Poly (p-dioxanone)-based Janus fiber membrane as well as preparation method and application thereof

By using electrospinning technology to composite hydrophilic, transition, and hydrophobic layers into a poly(p-dioxanone)-based Janus fiber membrane, the problem of unstable interfacial bonding in Janus fiber membranes was solved, achieving steady-state flow and unidirectional moisture-wicking properties, making it suitable for medical wound dressings.

CN118996723APending Publication Date: 2024-11-22TIANJIN UNIV OF SCI & TECH

Patent Information

Application Number
CN202411106693.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The hydrophilic and hydrophobic layers in existing Janus fiber membranes are not well bonded at the interface, which causes the liquid to easily separate at the interface and makes it impossible to achieve steady-state flow.

Method used

A polydioxanone-based Janus fiber membrane was synthesized layer by layer using electrospinning technology. The membrane consists of a hydrophilic layer, an intrinsic transition layer, and a hydrophobic layer. A stable multilayer structure was formed by dispersing inorganic nanoparticles in the hydrophilic fiber membrane and using a biodegradable polymer in the hydrophobic layer.

Benefits of technology

It achieves stable interfacial bonding of Janus fiber membranes, has unidirectional moisture-wicking function, is suitable for medical wound dressings, and improves the steady-state flow performance of liquids at the interface.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118996723A_ABST
    Figure CN118996723A_ABST
Patent Text Reader

Abstract

The invention discloses a poly (p-dioxanone)-based Janus fiber membrane as well as a preparation method and an application of the poly (p-dioxanone)-based Janus fiber membrane. The Janus fiber membrane is formed by compounding a poly (p-dioxanone) fiber membrane added with hydrophilic inorganic nanoparticles as a hydrophilic layer, poly (p-dioxanone) fibers as an intrinsic transition layer and a fiber membrane prepared from a hydrophobic biodegradable polymer as a hydrophobic layer in an electrostatic spinning mode layer by layer. The chemical structure design of each composite layer is matched with an electrostatic spinning forming mode, so that the problem of obvious interface layering of the existing Janus fiber membrane is effectively solved, the composite structure also realizes a one-way moisture conduction function of the Janus fiber membrane, and the hydrophilic layer and the hydrophobic layer are stably combined through a connecting interface of the intrinsic transition layer, so that the composite structure has a good moisture conduction function. Good application and popularization prospects are realized in the field of preparation of medical wound dressings.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of biomedical materials, and in particular to a polydioxanone-based Janus fiber membrane and a preparation method and application thereof. Background Art

[0002] Polydioxanone is an aliphatic polyether ester. The unique ether bonds in the main chain of the molecule give the polymer outstanding flexibility, and the ester bonds in the main chain of the molecule give the polymer excellent biodegradability, biocompatibility and absorbability. It is a medical biodegradable material that has been strictly tested and certified, and has broad prospects in the fields of medical dressings in the future.

[0003] The Janus structure is a structure with asymmetric wettability. It can spontaneously move liquid from one side to the other side according to the theory of wettability gradient or pore size gradient, and shows great potential in realizing unidirectional moisture-conducting wound dressings. The published patent CN116115813A proposes a composite dressing with continuous unidirectional moisture-conducting ability and a preparation method. The patent sets a hydrophobic silk fiber membrane and a hydrophilic electrospun cellulose membrane on both sides of a super absorbent sponge, and then sprays a graphene oxide dispersion onto the surface of the hydrophilic membrane, thereby realizing unidirectional continuous transport of wound exudate. The published patent CN118326616A proposes a method for preparing a unidirectional moisture-conducting nanofiber membrane with a porous Janus structure. The patent prepares a Janus structure that is both hydrophilic and hydrophobic by electrospinning a hydrophobic fiber membrane on the surface of a post-treated hydrophilic porous structure fiber membrane.

[0004] However, the above patents do not solve the problem that Janus fiber membranes composed of heterogeneous materials with greatly different wetting properties are prone to stratification at the interface and cannot ensure the steady flow of liquid at the interface. Therefore, solving the stability of the interface bonding between the hydrophilic layer and the hydrophobic layer in the Janus fiber membrane has become a technical problem in this field. Summary of the invention

[0005] The object of the present invention is to provide a polydioxanone-based Janus fiber membrane that solves the above-mentioned technical problems.

[0006] Another object of the present invention is to provide a method for preparing a polydioxanone-based Janus fiber membrane.

[0007] Another object of the present invention is to provide an application of a polydioxanone-based Janus fiber membrane.

[0008] To this end, the technical solution of the present invention is as follows:

[0009] A polydioxanone-based Janus fiber membrane is composited by sequentially arranged hydrophilic layer fiber membrane, intrinsic transition layer fiber membrane and hydrophobic layer fiber membrane; wherein the hydrophilic layer fiber membrane is formed by electrostatic spinning of polydioxanone spinning solution dispersed with hydrophilic inorganic nanoparticles; the intrinsic transition layer fiber membrane is formed by electrostatic spinning of polydioxanone spinning solution on the base membrane with the hydrophilic layer fiber membrane as the base membrane; and the hydrophobic layer fiber membrane is formed by electrostatic spinning of hydrophobic biodegradable polymer spinning solution on the surface of the polydioxanone intrinsic transition layer fiber membrane.

[0010] In the polydioxanone-based Janus fiber membrane, the thickness of the hydrophilic layer fiber membrane ranges from 200μm to 500μm, the fiber diameter in the membrane ranges from 0.2μm to 1.5μm, and the membrane pore size ranges from 20μm to 40μm; the thickness of the intrinsic transition layer fiber membrane ranges from 100μm to 200μm, the fiber diameter in the membrane ranges from 0.5μm to 2μm, and the membrane pore size ranges from 10μm to 20μm; the thickness of the hydrophobic layer fiber membrane ranges from 1μm to 100μm, the fiber diameter in the membrane ranges from 0.5μm to 5μm, and the membrane pore size ranges from 1μm to 10μm.

