Completely biodegradable functional paper-based mulching film as well as preparation and application thereof
By combining bagasse with glycolic acid pretreatment and polyphenol hydroxylignin nanoparticles, a functionalized paper-based film with high strength, ultraviolet resistance and completely degradable is prepared, solving the insufficient performance of bagasse resource utilization and biomass mulch films. The problem of this has achieved the improvement of soil and efficient utilization of resources.
Patent Information
- Application Number
- CN202411093116.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-07-01
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing technology cannot effectively utilize sugarcane bagasse, resulting in waste of resources and environmental pollution. At the same time, biomass mulch film has shortcomings in resistance to ultraviolet and complete degradation, making it difficult to improve the soil environment.
By mixing sugarcane bagasse with glycolic acid for pretreatment, efficient cellulose and lignin were extracted, and polyphenol hydroxylignin nanoparticles combined with urea was used to prepare a functionalized paper-based film with high strength, UV resistance and completely degradable content. , add palm wax to improve mechanical strength.
It realizes efficient extraction of cellulose and lignin, improves the mechanical strength and UV resistance of the membrane, promotes the degradation of biomulching membrane, improves the soil environment, and improves plant growth efficiency. All materials are fully biodegradable of.
Smart Images

Figure CN118996904A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of agricultural waste utilization technology, specifically a fully biodegradable functionalized paper-based membrane and its preparation and application. Background Art
[0002] my country is a major agricultural country. As the country with the largest user of agricultural film in Asia, China's consumption in 2018 was 2.5 million tons, accounting for more than 70% of Asia and nearly 50% of the world.
[0003] Sugarcane is an important sugar and energy crop in the world. Guangxi Zhuang Autonomous Region is the largest sugarcane producing area in China. In 2023, the sugarcane output and sucrose output accounted for nearly 70% of the country. The Guangxi Zhuang Autonomous Region crushes 50 million tons of sugarcane annually, but the high-value utilization of sugarcane bagasse is low. Most of the sugarcane bagasse is used for thermal power generation or discarded as agricultural waste, which not only causes low utilization rate but also becomes an environmental burden. Sugarcane bagasse is rich in cellulose, hemicellulose and lignin resources. Cellulose, as the world's largest renewable resource, is widely used in the biomass industry. However, the separation of biomass components has always been the biggest problem that plagues biomass utilization. The green, efficient and low-cost separation of biomass components is the core driving force for high-quality utilization of biomass.
[0004] CN117534944A uses polymer starch as raw material to prepare a composite biofilm product with a degradation rate of 80%. However, a large amount of non-degradable additives are added, and the requirement of complete degradation is not met. CN117186474A uses sea squirt cellulose as a base film, but fails to effectively improve the soil environment and has good UV resistance. The above technical problems need to be solved through research to promote the development of high-strength, fully degradable, UV-resistant and soil-improving biofilms.
[0005] Therefore, finding a functional bagasse-based membrane that is high in strength, UV-resistant, and completely degradable and can improve the soil is the current key research direction. Summary of the invention
[0006] In order to solve the above technical problems existing in the prior art, the present application provides a fully biodegradable functionalized paper-based membrane and its preparation and application.
[0007] A method for preparing a fully biodegradable functionalized paper-based film comprises the following steps:
[0008] (1) preparing a reaction solvent: taking water and an organic acid chemical and mixing them evenly in a mass ratio of 1:0.5-1, and stirring under magnetic stirring for 10-60 minutes to obtain an additive; taking dehydrated bagasse after a 40-60 mesh sieve, adding the obtained additive and mixing evenly, and performing a cooking reaction in a reactor at 60-170° C., wherein the mass ratio of the bagasse to the additive solution is between 1:0.1-1, and the reaction time is between 1-6 hours, and after the reaction, a solid product and a liquid product are obtained;
[0009] (2) taking the liquid product after the reaction in step (1), extracting polyphenol hydroxyl lignin nanoparticles after centrifugal precipitation, and then fully reacting the polyphenol hydroxyl lignin nanoparticles with urea at a ratio of 1:1-5 under magnetic stirring to obtain a lignin slow-release filler;
[0010] (3) The solid product obtained in step (1) is washed with ultrapure water for 3-10 times to a pH value between 5 and 10, and after drying, the remaining solid is taken, a slow-release lignin filler is added according to a proportion, and the mixture is dispersed and stirred at 600-2400 r / min to obtain a membrane liquid, and then the membrane liquid is naturally flowed down and fixed in the membrane mold to obtain a ground film formed object;
[0011] (4) Take the mulch film formed in step (3), attach wax to it by surface sizing, heat and dry it, and finally cut it to obtain a degradable mulch film formed product.
