Gadolinium-zirconium-europium-oxygen thermal barrier coating material and preparation method thereof

By preparing gadolinium-zirconium-europium thermal barrier coatings through rare earth praseodymium doping modification, the problem of phase transformation failure of YSZ thermal barrier coatings at high temperatures was solved, achieving high-temperature stability and low thermal conductivity, thereby improving the service life and performance of hot-end components of aero-engines.

CN118996334AInactive Publication Date: 2024-11-22AVIC BEIJING INST OF AERONAUTICAL MATERIALS
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411092000.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing YSZ thermal barrier coating material has a long-term operating temperature of no more than 1200℃. During the cooling process, a phase change occurs, causing the coating to fail. In addition, its high thermal conductivity cannot meet the requirements of the next generation of high-performance aero engines.

Method used

Gadolinium zirconium europium oxygen thermal barrier coating material was prepared by rare earth praseodymium doping modification. The coating material with unique columnar crystal structure was prepared by high temperature solid-state method and electron beam physical vapor deposition technology, which reduced thermal conductivity, increased thermal expansion coefficient and enhanced phase stability.

Benefits of technology

The gadolinium-zirconium europium oxygen thermal barrier coating does not undergo phase transformation after long-term use at 1200℃, its thermal expansion coefficient is close to that of YSZ, its thermal conductivity is reduced, and it has good thermal cycling performance and fracture toughness, extending its service life by about 400 hours.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118996334A_ABST
    Figure CN118996334A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of aero-engine stealth materials, and relates to a gadolinium-zirconium-europium-oxygen thermal barrier coating material and a preparation method thereof, the molecular formula of the coating material is (Gd1-xEux) 2Zr2O7, and x is equal to 0.05-0.15; selecting deposition process parameters: the vacuum degree lt of a deposition chamber; 5 * 10 <-4 > mbar; the beam intensity of the electron beam is 1.5-1.8 A; the temperature of the sample is 1000-1050 DEG C; the evaporation time is 50 to 80 minutes; and the evaporation time is controlled, and finally the gadolinium-zirconium-europium-oxygen thermal barrier coating is obtained on the rotating sample. The thermal expansion coefficient of the thermal barrier coating material is close to that of YSZ, the thermal barrier coating material has low thermal conductivity, meanwhile, the gadolinium-zirconium-europium-oxygen thermal barrier coating is prepared through the electron beam physical vapor deposition technology, the gadolinium-zirconium-europium-oxygen thermal barrier coating has a unique columnar crystal structure, and meanwhile the gadolinium-zirconium-europium-oxygen thermal barrier coating has the long service life; the thermal conductivity of the coating can be reduced, the service temperature of the coating can be increased, and the actual problems that the service life of the coating is short and the thermal expansion coefficient is low can be solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of thermal barrier coatings for aviation engines and relates to a gadolinium zirconium europium oxide thermal barrier coating material and a preparation method thereof. Background Art

[0002] At present, with the continuous improvement of the thrust and working efficiency of gas turbines, the gas intake temperature is getting higher and higher, and the working temperature of the nickel-based high-temperature alloy used in turbine blades and other hot end components has gradually approached its service temperature limit. Thermal barrier coatings (TBCs) are a surface protection technology that utilizes the high temperature resistance, erosion resistance, corrosion resistance and low thermal conductivity of ceramic materials and combines them with metal substrates in the form of coatings to increase the working temperature of metal parts, enhance the high temperature resistance of hot end parts, extend the service life of hot end parts, and improve the working efficiency of the engine. At present, the long-term maximum use temperature of the widely used YSZ (6-8wt.% Y2O3 partially stabilized ZrO2) thermal barrier coating material cannot exceed 1200℃. During the cooling process, the volume expansion occurs due to the phase change to produce a monoclinic phase, which leads to coating failure. However, the long-term use temperature of the next generation of high-performance aircraft engine thermal barrier coating materials must exceed 1200℃. Therefore, the research of new thermal barrier coating materials has become a topic for the development of the next generation of high-performance aircraft engines. Summary of the invention

[0003] The purpose of the present invention is to provide a gadolinium zirconium europium oxide thermal barrier coating material and a preparation method thereof in view of the deficiencies of the above-mentioned prior art. The purpose is to solve the problems of insufficient service life of a single zirconium dioxide thermal barrier coating and a service temperature of YSZ not exceeding 1200°C through rare earth praseodymium doping modification, while also reducing the thermal conductivity of the material and improving the thermal expansion coefficient of the material.