[0011] A method for preparing a polydioxanone-based Janus fiber membrane, the specific steps of which are:

[0012] S1. Preparation of hydrophilic layer fiber membrane:

[0013] Dissolving polydioxanone in an organic solvent I to prepare a polydioxanone spinning solution with a solid content of 5 wt.% to 20 wt.%; uniformly dispersing 0.1 wt.% to 20 wt.% of hydrophilic inorganic nanoparticles in the polydioxanone spinning solution, and forming a hydrophilic layer polydioxanone / hydrophilic inorganic nanoparticle fiber membrane by electrospinning;

[0014] S2. Preparation of polydioxanone intrinsic transition layer fiber membrane:

[0015] Taking the hydrophilic layer polydioxanone / hydrophilic inorganic nanoparticle fiber membrane prepared in step S1 as the substrate, depositing the polydioxanone spinning solution onto the surface of the hydrophilic layer by electrospinning to obtain a polydioxanone intrinsic transition layer fiber membrane;

[0016] S3. Preparation of hydrophobic layer fiber membrane:

[0017] The hydrophobic biodegradable polymer is dissolved in an organic solvent II to prepare a 5wt.% to 25wt.% hydrophobic biodegradable polymer spinning solution, and the spinning solution is electrospinned on the surface of the polydioxanone intrinsic transition layer fiber membrane prepared in step S2 to form a hydrophobic layer fiber membrane, thereby obtaining a polydioxanone-based Janus fiber membrane.

[0018] Preferably, in step S1, the organic solvent I is any one of hexafluoroisopropanol, chloroform, dimethyl sulfoxide or tetrachlorophenol, or a combination of two or more thereof. Among them, the organic solvent I is preferably hexafluoroisopropanol, and polydioxanone has the best solubility in hexafluoroisopropanol.

[0019] Preferably, the polydioxanone has a viscosity average molecular weight of 1.1×10 4 ~9.9×10 4 of polydioxanone.

[0020] Preferably, the hydrophilic inorganic nanoparticles are any one of cellulose nanocrystals, hydrophilic silicon dioxide, hydrophilic magnesium oxide, molybdenum oxide, titanium dioxide, and silver nanoparticles, or a mixture of two or more thereof.

[0021] Preferably, the particle size of the hydrophilic inorganic nanoparticles is in the range of 1 nm to 100 nm.

[0022] Preferably, in step S1, the electrospinning conditions are set as follows: spinning voltage of 15 kV to 20 kV, feed rate of 0.1 mL / h to 1.5 mL / h, spinning distance of 10 cm to 20 cm, collection roller speed of 100 r / min to 500 r / min, and spinning time of 1 h to 6 h.

[0023] Preferably, in step S2, the electrospinning conditions are set as follows: spinning voltage of 15 kV to 20 kV, feed rate of 0.1 mL / h to 1.5 mL / h, spinning distance of 10 cm to 20 cm, collection roller speed of 100 r / min to 500 r / min, and spinning time of 30 min to 60 min.

[0024] Preferably, in step S3, the hydrophobic biodegradable polymer includes any one or a combination of two or more of polylactic acid, poly-ε-caprolactone, poly-3-hydroxyalkanoate or polybutylene succinate.

[0025] Preferably, in step S3, the electrospinning conditions are set as follows: spinning voltage of 15 kV to 20 kV, feed rate of 0.1 mL / h to 1.5 mL / h, spinning distance of 10 cm to 20 cm, collection roller speed of 100 r / min to 500 r / min, and spinning time of 15 min to 30 min.

[0026] In the present invention, by controlling the electrospinning conditions in steps S1 to S3, the diameters of different fibers in the membrane, the size of the membrane pores, and the membrane thickness are regulated to adjust the membrane properties of the polydioxanone-based Janus fiber membrane.

[0027] Preferably, in step S3, the organic solvent II is one or a mixture of two or more of hexafluoroisopropanol, dichloromethane, chloroform, dimethyl sulfoxide, dimethylformamide, acetone or tetrahydrofuran in any proportion.

[0028] An application of the polydioxanone-based Janus fiber membrane is specifically to use the polydioxanone-based Janus fiber membrane for the preparation of medical wound dressings.

[0029] Compared with the prior art, the polydioxanone-based Janus fiber membrane is formed by electrospinning a polydioxanone fiber membrane with added hydrophilic inorganic nanoparticles as a hydrophilic layer, a polydioxanone fiber as an intrinsic transition layer and a fiber membrane prepared from a hydrophobic biodegradable polymer as a hydrophobic layer. The chemical structure design of each composite layer is combined with the electrospinning formation method to effectively solve the problem of obvious interface stratification of the existing Janus fiber membrane, and realize the preparation of a multilayer structure with a stable interface bonding jointly constructed by electrospinning a hydrophilic layer, an intrinsic transition layer and a hydrophobic layer layer by layer. In addition, the composite structure also realizes the unidirectional moisture conduction function of the Janus fiber membrane, and because the connection interface between the hydrophilic layer and the hydrophobic layer through the intrinsic transition layer is stable, it has good application and promotion prospects in the field of medical wound dressing preparation. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 The SEM image of the hydrophilic layer fiber membrane in the polydioxanone-based Janus fiber membrane of the present invention and its fiber diameter distribution diagram;

[0031] Figure 2 This is a test result diagram of the surface wettability of the hydrophilic layer fiber membrane in the polydioxanone-based Janus fiber membrane prepared in Example 1 of the present invention;

[0032] Figure 3 This is a SEM image of the hydrophobic layer fiber membrane formed in step S3 during the preparation of the polydioxanone-based Janus fiber membrane of Example 1 of the present invention;

[0033] Figure 4 This is a test result diagram of the surface wettability of the hydrophobic layer fiber membrane in the polydioxanone-based Janus fiber membrane prepared in Example 1 of the present invention;

[0034] Figure 5 This is a cross-sectional SEM image of the polydioxanone-based Janus fiber membrane prepared in Example 1 of the present invention;

[0035] Figure 6 This is a test graph of the unidirectional moisture conduction performance of the polydioxanone-based Janus fiber membrane prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0036] The present invention will be further described below in conjunction with the accompanying drawings and specific embodiments, but the following embodiments are by no means intended to limit the present invention in any way.