[0012] Furthermore, in step (1), the organic acid is a mixture of any one or more of formic acid, acetic acid, glycolic acid, p-toluenesulfonic acid, and maleic acid, and the acid concentration is above 95% of analytical grade.
[0013] Furthermore, in step (1), the cellulose content of bagasse is 40-50%, the hemicellulose content is 20-30%, the lignin content is 20-30%, and the residual ash content is less than 5%.
[0014] Furthermore, in step (2), the liquid product remaining after the reaction in step (1) is taken, and the complete polyphenolic hydroxyl lignin is extracted using a dioxane solution, and the dioxane is removed by fractional distillation to purify the lignin to obtain pure polyphenolic hydroxyl lignin.
[0015] Furthermore, in the step (2), the dioxane solution is used to extract the complete polyphenolic hydroxyl lignin. The dioxane used is of analytical purity of more than 98%, the solution concentration is 30%-99%, the stirring rate for extracting lignin is 10-400r / min, and the reaction time is 2-48h.
[0016] Furthermore, in step (3), the ratio of the solid product obtained in step (1) to the lignin slow-release filler is between 1:0.01-0.5, and the lignin addition rate is controlled at 0.1-10 g / h.
[0017] Furthermore, the wax in step (4) is palm wax, and the sizing amount is 4-8 g / m 2 .
[0018] Furthermore, in the surface sizing process in step (4), the ground film is placed in a dryer and dried at 20-80° C. for 2-8 hours before the surface sizing is applied.
[0019] The completely biodegradable functional paper-based film prepared by the above method can be applied to agricultural planting.
[0020] Compared with the prior art, the technical effects created by this application are embodied in:
[0021] (1) First, the problem of low separation efficiency of biomass components is addressed. For example, the conventional method CN110004756A uses an acetone-concentrated sulfuric acid system to treat cellulose, which easily causes cellulose damage and low extraction rate, and the addition of chemical additives easily causes the dual problems of high cost and environmental pollution. The present application achieves efficient extraction of cellulose and lignin by pretreating bagasse components with high-concentration glycolic acid, and the extraction rate can reach 90%. Glycolic acid is a green organic acid, and its properties are similar to those of formic acid. It has the dual properties of alcohol and carboxylic acid, such as low corrosion, low toxicity, high biodegradability and good water solubility. Due to its α-hydroxy structure, it has a strong ability to ionize hydrogen ions. 74.9±2.8% of the separated xylose exists in the form of oligomers in the hydrolyzate. The use of glycolic acid pretreatment can effectively separate hemicellulose, and the efficient extraction efficiency of cellulose reaches more than 90%. It can inhibit the depolymerization and polymerization of lignin, and the lignin component can increase the mechanical strength and UV resistance of the membrane.
[0022] (2) In view of the poor effect of biomass mulch on improving soil, this application provides a solution to the problem of biomass mulch degradation to improve soil environment. This application inhibits the self-condensation reaction of β-O-4 breakage of lignin during the reaction by reacting lignin with glycolic acid pretreatment. The broken reactive sites react with glycolic acid for esterification, and the extracted lignin has more reactive sites, which better promotes the slow release of its own nitrogen elements and urea additives, thereby achieving the improvement of soil environment by biomass mulch degradation and improving plant growth efficiency.
[0023] (3) In response to the problem that biological ground mulch is difficult to completely degrade, this application proposes an idea that cellulose is used as the basic material of the mulch and lignin is used as the filler of the mulch to play a supporting role. Cellulose and lignin are natural polymer materials that exist in nature. After degradation, they play an effect of improving the soil and increasing soil fertility. This application adds palm wax as a sizing agent, which can effectively improve the mechanical strength of the mulch. Palm wax is non-toxic and harmless. It can be decomposed into substances that are harmless to nature. The natural shell structure of lignin particles is used to wrap urea to achieve the slow-release function of nitrogen fertilizer. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 It is the technical roadmap of this application.