[0004] To solve this technical problem, the technical solution of the present invention is:

[0005] In one aspect, a gadolinium zirconium europium oxide thermal barrier coating material is provided, wherein the molecular formula of the gadolinium zirconium europium oxide thermal barrier coating material is (Gd 1-x Eu x )2Z r2 O7, wherein x = 0.05 to 0.15. Preferably, x = 0.06 to 0.12.

[0006] On the other hand, a method for preparing the gadolinium zirconium europium oxide thermal barrier coating is provided, comprising the following steps:

[0007] Step 1, the raw materials Gd2O3, Eu2O3, and ZrO2 are mixed according to the material molecular formula ratio, and a gadolinium zirconium europium oxide target is synthesized by a high-temperature solid phase method at a synthesis temperature of 1800-2000°C;

[0008] Step 2: Use vacuum arc plating equipment to prepare NiFeCrAlHf as the metal base layer of the thermal barrier coating, with a voltage of 600-650V and a current of 15-20A;

[0009] Step three, loading the gadolinium zirconium europium oxide target into an electron beam physical vapor deposition device, evaporating the gadolinium zirconium europium oxide target by electron beam, and preparing a gadolinium zirconium europium oxide thermal barrier coating on a NiFeCrAlHf substrate, with an electron beam current intensity of 1.5-1.8A and a sample temperature of 1000-1050°C.

[0010] In the step 1, the purity of the raw materials Gd2O3, Eu2O3 and ZrO2 is ≥98%.

[0011] The raw material mixing in step 1 should be mechanically ball milled for a time of ≥ 24 hours.

[0012] The high temperature solid phase synthesis time of step 1 is ≥ 24 hours.

[0013] The vacuum degree of the vacuum arc plating equipment in step 2 is less than 1×10 -2 Pa.

[0014] The deposition time of the vacuum arc plating equipment in step 2 is ≥100 min.

[0015] The vacuum degree of the electron beam physical vapor deposition equipment in step 3 is less than 5×10 -4 mbar.

[0016] The evaporation time of the electron beam physical vapor deposition thermal barrier coating in step three is 50-80 minutes.

[0017] In the step 3, the thermal barrier coating deposited by electron beam physical vapor deposition is cooled to below 150° C. in the furnace, and the cooling is natural cooling.

[0018] The present invention has the following advantages and beneficial effects:

[0019] As a new type of thermal barrier coating material, the gadolinium zirconium europium oxide thermal barrier coating has no phase change after long-term heat treatment at 1200°C and has high phase stability. Their thermal expansion coefficient is close to that of YSZ, and they have lower thermal conductivity and better fracture toughness. At the same time, the gadolinium zirconium europium oxide thermal barrier coating is prepared by electron beam physical vapor deposition technology, which will make the gadolinium zirconium europium oxide thermal barrier coating have a unique columnar crystal structure (such as Figure 4 As shown), it also has good thermal cycling performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] In order to more clearly illustrate the technical solutions implemented in the present invention, the following is a brief explanation of the drawings required to be used in the examples of the present invention. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative work.