[0037] Example 1

[0038] A polydioxanone-based Janus fiber membrane is prepared by the following steps:

[0039] S1. Preparation of hydrophilic layer fiber membrane:

[0040] The viscosity average molecular weight is 8.4×10 4 Polydioxanone is dissolved in hexafluoroisopropanol, and mechanically stirred at room temperature until completely dissolved to prepare a polydioxanone / hexafluoroisopropanol spinning solution with a solid content of 18 wt.%;

[0041] 15 wt.% of cellulose nanocrystal nanoparticles were added to the poly(p-dioxanone) / hexafluoroisopropanol) spinning solution, mechanically stirred at room temperature until uniformly dispersed, and allowed to stand for degassing for 4 h. The electrospinning voltage was set to 18 kV, the feed rate was 0.3 mL / h, the receiving distance was 18 cm, the collection roller speed was 200 r / min, and the spinning time was 1.5 h. The hydrophilic layer poly(p-dioxanone) / cellulose nanocrystal fiber membrane was prepared by electrospinning.

[0042] S2. Preparation of polydioxanone intrinsic transition layer fiber membrane:

[0043] Taking the hydrophilic layer polydioxanone / cellulose nanocrystal fiber membrane as the substrate, a polydioxanone / hexafluoroisopropanol spinning solution with a solid content of 18wt.% is deposited on the surface of the hydrophilic layer by electrospinning to obtain a polydioxanone intrinsic transition layer fiber membrane; wherein the spinning voltage is set to 18kV, the feed rate is set to 0.3mL / h, the receiving distance is set to 18cm, the collection roller speed is set to 200r / min, and the spinning time is set to 40min;

[0044] S3. Preparation of hydrophobic layer fiber membrane:

[0045] The hydrophobic biodegradable polylactic acid was dissolved in hexafluoroisopropanol solvent to prepare a 10 wt.% spinning solution, mechanically stirred at room temperature until completely dissolved, and then allowed to stand for degassing for 4 hours;

[0046] Electrospinning of polylactic acid is performed on the surface of the polydioxanone intrinsic transition layer fiber membrane obtained in step S2, and after the solvent evaporates, a polydioxanone-based Janus fiber membrane is obtained; wherein the spinning voltage of the electrospinning is set to 18 kV, the feed rate is 0.1 mL / h, the spinning distance is 18 cm, the collection roller speed is 200 r / min, and the spinning time is 15 min.

[0047] Example 2

[0048] A method for preparing a polydioxanone-based Janus fiber membrane comprises the following steps:

[0049] S1. Preparation of hydrophilic layer fiber membrane:

[0050] The viscosity average molecular weight is 5.6×10 4 Polydioxanone is dissolved in hexafluoroisopropanol, and mechanically stirred at room temperature until completely dissolved to prepare a polydioxanone / hexafluoroisopropanol spinning solution with a solid content of 18 wt.%;

[0051] 10 wt.% of hydrophilic silica nanoparticles were added to the polydioxanone / hexafluoroisopropanol spinning solution, mechanically stirred at room temperature until uniformly dispersed, and allowed to stand for degassing for 4 h. The electrospinning voltage was set to 20 kV, the feed rate was 0.3 mL / h, the receiving distance was 15 cm, the collection roller speed was 300 r / min, and the spinning time was 2 h. The hydrophilic polydioxanone / silica membrane was prepared by electrospinning.

[0052] S2. Preparation of polydioxanone intrinsic transition layer fiber membrane:

[0053] Taking the hydrophilic layer polydioxanone / silicon dioxide fiber membrane as the substrate, a polydioxanone / hexafluoroisopropanol spinning solution with a solid content of 18wt.% is deposited on the surface of the hydrophilic layer by electrospinning to obtain a polydioxanone intrinsic transition layer fiber membrane; wherein the spinning voltage is set to 20kV, the feed rate is set to 0.2mL / h, the receiving distance is set to 15cm, the collection roller speed is set to 300r / min, and the spinning time is set to 40min;

[0054] S3. Preparation of hydrophobic layer fiber membrane:

[0055] The hydrophobic biodegradable poly-ε-caprolactone was dissolved in dichloromethane solvent to prepare a 15 wt.% spinning solution, mechanically stirred at room temperature until completely dissolved, and then allowed to stand for degassing for 4 hours;

[0056] Electrospinning of poly-ε-caprolactone is performed on the surface of the polydioxanone intrinsic transition layer fiber membrane obtained in step S2, and after the solvent evaporates, a polydioxanone-based Janus fiber membrane is obtained; wherein the spinning voltage of the electrospinning is 20 kV, the feed rate is 0.2 mL / h, the spinning distance is 15 cm, the collection roller speed is 300 r / min, and the spinning time is 20 min.

[0057] Example 3

[0058] A method for preparing a polydioxanone-based Janus fiber membrane comprises the following steps:

[0059] S1. Preparation of hydrophilic layer fiber membrane:

[0060] The viscosity average molecular weight is 3.6×10 4 Polydioxanone is dissolved in hexafluoroisopropanol, and mechanically stirred at room temperature until completely dissolved to prepare a polydioxanone / hexafluoroisopropanol spinning solution with a solid content of 18 wt.%;

[0061] 10 wt.% of hydrophilic titanium dioxide nanoparticles were added to the polydioxanone / hexafluoroisopropanol spinning solution, mechanically stirred at room temperature until uniformly dispersed, and allowed to stand for degassing for 4 hours. The electrospinning voltage was set to 20 kV, the feed rate was 1 mL / h, the receiving distance was 15 cm, the collection roller speed was 500 r / min, and the spinning time was 3 hours. The hydrophilic layer polydioxanone / titanium dioxide fiber membrane was prepared by electrospinning.