[0025] Figure 2 This is a real picture of the ground film prepared by using the present invention.
[0026] Figure 3 The invention relates to a contact angle test of the ground film prepared by the invention.
[0027] Figure 4 The invention is a mechanical strength test of the ground film prepared by the invention.
[0028] Figure 5 The invention is to test the anti-ultraviolet performance of the ground film prepared by the invention. DETAILED DESCRIPTION
[0029] The technical solution of the present application is further limited below in conjunction with specific implementation methods, but the scope of protection required is not limited to the description.
[0030] The experimental methods in the following examples are all conventional methods unless otherwise specified; the biological and chemical reagents used are all conventional reagents in the art unless otherwise specified.
[0031] The bagasse used was provided by a local sugar factory (Guangxi Zhuang Autonomous Region, China). The chemical composition of the bagasse was analyzed. The cellulose content was 40-50%, the hemicellulose content was 20-30%, and the lignin content was 20-30%.
[0032] Embodiment 1:
[0033] (1): Ultrapure water and acetic acid are mixed uniformly in a mass ratio of 1:0.8 to obtain an auxiliary agent, 10 g of dehydrated bagasse after a 40-60 mesh sieve is taken, the solid-liquid ratio is 1:10, and the mixture is boiled in a reactor at 140°C for 3 hours. After the reaction, a solid product and a liquid product are obtained.
[0034] (2): Take the liquid product after step (1), use 98% dioxane solution to extract lignin, the stirring rate of lignin extraction is 300r / min, and the reaction time is 48h. After the end, dioxane is removed by fractional distillation to obtain purified polyphenol hydroxyl lignin, and the purified polyphenol hydroxyl lignin is freeze-dried. Take 2g of freeze-dried lignin, add 2g of urea, and stir at 30°C for 3h. After centrifugation, 3.14g of nano lignin slow-release particles are obtained.
[0035] (3): Take 5g of the solid product after step (1), wash it with ultrapure water for 5 times, wash it until it is neutral and dry it, and keep the remaining solid after drying for later use. Add 2g of the nano-lignin slow-release particles prepared in step (3) and add it dropwise at a rate of 0.05g / min. Disperse and stir evenly at 2400r / min to obtain a membrane liquid, and then the membrane liquid naturally flows down and is fixed in the membrane mold, and dried at 45 degrees Celsius for 6h.
[0036] (4) Take the mulch obtained in step (3) and evenly apply palm wax, with a quantitative amount of 3.55g / m 2 , dried at 60 degrees Celsius for 3 hours to obtain film 1.
[0037] Embodiment 2:
[0038] (1): Ultrapure water and glycolic acid are mixed uniformly in a mass ratio of 1:0.7 to obtain an additive. 10 g of dehydrated bagasse through a 40-60 mesh sieve is taken, and the solid-liquid ratio is 1:10. The mixture is steamed in a reactor at 150° C. for 3 hours.
[0039] (2): Take the liquid product after step (1), use 98% concentration of dioxane solution to extract lignin, the stirring rate of lignin extraction is 300r / min, and the reaction time is 48h. After the end, dioxane is removed by fractional distillation to obtain purified polyphenol hydroxyl lignin. The purified polyphenol hydroxyl lignin is freeze-dried, 2g of freeze-dried lignin is taken, 2g of urea is added, and stirred at 30°C for 3h. After centrifugation, 3.55g of nano-lignin slow-release particles are obtained.
[0040] (3): Take 6g of the solid product after step (1), wash it with ultrapure water for 3 times, wash it until it is neutral and dry it, and keep the remaining solid after drying for later use. Add 2g of the nano-lignin slow-release particles prepared in step (3) and add it dropwise at a rate of 0.05g / min. Disperse and stir evenly at 2400r / min to obtain a membrane liquid, and then the membrane liquid naturally flows down and is fixed in the membrane mold, and dried at 45 degrees Celsius for 6h.
