Box column and manufacturing method
Through innovation in layered welding bevels and welding sequence, combined with CO2 gas protective welding and submerged arc welding technology, the problem of box column welding deformation is solved, and the welding quality and structural stability are improved.
Patent Information
- Application Number
- CN202310550696.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-16
- Publication Date
- 2024-11-22
AI Technical Summary
During the welding process, box columns are prone to deformation due to welding temperature, which reduces welding quality and affects structural stability.
The method of layered welding bevel is adopted. First weld the inner layer of the weld, then the outer layer is welded, combined with CO2 gas protective welding and submerged arc welding technology, reduce deformation through the welding sequence and correction process, and flame correction is performed after welding. Ensure structural stability.
Effectively reduce or avoid box welding deformation, improve welding quality and structural stability, and avoid expansion problems caused by uneven heat input during welding.
Smart Images

Figure CN118997394A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of box-type columns for buildings, and in particular to a box-type column and a manufacturing method thereof. Background Art
[0002] In recent years, with the development of economic construction, steel structure buildings have been widely used, among which box columns account for a large proportion in steel structures. In the application process of box columns, the current box-shaped specifications and sizes in rolled steel cannot meet the needs of construction. Therefore, welded box columns are widely used in various steel structure buildings. The production process of box components is relatively complicated and requires high quality. Therefore, the design and production method of box columns has been a research direction that people have been pursuing.
[0003] In the prior art, a Chinese patent application document with authorization announcement number CN105458536A discloses a welding process for a steel structure box column; during the welding process, two main welds are welded simultaneously, and the welds are insulated after welding.
[0004] However, since the welding temperature is relatively high during the welding of the box body, according to the principle of thermal expansion and contraction, the box-type column is deformed after welding, which reduces the welding quality and affects the structure of the box-type column. Summary of the invention
[0005] The present invention provides a box-type column and a manufacturing method thereof, with the aim of providing a box-type column structure and a manufacturing process thereof, and providing a box-type column welding method during the manufacturing process to solve the problem of welding deformation of the box-type column during the manufacturing process.
[0006] In order to achieve the above object, the present invention adopts the following scheme: A box-type column provided by the present invention comprises a box-column main body, wherein the box-column main body comprises an inner partition plate located inside the box-column main body, a bottom plate, a top plate corresponding to the bottom plate, and a web connecting the bottom plate and the top plate; the box-column main body further comprises a rib plate fixed to the bottom plate, the top plate, and the surface of the web; and an external connecting part fixed to the box-column main body, wherein the external connecting part comprises a box-column corbel.
[0007] Optionally, the box-type column may be composed of a plurality of box-column bodies connected in sequence by welding.
[0008] Optionally, the box column body further includes a box column foot plate, and the box column foot plate is located at the end of the box column body.
[0009] Optionally, the box column body further includes a protruding portion, which includes a protruding bottom plate, a protruding top plate, a protruding stiffening plate, a protruding web plate and a sealing plate; the protruding bottom plate is integrally formed with the bottom plate, and the protruding top plate is integrally formed with the top plate.
[0010] Optionally, the external connection part also includes a variable cross-section box, which includes a box bottom plate, a box top plate and a box belly plate, and the box bottom plate and the box top plate are formed by splicing a plurality of flat plates or bent plates at a preset angle.
[0011] The present invention provides a method for manufacturing a box-type column, comprising the following steps: S10, material preparation: pre-process the parts that make up the box column; S11. Positioning and assembling the inner baffles: vertically arranging the inner baffles on the bottom plate at a preset spacing, and assembling and welding the ribs longitudinally arranged on the bottom plate; S12. Assemble the web: press the bottom plate, web and inner partition together, check the verticality of the web and bottom plate edges, ensure that the ends of the web and bottom plates are aligned, and perform positioning welding after passing the test; S13, welding inner diaphragm: welding the full penetration weld between the inner diaphragm and the web and bottom plate, and conducting ultrasonic testing after welding; S14. Welding of ribs on the web: Weld double-sided fillet welds between the ribs and the web and inner partitions. When welding, first weld in parallel with the web. For positions that require overhead welding, wait until the box is turned over before welding inside the box. S15. Top plate assembly: When ribs are provided on the top plate, the ribs are welded to the top plate in advance, and then the top plate is covered on the webs on both sides. When covering the plate, a 2-3mm welding shrinkage allowance is added in the direction of the cross-sectional height, and the top plate is pressed against the web and inner partition, and the cross-sectional dimensions and the alignment of the web, bottom plate and top plate corners are confirmed. Positioning welding is performed after the distortion is qualified.