[0062] S2. Preparation of polydioxanone intrinsic transition layer fiber membrane:

[0063] Taking the hydrophilic layer polydioxanone / titanium dioxide fiber membrane as the substrate, a polydioxanone / hexafluoroisopropanol spinning solution with a solid content of 18wt.% is deposited on the surface of the hydrophilic layer by electrospinning to obtain a polydioxanone intrinsic transition layer fiber membrane; wherein the spinning voltage is 18kV, the feed rate is 0.1mL / h, the receiving distance is 18cm, the collection roller speed is 500r / min, and the spinning time is 40min;

[0064] S3. Preparation of hydrophobic layer fiber membrane:

[0065] The hydrophobic biodegradable poly 3-hydroxyalkanoate was dissolved in hexafluoroisopropanol solvent to prepare a 25 wt.% spinning solution, mechanically stirred at room temperature until completely dissolved, and then allowed to stand for degassing for 4 hours;

[0066] Electrospinning of poly (3-hydroxyalkanoate) was performed on the surface of the poly (dioxanone) intrinsic transition layer fiber membrane obtained in step S2, and after the solvent evaporated, a poly (dioxanone)-based Janus fiber membrane was obtained; wherein the spinning voltage of the electrospinning was 20 kV, the feed rate was 1 mL / h, the spinning distance was 15 cm, the collection roller speed was 500 r / min, and the spinning time was 5 min.

[0067] Example 4

[0068] A method for preparing a polydioxanone-based Janus fiber membrane comprises the following steps:

[0069] S1. Preparation of hydrophilic layer fiber membrane:

[0070] The viscosity average molecular weight is 8.4×10 4Polydioxanone is dissolved in hexafluoroisopropanol, and mechanically stirred at room temperature until completely dissolved to prepare a polydioxanone / hexafluoroisopropanol spinning solution with a solid content of 18 wt.%;

[0071] 1 wt.% of hydrophilic magnesium oxide nanoparticles were added to the polydioxanone / hexafluoroisopropanol spinning solution, mechanically stirred at room temperature until uniformly dispersed, and allowed to stand for degassing for 4 hours. The electrospinning voltage was set to 15 kV, the feed rate was 0.1 mL / h, the receiving distance was 10 cm, the collection roller speed was 100 r / min, and the spinning time was 3 hours. The hydrophilic layer polydioxanone / magnesium oxide fiber membrane was prepared by electrospinning.

[0072] S2. Preparation of polydioxanone intrinsic transition layer fiber membrane:

[0073] Taking the hydrophilic layer polydioxanone / magnesium oxide fiber membrane as the substrate, a polydioxanone / hexafluoroisopropanol spinning solution with a solid content of 18wt.% is deposited on the surface of the hydrophilic layer by electrospinning to obtain a polydioxanone intrinsic transition layer fiber membrane; wherein the spinning voltage is 18kV, the feed rate is 0.05mL / h, the receiving distance is 18cm, the collection roller speed is 200r / min, and the spinning time is 40min;

[0074] S3. Preparation of hydrophobic layer fiber membrane:

[0075] The hydrophobic biodegradable polybutylene succinate was dissolved in chloroform solvent to prepare a 5wt.% spinning solution, mechanically stirred at room temperature until completely dissolved, and then allowed to stand for degassing for 4 hours;

[0076] Electrospinning of polybutylene succinate is performed on the surface of the polydioxanone intrinsic transition layer fiber membrane obtained in step S2, and after the solvent evaporates, a polydioxanone-based Janus fiber membrane is obtained; wherein the spinning voltage of the electrospinning is 15 kV, the feed rate is 0.1 mL / h, the spinning distance is 10 cm, the collection roller speed is 200 r / min, and the spinning time is 10 min.

[0077] Example 5

[0078] A method for preparing a polydioxanone-based Janus fiber membrane comprises the following steps:

[0079] S1. Preparation of hydrophilic layer fiber membrane:

[0080] The viscosity average molecular weight is 2.1×10 4 Polydioxanone is dissolved in hexafluoroisopropanol, and mechanically stirred at room temperature until completely dissolved to prepare a polydioxanone / hexafluoroisopropanol spinning solution with a solid content of 20 wt.%;

[0081] 5 wt.% of hydrophilic molybdenum oxide nanoparticles were added to the polydioxanone / hexafluoroisopropanol spinning solution, mechanically stirred at room temperature until uniformly dispersed, and allowed to stand for degassing for 4 hours. The electrospinning voltage was set to 15 kV, the feed rate was 0.5 mL / h, the receiving distance was 15 cm, the collection roller speed was 200 r / min, and the spinning time was 3 hours. The hydrophilic layer polydioxanone / molybdenum oxide fiber membrane was prepared by electrospinning.

[0082] S2. Preparation of polydioxanone intrinsic transition layer fiber membrane:

[0083] Taking the hydrophilic layer polydioxanone / molybdenum oxide fiber membrane as the substrate, a polydioxanone / hexafluoroisopropanol spinning solution with a solid content of 18wt.% is deposited on the surface of the hydrophilic layer by electrospinning to obtain a polydioxanone intrinsic transition layer fiber membrane; wherein the spinning voltage is 18kV, the feed rate is 0.01mL / h, the receiving distance is 18cm, the collection roller speed is 200r / min, and the spinning time is 30min;

[0084] S3. Preparation of hydrophobic layer fiber membrane:

[0085] The hydrophobic biodegradable polylactic acid was dissolved in hexafluoroisopropanol solvent to prepare a 5wt.% spinning solution, mechanically stirred at room temperature until completely dissolved, and then allowed to stand for degassing for 4 hours;

[0086] Electrospinning of polylactic acid is performed on the surface of the polydioxanone intrinsic transition layer fiber membrane obtained in step S2, and after the solvent evaporates, a polydioxanone-based Janus fiber membrane is obtained; wherein the spinning voltage of the electrospinning is 15 kV, the feed rate is 0.1 mL / h, the spinning distance is 15 cm, the collection roller speed is 200 r / min, and the spinning time is 15 min.