[0041] (4) Take the mulch obtained in step (3) and evenly apply palm wax, with a quantitative amount of 3.87 g / m 2 , dried at 60 degrees Celsius for 3 hours to obtain film 2.
[0042] Embodiment 3:
[0043] (1): Ultrapure water and p-toluenesulfonic acid are mixed uniformly in a mass ratio of 1:0.5 to obtain an auxiliary agent. 10 g of dehydrated bagasse after a 40-60 mesh sieve is taken, and the solid-liquid ratio is 1:10. The mixture is steamed in a reactor at 80°C for 3 hours.
[0044] (2): Take the liquid product after step (1), use 98% concentration of dioxane solution to extract lignin, the stirring rate of lignin extraction is 300r / min, and the reaction time is 48h. After the end, remove dioxane by fractional distillation to obtain purified polyphenol hydroxyl lignin. Freeze-dry the purified polyphenol hydroxyl lignin, take 2g of freeze-dried lignin, add 2g of urea, and stir at 30°C for 3h. After centrifugation, 3.25g of nano lignin slow-release particles are obtained.
[0045] (3): Take 5g of the solid product after step (1), wash it with ultrapure water 10 times, wash it until it is neutral and dry it, and keep the remaining solid after drying for later use. Add 2g of the nano-lignin slow-release particles prepared in step (3) and add it dropwise at a rate of 0.05g / min. Disperse and stir evenly at 2400r / min to obtain a membrane liquid, and then the membrane liquid naturally flows down and is fixed in the membrane mold, and dried at 45 degrees Celsius for 6h.
[0046] (4) Take the mulch obtained in step (3) and evenly apply palm wax, with a quantitative amount of 3.55g / m 2 , dried at 60 degrees Celsius for 3 hours to obtain film 3.
[0047] Comparative Example 1:
[0048] A degradable mulch film is different from Example 2 in that the addition of nano-lignin slow-release particles in steps (2) and (3) is omitted, and other raw materials, preparation process steps and parameters are the same as those in Example 2.
[0049] Comparative Example 2:
[0050] A degradable mulch film, which is different from Example 2 in that step (4) of adding palm wax is omitted, and other raw materials, preparation process steps and parameters are the same as those in Example 2.
[0051] 1. Water resistance test
[0052] The water resistance of the ground film can be reflected by testing the contact angle of the ground film on the absorption of water droplets. The waterproof performance of the ground film can be reflected by observing the absorption capacity of the surface of the object on the liquid. The larger the contact angle, the worse the ability of the ground film surface to absorb water, and the better the waterproof performance. According to the experiment Figure 3 It shows that adding lignin and palm wax can effectively improve the poor waterproof performance of cellulose itself.
[0053] Table 1 Sample contact angle experimental data
[0054] Sample name Comparative Example 1 Comparative Example 2 Example 2 Contact angle 50.5° 105.5° 117.5°
[0055] 2. Mechanical strength performance test
[0056] According to the requirements of the Technical Specifications for Evaluation of Biodegradable Ground Films, the tensile strength test of ground films can be carried out by a uniaxial tensile testing machine. According to Table 2, the strength of the biodegradable ground film prepared by the present invention reaches 73Mpa, which is much higher than the standard required by the document (40Mpa).
[0057] Table 2 Experimental data of sample breaking strength and breaking elongation
[0058] Sample name Comparative Example 1 Comparative Example 2 Example 2 Breaking strength(N) 93 100 113 Elongation at break (%) 39 57 76
[0059] 3. Anti-ultraviolet performance test
[0060] The shading degree of the ground film samples of Example 2 and Comparative Example 1 was tested, and the test results of the sample laser particle size analyzer ( Figure 5 ) for analysis. Figure 5 As shown in the figure, by adding lignin to the ground film sample, the anti-ultraviolet ability of the ground film can be effectively improved, because lignin is a natural anti-ultraviolet material. Under the condition of 0-500 wavelength, it can completely and effectively block ultraviolet rays.