[0012] S16. Perform base welding and reinforcement on the main welds of the box column body: After turning over the box column body, the welder enters the interior of the box column body to weld the full penetration welds between the inner partition and the top plate, and welds the welds between the rib plate and the top plate, bottom plate, web plate and inner partition.
[0013] S17, welding the main weld of the box column, the welding sequence is as follows: a. Use CO2 gas shielded welding to weld the weld between the web and the bottom plate to 1 / 3 of the groove depth, and turn it upside down; b. Use CO2 gas shielded welding and submerged arc welding to weld the welds between the web and the top plate to 1 / 2 of the groove depth, and turn it upside down; c. Use submerged arc welding to weld the remaining 2 / 3 of the groove depth of the weld between the web and the bottom plate, and turn it upside down; d. Use submerged arc welding to weld the remaining 1 / 2 of the groove depth of the weld between the web and the top plate.
[0014] S18, Correction: Flame correction is performed on the bending and twisting deformation of the box.
[0015] S19, end milling: Place the box column body on the end milling machine platform, the box column body is perpendicular to the end milling equipment, and press the box column body on the working platform. Milling plane requirements: flatness is less than 0.3mm, and the verticality of the milling plane and the first body is less than or equal to 1.5h / 1000.
[0016] S20. Assembly of box column corbels and box column base plates.
[0017] Optionally, in step S17, welding the box column body further includes the following process: 1) The welding method adopts CO2 gas shielded welding and submerged arc welding; 2) During the welding process, the welding wire for CO2 gas shielded welding is Q355 steel, model ER50-6, type solid wire, diameter 1.2mm; the welding wire for submerged arc welding is Q355 steel, model H 10 Mn2, type is solid wire, diameter is 4.0mm, flux is CHF101; 3) Welding process parameters: a. Gas shielded welding parameters: welding current 200-290 (A), voltage 26-32 (V), welding speed 30-45cm / min; b. Submerged arc welding parameters: welding current 600-750 (A), voltage 34-40 (V), welding speed 27-40cm / min; 4) Preparation before welding: Before welding, the oxides and cutting slag within 100mm on both sides of the groove need to be cleaned; 5) Preheating of welding.
[0018] Optionally, in step S20, the process of assembling the box column corbel and the box column foot plate includes: 1) Make the box column corbel: The box column corbel includes the wing plates on both sides and the web plate between the wing plates. Double-sided fillet welds are used between the web plate and the wing plates of the H-shaped steel corbel. After welding, the angular deformation of the wing plates is flame corrected, and the stiffening plates on the web plates are assembled and welded. The wing plates and the main body are fully melted to the first level, and the web plates and the box body are partially melted; 2) Shot blasting and rust removal on the box column corbels.
[0019] 3) Main body fixed length: according to the drawing size, the added margin of the main body is marked and cut by a semi-automatic cutting machine, the groove of the welding part of the box column foot plate is processed, and the groove is polished after completion; 4) Place the main body on the assembly platform, establish a horizontal reference, and draw lines on the main body according to the size and position of each component external to the main body on the drawing. The lines include the center line and the reference line, and the part position is marked with double lines; The components of the multi-layer corbels are made by the method of drawing wires and erecting poles, and the corbels and connecting plates are based on the milling plane of the column top; 5) Assemble the box column foot plate: The weld between the box column foot plate and the main body is required to be fully penetrated to the first level; the stiffening plate, the first rib plate and the box column foot plate are tightly pressed against the box column foot plate without welding; 6) Painting: After sandblasting and rust removal, the box-type columns that have been manufactured and inspected are sprayed according to the spraying positions in the drawings.