[0087] Example 6

[0088] A method for preparing a polydioxanone-based Janus fiber membrane comprises the following steps:

[0089] S1. Preparation of hydrophilic layer fiber membrane:

[0090] The viscosity average molecular weight is 8.4×10 4 Polydioxanone is dissolved in hexafluoroisopropanol, and mechanically stirred at room temperature until completely dissolved to prepare a polydioxanone / hexafluoroisopropanol spinning solution with a solid content of 15 wt.%;

[0091] A mixture of 3 wt.% of hydrophilic cellulose nanocrystals and silicon dioxide nanoparticles (the mass ratio of the two is 1:1) is added to the polydioxanone / hexafluoroisopropanol spinning solution, and mechanically stirred at room temperature until uniformly dispersed. After standing and degassing for 4 hours, the electrospinning voltage is set to 18 kV, the feed rate is 1 mL / h, the receiving distance is 18 cm, the collection roller speed is 200 r / min, and the spinning time is 2 hours. The hydrophilic layer polydioxanone / cellulose nanocrystal / silica fiber membrane is prepared by electrospinning;

[0092] S2. Preparation of polydioxanone intrinsic transition layer fiber membrane:

[0093] Taking the hydrophilic layer polydioxanone / cellulose nanocrystal / silica fiber membrane as the substrate, a polydioxanone / hexafluoroisopropanol spinning solution with a solid content of 15wt.% is deposited on the surface of the hydrophilic layer by electrospinning to obtain a polydioxanone intrinsic transition layer fiber membrane; wherein the spinning voltage is 18kV, the feed rate is 1mL / h, the receiving distance is 18cm, the collection roller speed is 200r / min, and the spinning time is 40min;

[0094] S3. Preparation of hydrophobic layer fiber membrane:

[0095] The hydrophobic biodegradable polylactic acid was dissolved in hexafluoroisopropanol solvent to prepare a 10 wt.% spinning solution, mechanically stirred at room temperature until completely dissolved, and then allowed to stand for degassing for 4 hours;

[0096] Electrospinning of polylactic acid is performed on the surface of the polydioxanone intrinsic transition layer fiber membrane obtained in step S2, and after the solvent evaporates, a polydioxanone-based Janus fiber membrane is obtained; wherein the spinning voltage of the electrospinning is 18 kV, the feed rate is 1 mL / h, the spinning distance is 18 cm, the collection roller speed is 200 r / min, and the spinning time is 20 min.

[0097] Example 7

[0098] A method for preparing a polydioxanone-based Janus fiber membrane comprises the following steps:

[0099] S1. Preparation of hydrophilic layer fiber membrane:

[0100] The viscosity average molecular weight is 8.4×10 4 Polydioxanone is dissolved in hexafluoroisopropanol, and mechanically stirred at room temperature until completely dissolved to prepare a polydioxanone / hexafluoroisopropanol spinning solution with a solid content of 18 wt.%;

[0101] A mixture of 3 wt.% of hydrophilic cellulose nanocrystals and magnesium oxide nanoparticles (the mass ratio of the two is 3:1) is added to the polydioxanone / hexafluoroisopropanol spinning solution, and mechanically stirred at room temperature until uniformly dispersed. After standing and degassing for 4 hours, the electrospinning voltage is set to 20 kV, the feed rate is 0.5 mL / h, the receiving distance is 20 cm, the collection roller speed is 200 r / min, and the spinning time is 4 hours. The hydrophilic layer polydioxanone / cellulose nanocrystal / magnesium oxide fiber membrane is prepared by electrospinning;

[0102] S2. Preparation of polydioxanone intrinsic transition layer fiber membrane:

[0103] Taking the hydrophilic layer polydioxanone / cellulose nanocrystal / magnesium oxide fiber membrane as the substrate, a polydioxanone / hexafluoroisopropanol spinning solution with a solid content of 18wt.% is deposited on the surface of the hydrophilic layer by electrospinning to obtain a polydioxanone intrinsic transition layer fiber membrane; wherein the spinning voltage is 20kV, the feed rate is 0.5mL / h, the receiving distance is 20cm, the collection roller speed is 200r / min, and the spinning time is 40min;

[0104] S3. Preparation of hydrophobic layer fiber membrane:

[0105] The hydrophobic biodegradable poly-ε-caprolactone was dissolved in chloroform solvent to prepare a 15 wt.% spinning solution, mechanically stirred at room temperature until completely dissolved, and then allowed to stand for degassing for 4 hours;

[0106] Electrospinning of poly-ε-caprolactone is performed on the surface of the polydioxanone intrinsic transition layer fiber membrane obtained in step S2, and after the solvent evaporates, a polydioxanone-based Janus fiber membrane is obtained; wherein the spinning voltage of the electrospinning is 20 kV, the feed rate is 0.5 mL / h, the spinning distance is 20 cm, the collection roller speed is 200 r / min, and the spinning time is 30 min.

[0107] Example 8

[0108] A method for preparing a polydioxanone-based Janus fiber membrane comprises the following steps:

[0109] S1. Preparation of hydrophilic layer fiber membrane:

[0110] The viscosity average molecular weight is 8.4×10 4 Polydioxanone is dissolved in hexafluoroisopropanol, and mechanically stirred at room temperature until completely dissolved to prepare a polydioxanone / hexafluoroisopropanol spinning solution with a solid content of 17 wt.%;

[0111] A mixture of 3 wt.% of hydrophilic silica and magnesium oxide nanoparticles (mass ratio of the two is 5:1) is added to the polydioxanone / hexafluoroisopropanol spinning solution, and mechanically stirred at room temperature until uniformly dispersed. After standing and degassing for 4 hours, the electrospinning voltage is set to 20 kV, the feed rate is 0.5 mL / h, the receiving distance is 20 cm, the collection roller speed is 200 r / min, and the spinning time is 4 hours. The hydrophilic layer polydioxanone / silica / magnesium oxide fiber membrane is prepared by electrospinning;

[0112] S2. Preparation of polydioxanone intrinsic transition layer fiber membrane:

[0113] Taking the hydrophilic layer polydioxanone / silicon dioxide / magnesium oxide fiber membrane as the substrate, a polydioxanone / hexafluoroisopropanol spinning solution with a solid content of 17wt.% is deposited on the surface of the hydrophilic layer by electrospinning to obtain a polydioxanone intrinsic transition layer fiber membrane; wherein the spinning voltage is 20kV, the feed rate is 0.5mL / h, the receiving distance is 20cm, the collection roller speed is 200r / min, and the spinning time is 30min;

[0114] S3. Preparation of hydrophobic layer fiber membrane:

[0115] The hydrophobic biodegradable polybutylene succinate was dissolved in hexafluoroisopropanol solvent to prepare a 13 wt.% spinning solution, mechanically stirred at room temperature until completely dissolved, and then allowed to stand for degassing for 4 hours;

[0116] Electrospinning of polybutylene succinate is performed on the surface of the polydioxanone intrinsic transition layer fiber membrane obtained in step S2, and after the solvent evaporates, a polydioxanone-based Janus fiber membrane is obtained; wherein the spinning voltage of the electrospinning is 20 kV, the feed rate is 0.5 mL / h, the spinning distance is 20 cm, the collection roller speed is 200 r / min, and the spinning time is 20 min.