[0021] Figure 1 It is a schematic diagram of thermal conductivity of Example 1, Example 2, Example 3 and Comparative Example;

[0022] Figure 2 It is a schematic diagram of thermal expansion coefficient of Example 1, Example 2, Example 3 and Comparative Example;

[0023] Figure 3 It is a schematic diagram of thermal life of Example 1, Example 2, Example 3 and the comparative example;

[0024] Figure 4 It is a schematic diagram of the columnar crystal structure of the present invention;

[0025] Figure 5 A schematic diagram of thermal life with different Eu contents was prepared using the method of Example 2. DETAILED DESCRIPTION

[0026] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0027] The features of various aspects of the embodiments of the present invention will be described in detail below. In the detailed description below, many specific details are proposed to provide a comprehensive understanding of the present invention. However, it is obvious to those skilled in the art that the present invention can also be implemented without these specific details. The following description of the embodiments is only for a better understanding of the present invention by illustrating examples of the present invention. The technical solution of the present invention will be further described in detail below in conjunction with the accompanying drawings and embodiments:

[0028] The gadolinium zirconium europium oxide thermal barrier coating material of the present invention has a molecular formula of (Gd 1- x Eu x )2Z r2 O7, where x = 0.05 to 0.15.

[0029] A method for preparing a gadolinium zirconium europium oxide thermal barrier coating material coating comprises the following steps:

[0030] The raw materials Gd2O3, Eu2O3 and ZrO2 are mixed according to the material molecular formula ratio, the purity of the raw materials is ≥98%, the mixing method is mechanical ball milling, and the time is ≥24 hours; the praseodymium-modified zirconium dioxide target is synthesized by high-temperature solid phase method, the synthesis temperature is 1800-2000°C, and the synthesis time is ≥24 hours; NiFeCrAlHf is prepared as the metal bottom layer of the thermal barrier coating by vacuum arc plating equipment (the specific composition is consistent in the embodiment), and the vacuum degree is <1×10 -2 Pa, voltage is 600-650V, current is 15-20A, deposition time is ≥100min; the prepared target material is loaded into the electron beam physical vapor deposition equipment, and the vacuum degree is <5×10 -4 mbar, the electron beam current intensity is 1.5-1.8A, the evaporation time is 50-80min, the thermal barrier coating is prepared, and the furnace is naturally cooled to below 150°C.

[0031] Embodiment 1:

[0032] ⑴. Raw material ratio: According to the chemical formula of gadolinium zirconium europium oxide thermal barrier coating material (Gd0.95Eu0.05)2Zr2O7, weigh the raw materials Gd2O3, Eu2O3, and ZrO2.

[0033] (2) High temperature solid phase synthesis: The raw materials were mechanically ball milled for 30 hours, and the gadolinium zirconium europium oxide target was synthesized by a 1900°C high temperature solid phase method for 30 hours;

[0034] (3) Preparation of bottom layer: NiFeCrAlHf is prepared as the metal bottom layer of thermal barrier coating by vacuum arc plating equipment (the specific composition of the bottom layer is Ni20Fe20Cr20Al20Hf20), and the vacuum degree is <1×10 -2 Pa, voltage is 625 V, current is 18 A, and deposition time is 150 min;

[0035] (4) Preparation of thermal barrier coating: Load the gadolinium zirconium europium oxide target into the electron beam physical vapor deposition equipment. Deposition process parameters: vacuum degree <5×10 -4 mbar, electron beam current intensity 1.6A, evaporation time 70min, after cooling to below 100 degrees Celsius, turn on the deposition equipment to obtain the gadolinium zirconium europium oxide thermal barrier coating.

[0036] Embodiment 2:

[0037] ⑴. Raw material ratio: According to the chemical formula of gadolinium zirconium europium oxide thermal barrier coating material (Gd0.9Eu0.1)2Zr2O7, weigh the raw materials Gd2O3, Eu2O3, and ZrO2.