[0020] Optionally, the material preparation process in step S10 includes: 1) Cutting: Set a 30mm machining allowance along the length direction of the bottom plate, web plate and top plate; 2) Bevel processing: semi-automatic flame cutting machine is used for processing; 3) Processing of special-shaped parts: Special-shaped parts are processed by flame CNC cutting or plasma cutting; 4) Splicing requirements: The butt length between the bottom plate, top plate and web plate is greater than or equal to 600mm, the butt welds between the bottom plate, top plate and web plate are staggered by at least 200mm, and the butt welds and the inner partition and stiffening plate are staggered by at least 200mm; 5) Rib processing: T-shaped ribs can be cut along the axis of I-beams; 6) Inner partition processing: Assemble the welding backing plate according to the requirements of the inner partition weld, control the width and diagonal size of the inner partition, the length of the positioning weld on the inner partition is 40-60mm, and the spacing of the positioning weld is 200-300mm.
[0021] Optionally, a longer box column is divided into multiple parts, and the box columns are manufactured separately and then assembled. When multiple box columns are combined and assembled, the direct butt welds of the main bodies of adjacent box columns are staggered by at least 200 mm, and submerged arc welding is used in the butt welding process.
[0022] Optionally, when the box column body is provided with a protrusion: S21, the protruding bottom plate and the bottom plate, the protruding top plate and the top plate are integrally formed; S22. Conduct concealed inspection and ultrasonic inspection on the main weld of the protruding part, assemble the protruding stiffening plate between the protruding top plate and the protruding bottom plate, and adopt single-sided backing welding; S23. Assemble the protruding web, use single-sided groove full penetration welding between the protruding web and the top plate and bottom plate, and use single-sided groove backing welding between the protruding web and the protruding stiffening plate, and perform ultrasonic testing after welding; S24. Sealing plate welding: The sealing plate weld adopts single-sided groove backing welding.
[0023] Optionally, the variable-section box is manufactured separately from the box column body, and the manufacturing of the variable-section box includes the following processes: S25, installing the inner partition plate on the bottom plate of the box; S26, install the box body belly plate and the box body top plate, and weld them after installation; S27, performing end milling on the welded variable cross-section box to complete the production of the variable cross-section box; When the box column body is provided with a variable cross-section box; S28. The variable-section box body is butt-jointed with the main box body, and full-penetration welding is performed with a single-sided liner at the joint to control the misalignment. After the butt-jointing is completed, the weld is ultrasonically inspected and shot blasted to remove rust, thereby obtaining the box column in claim 5.
[0024] Compared with the prior art, the present invention has the following advantages: 1. By designing the manufacturing sequence of the box-type column and the external connection part connected to the box-type column, the processing and manufacturing of one or several box-type columns with the same or similar structures can be realized; 2. When welding the main body weld, the weld groove is divided into multiple layers. The inner layer of the weld groove is welded first, and then the outer layer of the weld groove is welded. This makes the welding heat input of the welds on the upper and lower sides almost equal, thereby reducing or avoiding the deformation problem during the box welding process; 3. During the production process of box-type columns, the main welds of the box column body are welded by gas shielded welding for priming and submerged arc welding for covering, in accordance with the welding sequence, to avoid welding deformation of the box column body and the problem of easy penetration of the liner plate when using submerged arc welding alone. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] The present application is further described in detail below in conjunction with the accompanying drawings and specific implementation methods.
[0026] Figure 1 This is the first viewing angle of a stereoscopic image of a box-type column provided in Example 1 of the present invention.
[0027] Figure 2 This is a second viewing angle of a stereoscopic image of a box-type column provided in the first embodiment of the present invention.
[0028] Figure 3 This is a diagram showing the installation status of the first top plate of a box-type column provided in Example 1 of the present invention.
[0029] Figure 4 This is a diagram showing the installation status of the first rib of a box-type column provided in Example 1 of the present invention.
[0030] Figure 5 This is a diagram showing the installation state of the first web of a box-type column provided in Example 1 of the present invention.