[0117] Comparative Example 1

[0118] A method for preparing a polydioxanone-based Janus fiber membrane comprises the following steps:

[0119] S1. Preparation of hydrophilic layer fiber membrane:

[0120] The weight average molecular weight is 1.45×10 5Polyvinyl alcohol was dissolved in distilled water and mechanically stirred until completely dissolved to prepare a polyvinyl alcohol spinning solution with a solid content of 10 wt. %; 15 wt. % of cellulose nanocrystal nanoparticles were added to the polyvinyl alcohol spinning solution, mechanically stirred at room temperature until uniformly dispersed, and after standing and degassing for 4 hours, the electrospinning voltage was set to 18 kV, the feed rate was 0.3 mL / h, the receiving distance was 18 cm, the collection roller speed was 200 r / min, and the spinning time was 1.5 hours, and a hydrophilic layer polyvinyl alcohol / cellulose nanocrystal fiber membrane was prepared by electrospinning;

[0121] S2. Preparation of polydioxanone transition layer fiber membrane:

[0122] The viscosity average molecular weight is 8.4×10 4 Polydioxanone is dissolved in hexafluoroisopropanol, and mechanically stirred at room temperature until it is completely dissolved to prepare a polydioxanone / hexafluoroisopropanol spinning solution with a solid content of 18wt.%; a hydrophilic layer polyvinyl alcohol fiber membrane is used as a substrate, and the polydioxanone / hexafluoroisopropanol spinning solution with a solid content of 18wt.% is deposited on the surface of the hydrophilic layer by electrospinning to obtain a polydioxanone intrinsic transition layer fiber membrane; wherein the spinning voltage is 18kV, the feed rate is 0.3mL / h, the receiving distance is 18cm, the collection roller speed is 200r / min, and the spinning time is 40min;

[0123] S3. Preparation of hydrophobic layer fiber membrane:

[0124] The hydrophobic biodegradable polylactic acid is dissolved in hexafluoroisopropanol solvent to prepare a 10wt.% spinning solution, and after mechanical stirring at room temperature until it is completely dissolved, it is allowed to stand for degassing for 4 hours; electrospinning of polylactic acid is performed on the surface of the polydioxanone intrinsic transition layer fiber membrane obtained in step S2, and after the solvent evaporates, a polydioxanone-based Janus fiber membrane is obtained; wherein the spinning voltage of the electrospinning is 18kV, the feed rate is 0.1mL / h, the spinning distance is 18cm, the collection roller speed is 200r / min, and the spinning time is 15min.

[0125] The following are relevant performance tests of the polydioxanone-based Janus fiber membranes prepared in Examples 1 to 8 of the present invention and Comparative Example 1.

[0126] like Figure 1 The SEM image of the hydrophilic layer fiber membrane in the polydioxanone-based Janus fiber membrane of Example 1 and its fiber diameter distribution diagram are shown; it can be clearly seen from the figure that the fiber diameter distribution in the hydrophilic layer fiber membrane is uniform. Similarly, in the preparation process of the polydioxanone-based Janus fiber membrane of Examples 2 to 8, the hydrophilic layer fiber membrane prepared in step S1 also has the advantage of uniform diameter distribution.

[0127] According to the SEM images of the hydrophilic layer fiber membrane in the polydioxanone-based Janus fiber membrane prepared in Examples 1 to 8 and their fiber diameter distribution diagrams, the thickness range of the hydrophilic layer fiber membrane of the polydioxanone-based Janus fiber membrane of the present invention is 200μm to 500μm, the fiber diameter range in the membrane is 0.2μm to 1.5μm, and the membrane pore size range is 20μm to 40μm; the thickness range of the intrinsic transition layer fiber membrane is 100μm to 200μm, the fiber diameter range in the membrane is 0.5μm to 2μm, and the membrane pore size range is 10μm to 20μm; the thickness range of the hydrophobic layer fiber membrane is 1μm to 100μm, the fiber diameter range in the membrane is 0.5μm to 5μm, and the membrane pore size range is 1μm to 10μm.

[0128] like Figure 2 Shown is a graph showing the test results of the surface wettability of the hydrophilic layer fiber membrane in the polydioxanone-based Janus fiber membrane prepared in Example 1; wherein the test method is to cut the polydioxanone-based Janus fiber membrane into a square with a size of 20 mm × 20 mm, drop 3 μL of water on the surface of the hydrophilic layer fiber membrane, and record the time for the water contact angle to drop to 0°.

[0129] from Figure 2 It can be seen from the test result graph that the contact angle of water on the membrane surface decreases rapidly with time, and the surface water contact angle decreases to 0° at 160ms, showing excellent hydrophilic properties.

[0130] Table 1 below shows the time it takes for the surface water contact angle of the hydrophilic fiber membrane in the polydioxanone-based Janus fiber membrane prepared in Examples 2 to 8 to decrease to 0° in the surface wettability test.

[0131] Table 1:

[0132] test Example 2 Example 3 Example 4 Example 5 Example 6 Example 7 Example 8 Time / ms 200 180 300 255 360 335 345

[0133] From the test results in Table 1, it can be seen that the time for the water contact angle of the hydrophilic layer fiber membrane on the surface of the polydioxanone-based Janus fiber membrane of the present invention to decrease to 0° is 160ms to 360ms, both of which show excellent hydrophilic properties; in addition, according to tests, the time for the water contact angle of the hydrophilic layer fiber membrane on the surface of the polydioxanone-based Janus fiber membrane prepared in Comparative Example 1 to decrease to 0° is 500ms, which proves that the polydioxanone-based Janus fiber membrane of the present invention exhibits more excellent hydrophilicity.

