehydration and drying: Soak the sample in an organic solvent for 30 minutes, then take it out and put it in an oven, and dry it at 80℃ for 30 minutes. The organic solvent is anhydrous ethanol with analytical purity;

[0050] ⑷. Preparation of thermal barrier coating: Load the europium-modified samarium zirconate target into the deposition chamber of the electron beam physical vapor deposition equipment, where the Eu weight content is 30%. Obtain the Eu-Sm2ZrO7 thermal barrier coating on the rotating sample, the rotation speed is 30RPM; the deposition process parameters are: vacuum degree 2.5×10 -4 mbar, beam intensity 1.8A, evaporation time 40min, after cooling to below 200°C, the loading chamber was opened to obtain the Eu-Sm2Zr2O7 thermal barrier coating.

[0051] It can be seen from the above examples that:

[0052] (1) In terms of preparation method, electron beam physical vapor deposition technology is used. In a high vacuum environment, high-speed electrons generated by an electron gun are used to bombard the material to be evaporated, causing it to heat up and melt, and then turn into vapor and condense on the surface of the sample. The use of electron beam physical vapor deposition technology to prepare thermal barrier coatings will give the thermal barrier coatings a unique columnar crystal structure and good thermal cycling performance.

[0053] (2) In terms of coating design, a uniform coating structure is obtained by modifying samarium zirconate with europium. The present invention can not only reduce the thermal conductivity of the zirconate coating, but also improve the practical problem of insufficient service life of a single zirconate.

[0054] from Figure 1-2 It can be seen that the thermal conductivity and thermal expansion coefficient of europium-modified samarium zirconate thermal barrier coating material decrease with the increase of Eu doping, but the key performance of thermal barrier coating is thermal life. Figure 3 As shown, Example 2 has the best lifespan, reaching 875 hours, which is greater than that of YSZ. However, the performance of the coating prepared by using materials (Eu weight content) and parameters other than the technical solution of the present invention is much different from that of Example 2. Therefore, the parameters required by the present invention (evaporation electron beam current: 1.5-1.7A, rotation speed: 10-20RPM) can maximize the improvement of thermal lifespan performance while meeting the other performance requirements.

[0055] In addition, Figure 5 As shown, in view of the difference in the weight content of Eu in the material component, the same preparation parameters as in Example 2 are adopted, but the weight content of Eu is different, and the thermal life performance obtained is different. It can be seen that when the weight content of Eu is 6%-10%, the thermal life performance of the coating has the best performance.

[0056] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the field can easily think of various equivalent modifications or substitutions within the technical scope disclosed by the present invention, and these modifications or substitutions should all be covered within the protection scope of the present invention.

Claims

1. A method for preparing a europium-modified samarium zirconate thermal barrier coating material, characterized in that: The steps of the preparation method for the thermal barrier coating are as follows: Step 1: Loading a europium-modified samarium zirconate target into a deposition chamber of an electron beam physical vapor deposition device, wherein the europium-modified samarium zirconate target has a molecular formula of Eu-Sm2ZrO7 and a Eu weight content of 5%-15%; Step 2: Evaporating the europium-modified samarium zirconate target in a deposition chamber to obtain a europium-modified samarium zirconate thermal barrier coating on a rotating sample.

2. The method for preparing the europium-modified samarium zirconate thermal barrier coating according to claim 1, characterized in that: The sample material is GH3039.

3. The method for preparing the europium-modified samarium zirconate thermal barrier coating according to claim 1, characterized in that: The deposition process parameters in step 2 are selected as follows: The vacuum degree of the deposition chamber is <5×10 -4 mbar; electron beam current intensity 1.5-1.7A; evaporation time 30-60min, rotation speed: 10-20RPM.

4. The method for preparing the europium-modified samarium zirconate thermal barrier coating according to claim 1, characterized in that: The preparation method also includes a cooling operation after step 2, specifically: cooling the sample to below 200 degrees Celsius to obtain a europium-modified samarium zirconate thermal barrier coating on the rotating sample, and the cooling is natural cooling.

5. The method for preparing the europium-modified samarium zirconate thermal barrier coating according to claim 1, characterized in that: The preparation method also includes a pretreatment operation before step 1, the steps are as follows: Step 1: Sand blasting: treat the surface of the bonding layer of the sample with pollutants, the sand particle size is 120 mesh, and the compressed air pressure is 0.1-0.3MPa; Step 2: Cleaning: Rinse the surface of the sample with tap water, and then soak the sample in deionized water; Step 3: Dehydration and drying: Soak the sample in an organic solvent, then take it out and put it in an oven to dry.

6. The method for preparing the europium-modified samarium zirconate thermal barrier coating according to claim 5, characterized in that: In the step 1, a water-blown sand method is used, and the sand particles are Al2O3 sand particles or ZrO2 sand particles.

7. The method for preparing the europium-modified samarium zirconate thermal barrier coating according to claim 5, characterized in that: In the step 2, the rinsing time is greater than or equal to 20 minutes; and the soaking time is greater than or equal to 20 minutes.

8. The method for preparing the europium-modified samarium zirconate thermal barrier coating according to claim 5, characterized in that: The soaking time in step 3 is greater than or equal to 20 minutes.

9. The method for preparing the europium-modified samarium zirconate thermal barrier coating according to claim 5, characterized in that: The organic solvent in step 3 is anhydrous ethanol, and the purity is analytical grade.

10. The method for preparing the europium-modified samarium zirconate thermal barrier coating according to claim 5, characterized in that: The specific drying operation in the step 3 is drying at 80° C. for 30 minutes.

Citation Information

Patent Citations

  • Rare-earth-based aerogel material with radiation shielding effect and heat insulation property as well as preparation and application of rare-earth-based aerogel material

    CN110563435A

  • Preparation method for thermal barrier coating of turbine working blade

    CN110791734A

  • Doped and modified rare earth zirconate powder and preparation method and application thereof

    CN112661511A

  • Lanthanum samarium zirconium oxide thermal barrier coating material and preparation method thereof

    CN115341181A

  • Preparation method of double-ceramic-layer thermal barrier coating of small-size multi-union guide blade

    CN115558894A

Cited By

  • Boron nitride fiber-based ceramic material as well as preparation method and application thereof

    CN120736912A