[0038] (2) High temperature solid phase synthesis: The raw materials were mechanically ball milled for 36 hours, and the gadolinium zirconium europium oxide target was synthesized by a high temperature solid phase method at 1800°C for 26 hours;

[0039] (3) Bottom layer preparation: NiFeCrAlHf is prepared as the metal bottom layer of the thermal barrier coating using vacuum arc plating equipment, with a vacuum degree of <1×10 -2 Pa, voltage is 645 V, current is 16 A, and deposition time is 125 min;

[0040] (4) Preparation of thermal barrier coating: Load the gadolinium zirconium europium oxide target into the electron beam physical vapor deposition equipment. Deposition process parameters: vacuum degree <5×10 -4 mbar, electron beam current intensity 1.7A, evaporation time 60min, after cooling to below 100 degrees Celsius, turn on the deposition equipment to obtain the gadolinium zirconium europium oxide thermal barrier coating.

[0041] Embodiment 3:

[0042] ⑴. Raw material ratio: According to the chemical formula of gadolinium zirconium europium oxide thermal barrier coating material (Gd0.85Eu0.15)2Zr2O7, weigh the raw materials Gd2O3, Eu2O3, and ZrO2.

[0043] (2) High temperature solid phase synthesis: The raw materials were mechanically ball milled for 40 hours, and the gadolinium zirconium europium oxide target was synthesized by a high temperature solid phase method at 1700°C for 24 hours;

[0044] (3) Bottom layer preparation: NiFeCrAlHf is prepared as the metal bottom layer of the thermal barrier coating using vacuum arc plating equipment, with a vacuum degree of <1×10 -2 Pa, voltage 645 V, current 17 A, deposition time 125 min;

[0045] (4) Preparation of thermal barrier coating: Load the gadolinium zirconium europium oxide target into the electron beam physical vapor deposition equipment. Deposition process parameters: vacuum degree <5×10 -4 mbar, electron beam current intensity 1.8A, evaporation time 50min, after cooling to below 100 degrees Celsius, turn on the deposition equipment to obtain the gadolinium zirconium europium oxide thermal barrier coating.

[0046] Comparative Example:

[0047] ⑴. Raw material ratio: According to the chemical formula of gadolinium zirconium europium oxide thermal barrier coating material (Gd0.5Eu0.5)2Zr2O7, weigh the raw materials Gd2O3, Eu2O3, and ZrO2.

[0048] (2) High temperature solid phase synthesis: The raw materials were mechanically ball milled for 20 hours, and the gadolinium zirconium europium oxide target was synthesized by 1800°C high temperature solid phase method for 24 hours;

[0049] (3) Preparation of bottom layer: NiFeCrAlHf is prepared as the metal bottom layer of thermal barrier coating using vacuum arc plating equipment (the specific composition of the bottom layer is Ni20Fe20Cr20Al20Hf20), and the vacuum degree is <1×10 -2 Pa, voltage 680 V, current 20 A, deposition time 100 min;

[0050] (4) Preparation of thermal barrier coating: Load the gadolinium zirconium europium oxide target into the electron beam physical vapor deposition equipment. Deposition process parameters: vacuum degree <5×10 -4 mbar, electron beam current intensity 1.2A, evaporation time 100min, after cooling to below 100 degrees Celsius, turn on the deposition equipment to obtain the gadolinium zirconium europium oxide thermal barrier coating.

[0051] It can be seen from the above examples that:

[0052] (1) The use of electron beam physical vapor deposition technology to prepare thermal barrier coatings will give the thermal barrier coatings a unique columnar crystal structure and better thermal cycling performance.

[0053] (2) In terms of coating design, a uniform coating structure is obtained through the composite modification of gadolinium zirconium europium oxide. The present invention can not only reduce the thermal conductivity of the zirconium dioxide coating (by about 30%), but also improve the actual problem of insufficient service life of single zirconium dioxide (by about 400 hours).