[0134] like Figure 3 The figure shows a SEM image of the hydrophobic layer fiber membrane formed in step S3 during the preparation of the polydioxanone-based Janus fiber membrane of Example 1; it can be seen from the figure that the fibers in the hydrophobic layer fiber membrane also have the characteristic of uniform diameter distribution.

[0135] like Figure 4 Shown is a graph showing the test results of the surface wettability of the hydrophobic layer fiber membrane in the polydioxanone-based Janus fiber membrane prepared in Example 1; the test method is to cut the polydioxanone-based Janus fiber membrane into a square with a size of 20mm×20mm, drop 3μL of water on the surface of the hydrophobic layer fiber membrane, and use a five-point fitting method to test the water contact angle of the droplet after standing on the hydrophobic fiber membrane surface for different time periods.

[0136] It can be seen from the test result graph that the contact angle of water on the surface of the hydrophobic layer fiber membrane changes with time. The contact angle at 20s is 122.73°, and finally after standing for 60s, its contact angle can reach 101.9°, indicating its excellent hydrophobic properties.

[0137] Table 2 below shows the results of the surface water contact angle of the hydrophobic fiber membrane in the polydioxanone-based Janus fiber membrane prepared in Examples 2 to 8 after standing for 60 seconds in the surface wettability test.

[0138] Table 2:

[0139] test Example 2 Example 3 Example 4 Example 5 Example 6 Example 7 Example 8 Contact angle / ° 120.3 131.2 98.7 95.6 105.6 123.5 118.6

[0140] It can be seen from the test results in Table 2 that the contact angle of water on the hydrophobic fiber membrane surface of the polydioxanone-based Janus fiber membrane of the present invention after standing for 60 seconds is 95.6° to 131.2°, both showing excellent hydrophobic properties.

[0141] like Figure 5 The cross-sectional SEM image of the polydioxanone-based Janus fiber membrane prepared in Example 1 is shown; Figure 5 From the left part a in the middle, it can be seen that a polydioxanone intrinsic transition layer fiber membrane is formed on the hydrophilic layer polydioxanone / cellulose nanocrystal fiber membrane as the substrate; Figure 5 It can be seen from the left side b that a hydrophobic layer fiber membrane is formed on the surface of the polydioxanone intrinsic transition layer fiber membrane; and, from the two parts a and b, it can be seen that the interface between the hydrophilic layer polydioxanone / cellulose nanocrystal fiber membrane and the polydioxanone intrinsic transition layer fiber membrane, as well as the interface between the polydioxanone intrinsic transition layer fiber membrane and the hydrophobic layer fiber membrane are stably bonded without stratification.

[0142] like Figure 6The figure shows the unidirectional moisture conduction performance test diagram of the polydioxanone-based Janus fiber membrane prepared in Example 1. It can be seen from part (a) of the figure that when a water droplet is dropped onto the hydrophobic layer fiber membrane, the penetration state of the water droplet relative to the hydrophobic layer fiber membrane changes at 0s, 3s, 6s, 9s, 12s, 15s, 18s and 21s, respectively, that is, the water droplet infiltrates slowly on one side of the hydrophobic layer fiber membrane, and the hydrophilic layer in the Janus fiber membrane is wetted after 21s; on the contrary, Figure 6 It can be seen from part (b) that when a water droplet falls on the hydrophilic layer fiber membrane, the penetration state of the water droplet relative to the hydrophobic layer fiber membrane changes at 0s, 1s, 2s, 3s, and 4s, respectively. That is, the water droplet penetrates very quickly on one side of the hydrophilic layer fiber membrane and is quickly absorbed within 3s, but the hydrophobic layer fiber membrane is not wetted by water, showing good unidirectional moisture conduction performance.

[0143] The following Table 3 shows the test results of the unidirectional moisture conduction performance of the polydioxanone-based Janus fiber membranes prepared in Examples 2 to 8.

[0144] Table 3:

[0145]

[0146] It can be seen from the test results in Table 3 that the polydioxanone-based Janus fiber membranes prepared in the present invention all have excellent unidirectional moisture conduction properties; in addition, after testing, there is an obvious stratification phenomenon between the hydrophilic layer and the polydioxanone intrinsic transition layer in the polydioxanone-based Janus fiber membrane prepared in Comparative Example 1, which makes it difficult for water droplets to stably and spontaneously penetrate from the hydrophobic layer to the hydrophilic layer.

[0147] Different from Example 1, in Comparative Example 1, the viscosity average molecular weight of 8.4×10 4 Polydioxanone was replaced with a weight average molecular weight of 1.45×10 5 Polyvinyl alcohol; For those skilled in the art, polyvinyl alcohol is a polymer material commonly used in the preparation of hydrophilic membranes, and dispersing hydrophilic cellulose nanocrystals and nanoparticles therein will inevitably contribute to the hydrophilic properties of the membrane; but in fact, the hydrophilic membrane of Comparative Example 1 and the polydioxanone intrinsic transition layer are prone to obvious stratification during the layer-by-layer electrospinning process, and affect the subsequent stable transmission of water droplets between the hydrophilic layer and the hydrophobic layer, and do not have the good hydrophilicity and unidirectional moisture conductivity of the polydioxanone-based Janus fiber membrane of the present invention.

[0148] In summary, the connection interface between the hydrophilic layer and the hydrophobic layer of the polydioxanone-based Janus fiber membrane of the present invention is stably connected through the intrinsic transition layer and can efficiently realize the unidirectional moisture conduction function, and has good application and promotion prospects in the field of medical wound dressing preparation.

[0149] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the benzene invention has been described in detail with reference to the aforementioned embodiments, it is still possible for a person skilled in the art to modify the technical solutions described in the aforementioned embodiments, or to replace some of the technical features therein by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions claimed to be protected by the present invention.