[0061] Finally, it should be pointed out that the above embodiments are only representative examples of the present application. Obviously, the technical solution of the present application is not limited to the above embodiments, and there may be many variations. All variations that can be directly derived or associated with the contents disclosed in the present application by a person of ordinary skill in the art should be considered as the protection scope of the present application.
Claims
1. A method for preparing a fully biodegradable functionalized paper-based film. It is characterized in that The specific steps include: (1) preparing a reaction solvent: taking water and an organic acid chemical and mixing them evenly in a mass ratio of 1:0.5-1, and stirring under magnetic stirring for 10-60 minutes to obtain an additive; taking dehydrated bagasse after a 40-60 mesh sieve, adding the obtained additive and mixing evenly, and performing a cooking reaction in a reactor at 60-170° C., wherein the mass ratio of the bagasse to the additive solution is between 1:0.1-1, and the reaction time is between 1-6 hours, and after the reaction, a solid product and a liquid product are obtained; (2) taking the liquid product after the reaction in step (1), extracting polyphenol hydroxyl lignin nanoparticles after centrifugal precipitation, and then fully reacting the polyphenol hydroxyl lignin nanoparticles with urea at a ratio of 1:1-5 under magnetic stirring to obtain a lignin slow-release filler; (3) The solid product obtained in step (1) is washed with ultrapure water for 3-10 times to a pH value between 5 and 10, and after drying, the remaining solid is taken, a slow-release lignin filler is added according to a proportion, and the mixture is dispersed and stirred at 600-2400 r / min to obtain a membrane liquid, and then the membrane liquid is naturally flowed down and fixed in the membrane mold to obtain a ground film formed object; (4) Take the mulch film formed in step (3), attach wax using a surface sizing process, heat and dry, and finally cut to obtain a degradable mulch film formed product.
2. The method for preparing the fully biodegradable functionalized paper-based film according to claim 1, It is characterized in that In the step (1), the organic acid is a mixture of any one or more of formic acid, acetic acid, glycolic acid, p-toluenesulfonic acid, and maleic acid, and the acid concentration is above 95% of analytical grade.
3. The method for preparing the fully biodegradable functionalized paper-based film according to claim 1, It is characterized in that In the step (1), the cellulose content of the bagasse is 40-50%, the hemicellulose content is 20-30%, the lignin content is 20-30%, and the residual ash content is less than 5%.
4. The method for preparing the fully biodegradable functionalized paper-based film according to claim 1, It is characterized in that In the step (2), the liquid product remaining after the reaction in step (1) is taken, and the complete polyphenolic hydroxyl lignin is extracted using a dioxane solution, and the dioxane is removed by fractional distillation to purify the lignin to obtain pure polyphenolic hydroxyl lignin.
5. The method for preparing the fully biodegradable functionalized paper-based film according to claim 4, It is characterized in that In the step (2), the dioxane solution is used to extract the complete polyphenolic hydroxyl lignin. The dioxane used is of analytical purity of more than 98%, the solution concentration is 30%-99%, the stirring speed of the extracted lignin is 10-400 r / min, and the reaction time is 2-48h.
6. The method for preparing the fully biodegradable functionalized paper-based film according to claim 1, It is characterized in that In the step (3), the ratio of the solid product obtained in the step (1) to the lignin slow-release filler is between 1:0.01-0.5, and the lignin addition rate is controlled at 0.1-10 g / h.
7. The method for preparing the fully biodegradable functionalized paper-based film according to claim 1, It is characterized in that The wax in step (4) is palm wax, and the sizing amount is 4-8 g / m 2 .
8. The method for preparing the fully biodegradable functionalized paper-based film according to claim 1, It is characterized in that In the surface sizing process in step (4), the ground film is placed in a dryer and dried at 20-80° C. for 2-8 hours before surface sizing.
9. A fully biodegradable functional paper-based film. It is characterized in that It is prepared by the method according to any one of claims 1 to 7.
10. Use of the fully biodegradable functional paper-based film according to claim 9 in agricultural planting.
Citation Information
Cited By
Straw fiber-based antibacterial mulching film with temperature and humidity response performance and preparation method
CN120535800A
Straw fiber-based antibacterial mulching film with temperature and humidity response performance and preparation method thereof
CN120535800B