[0054] from Figure 1-3 It can be seen that the thermal conductivity and thermal expansion coefficient of the Gadolinium Zirconium Europium Oxide thermal barrier coating material decrease with the increase of Eu doping, but the key performance of the thermal barrier coating is the thermal life. Figure 3 As shown, Example 2 has the best lifespan, reaching 1050 hours, which is greater than that of YSZ. However, the thermal lifespan performance of the parameters and material components other than the technical solution of the present invention is quite different from that of Example 2. Therefore, the parameter combination of the present invention (electron beam current intensity 1.5-1.8A, sample temperature 1000-1050°C) can maximize the improvement of thermal lifespan performance while meeting the other performance requirements.

[0055] In addition, Figure 5 As shown, for the material composition (Gd 1-x Eu x )2Z r2 The difference in Eu content in O7, using the same parameters as in the preparation method of Example 2, we found that due to the different Eu atomic ratios, the thermal life performance obtained was different. When x = 0.06 ~ 0.12, the thermal life performance of the coating has the best performance.

[0056] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the field can easily think of various equivalent modifications or substitutions within the technical scope disclosed by the present invention, and these modifications or substitutions should all be covered within the protection scope of the present invention.

Claims

1. A gadolinium zirconium europium oxide thermal barrier coating material, characterized in that: The molecular formula of the gadolinium zirconium europium oxide thermal barrier coating material is (Gd 1-x Eu x )2Z r2 O7, where x = 0.05 to 0.

15.

2. The method for preparing the gadolinium zirconium europium oxide thermal barrier coating according to claim 1, characterized in that: The following steps are involved: Step 1, the raw materials Gd2O3, Eu2O3, and ZrO2 are mixed according to the material molecular formula ratio, and a gadolinium zirconium europium oxide target is synthesized by a high-temperature solid phase method at a synthesis temperature of 1800-2000°C; Step 2: Use vacuum arc plating equipment to prepare NiFeCrAlHf as the metal base layer of the thermal barrier coating, with a voltage of 600-650V and a current of 15-20A; Step three, loading the gadolinium zirconium europium oxide target into an electron beam physical vapor deposition device, evaporating the gadolinium zirconium europium oxide target by electron beam, and preparing a gadolinium zirconium europium oxide thermal barrier coating on a NiFeCrAlHf substrate, with an electron beam current intensity of 1.5-1.8A and a sample temperature of 1000-1050°C.

3. The preparation method according to claim 2, characterized in that: In the step 1, the purity of the raw materials Gd2O3, Eu2O3 and ZrO2 is ≥98%.

4. The preparation method according to claim 2, characterized in that: The raw material mixing in step 1 should be mechanically ball milled for a time of ≥ 24 hours.

5. The preparation method according to claim 2, characterized in that: The high temperature solid phase synthesis time of step 1 is ≥ 24 hours.

6. The preparation method according to claim 2, characterized in that: The vacuum degree of the vacuum arc plating equipment in step 2 is less than 1×10 -2 Pa.

7. The preparation method according to claim 2, characterized in that: The deposition time of the vacuum arc plating equipment in step 2 is ≥100 min.

8. The preparation method according to claim 2, characterized in that: The vacuum degree of the electron beam physical vapor deposition equipment in step 3 is less than 5×10 -4 mbar.

9. The preparation method according to claim 2, characterized in that: The evaporation time of the electron beam physical vapor deposition thermal barrier coating in step three is 50-80 minutes.

10. The preparation method according to claim 2, characterized in that: In the step 3, the thermal barrier coating deposited by electron beam physical vapor deposition is cooled to below 150° C. in the furnace, and the cooling is natural cooling.

Citation Information

Patent Citations

  • Doped and modified rare earth zirconate powder and preparation method and application thereof

    CN112661511A

  • Dysprosium-doped gadolinium zirconate thermal barrier coating material and preparation method of coating

    CN113373408A

  • Gadolinium samarium zirconium oxide thermal barrier coating material and preparation method of coating

    CN113403580A

  • Lanthanum gadolinium samarium-based high-entropy thermal barrier coating and preparation method thereof

    CN115161595A

  • Lanthanum-zirconium-praseodymium-oxygen thermal barrier coating material and preparation method thereof

    CN115341174A