Claims

1. A polydioxanone-based Janus fiber membrane, which is composed of a hydrophilic layer fiber membrane, an intrinsic transition layer fiber membrane and a hydrophobic layer fiber membrane arranged in sequence; wherein: The hydrophilic layer fiber membrane is formed by electrospinning a polydioxanone spinning solution dispersed with hydrophilic inorganic nanoparticles; the intrinsic transition layer fiber membrane is formed by electrospinning a polydioxanone spinning solution on the base membrane with the hydrophilic layer fiber membrane as the base membrane; the hydrophobic layer fiber membrane is formed by electrospinning a hydrophobic biodegradable polymer spinning solution on the surface of the polydioxanone intrinsic transition layer fiber membrane.

2. The polydioxanone-based Janus fiber membrane according to claim 1, characterized in that: The thickness of the hydrophilic layer fiber membrane ranges from 200μm to 500μm, the fiber diameter in the membrane ranges from 0.2μm to 1.5μm, and the membrane pore size ranges from 20μm to 40μm; the thickness of the intrinsic transition layer fiber membrane ranges from 100μm to 200μm, the fiber diameter in the membrane ranges from 0.5μm to 2μm, and the membrane pore size ranges from 10μm to 20μm; the thickness of the hydrophobic layer fiber membrane ranges from 1μm to 100μm, the fiber diameter in the membrane ranges from 0.5μm to 5μm, and the membrane pore size ranges from 1μm to 10μm.

3. A method for preparing a polydioxanone-based Janus fiber membrane, characterized in that: The steps are: S1. Preparation of hydrophilic layer fiber membrane: The viscosity average molecular weight is 1.1×10 4 ~9.9×10 4 Polydioxanone is dissolved in an organic solvent I to prepare a polydioxanone spinning solution with a solid content of 5wt.% to 20wt.%; 0.1wt.% to 20wt.% of hydrophilic inorganic nanoparticles are uniformly dispersed in the polydioxanone spinning solution, and the hydrophilic layer polydioxanone / hydrophilic inorganic nanoparticle fiber membrane is formed by electrospinning; S2. Preparation of polydioxanone intrinsic transition layer fiber membrane: Taking the hydrophilic layer polydioxanone / hydrophilic inorganic nanoparticle fiber membrane prepared in step S1 as the substrate, depositing the polydioxanone spinning solution onto the surface of the hydrophilic layer by electrospinning to obtain a polydioxanone intrinsic transition layer fiber membrane; S3. Preparation of hydrophobic layer fiber membrane: The hydrophobic biodegradable polymer is dissolved in an organic solvent II to prepare a 5wt.% to 25wt.% hydrophobic biodegradable polymer spinning solution, and the spinning solution is electrospinned on the surface of the polydioxanone intrinsic transition layer fiber membrane prepared in step S2 to form a hydrophobic layer fiber membrane, thereby obtaining a polydioxanone-based Janus fiber membrane.

4. The method for preparing a polydioxanone-based Janus fiber membrane according to claim 2, characterized in that: In step S1, the hydrophilic inorganic nanoparticles are any one of cellulose nanocrystals, hydrophilic silicon dioxide, hydrophilic magnesium oxide, molybdenum oxide, titanium dioxide, and silver nanoparticles, or a mixture of two or more thereof.

5. The method for preparing a polydioxanone-based Janus fiber membrane according to claim 2, characterized in that: In step S1, the electrospinning conditions are set as follows: spinning voltage is 15 kV to 20 kV, feed rate is 0.1 mL / h to 1.5 mL / h, spinning distance is 10 cm to 20 cm, collection roller speed is 100 r / min to 500 r / min, and spinning time is 1 h to 6 h.

6. The method for preparing a polydioxanone-based Janus fiber membrane according to claim 2, characterized in that: In step S2, the electrospinning conditions are set as follows: spinning voltage of 15 kV to 20 kV, feed rate of 0.1 mL / h to 1.5 mL / h, spinning distance of 10 cm to 20 cm, collection roller speed of 100 r / min to 500 r / min, and spinning time of 30 min to 60 min.

7. The method for preparing a polydioxanone-based Janus fiber membrane according to claim 2, characterized in that: In step S3, the hydrophobic biodegradable polymer includes any one or a combination of two or more of polylactic acid, poly-ε-caprolactone, poly-3-hydroxyalkanoate or polybutylene succinate.

8. The method for preparing a polydioxanone-based Janus fiber membrane according to claim 2, characterized in that: In step S3, the electrospinning conditions are set as follows: spinning voltage of 15 kV to 20 kV, feed rate of 0.1 mL / h to 1.5 mL / h, spinning distance of 10 cm to 20 cm, collection roller speed of 100 r / min to 500 r / min, and spinning time of 15 min to 30 min.

9. The method for preparing a polydioxanone-based Janus fiber membrane according to claim 2, characterized in that: In step S1, the organic solvent I is any one of hexafluoroisopropanol, chloroform, dimethyl sulfoxide or tetrachlorophenol, or a combination of two or more thereof; in step S3, the organic solvent II is one of hexafluoroisopropanol, dichloromethane, chloroform, dimethyl sulfoxide, dimethylformamide, acetone or tetrahydrofuran, or a mixture of two or more thereof in any proportion.

10. An application of the polydioxanone-based Janus fiber membrane as claimed in claim 1 or 2, characterized in that: Polydioxanone-based Janus fiber membrane is used in the preparation of medical wound dressings.

Citation Information

Patent Citations

  • Composite dressing with continuous one-way moisture conduction capability and preparation method

    CN116115813A

  • Preparation method of one-way moisture-conducting nanofiber membrane with porous Janus structure

    CN118326616A

  • Multi-layer hernia repairing patch and preparation method thereof

    CN102217981A

  • Composite membrane, and preparation method and application of composite membrane

    CN106730018A

  • Wet gradient honeycomb structure fiber membrane for medical and health protection and preparation method thereof

    CN111575814A

Cited By

  • One-way moisture conducting film with gradient aperture and preparation method of one-way moisture conducting film

    CN121719021A

  • A one-way moisture management film with gradient pore size and a method of making the same

    CN121719021B