[0031] Figure 6 This is a diagram showing the installation status of the first inner partition of a box-type column provided in Example 1 of the present invention.
[0032] Figure 7 This is a three-dimensional diagram of a box-type column provided in Example 3 of the present invention.
[0033] Figure 8 This is an installation status diagram of a box-type column variable-section box provided in Example 3 of the present invention.
[0034] Fig. 9 This is a diagram showing the installation status of a protruding portion of a box-type column provided in Example 3 of the present invention.
[0035] Fig.10 This is an installation status diagram of a box-type column sealing plate provided in Example 3 of the present invention.
[0036] Fig.11 This is a diagram showing the installation status of a protruding stiffening plate of a box-type column provided in Example 3 of the present invention.
[0037] Fig.12 This is a diagram showing the installation status of a box-type column protruding from a top plate provided in Example 3 of the present invention.
[0038] Fig.13 This is a diagram showing the installation status of the second rib of a box-type column provided in the third embodiment of the present invention.
[0039] Fig.14 This is a diagram showing the installation status of the second web of a box-type column provided in Example 3 of the present invention.
[0040] Fig.15 This is a diagram showing the installation status of the second inner partition of a box-type column provided in Example 3 of the present invention.
[0041] Fig.16 It is a stereoscopic diagram of a box-type column provided in Example 4 of the present invention.
[0042] Fig.17 This is an installation status diagram of the third top plate of a box-type column provided in Example 4 of the present invention.
[0043] Fig.18 This is a diagram showing the installation status of the third rib of a box-type column provided in the fourth embodiment of the present invention.
[0044] Fig.19 This is a diagram showing the installation status of the third web of a box-type column provided in Example 4 of the present invention.
[0045] Fig. 20 This is a diagram showing the installation status of the third inner partition of a box-type column provided in Example 4 of the present invention.
[0046] Main component symbols: 1. First body; 11. First inner partition; 12. First bottom plate; 13. First web plate; 14. First top plate; 15. First rib plate; 16. Box column foot plate; 2. The first box column corbel; 3. Second main body; 31. Second inner partition; 32. Second bottom plate; 33. Second web plate; 34. Second top plate; 35. Second rib plate; 4. protrusion; 41. protruding bottom plate; 42. protruding top plate; 43. protruding stiffening plate; 44. protruding web plate; 45. closing plate; 5. Variable cross-section box; 51. Box bottom plate; 52. Box belly plate; 53. Box top plate; 6. Second box column corbel; 7. third main body; 71. third inner partition; 72. third bottom plate; 73. third web plate; 74. third top plate; 75. third rib plate; 8. The third box column corbel. DETAILED DESCRIPTION
[0047] The following will be combined with the accompanying drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0048] The term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure or characteristic that may be included in at least one implementation of the present invention. In the description of the present invention, it should be understood that the orientation or positional relationship indicated by the terms "upper", "lower", "top", "bottom", etc. is based on the orientation or positional relationship shown in the accompanying drawings, which is only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation of the present invention. In addition, the terms "first" and "second" are used only for descriptive purposes, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Thus, the features defined as "first" and "second" may include one or more of the features explicitly or implicitly. Moreover, the terms "first", "second", etc. are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchangeable where appropriate, so that the embodiments of the present invention described herein can be implemented in an order other than those illustrated or described herein.
[0049] Embodiment 1 Refer to the attached drawings of the specification, such as Figure 1-Figure 6As shown, a box column proposed in the present application includes a first main body 1 and a plurality of first box column corbels 2 welded to the surface of the first main body 1. The first main body 1 includes a first bottom plate 12, a first top plate 14 arranged at a position corresponding to the first bottom plate 12, and first web plates 13 on both sides connecting the first bottom plate 12 and the first top plate 14. The front and rear ends of the first main body 1 are closed by a box column foot plate 16.
[0050] A first inner partition plate 11 is disposed inside the first main body 1, and the first inner partition plate 11 is welded and fixed to the first bottom plate 12, the first web plate 13 and the first top plate 14 of the first main body 1. A through hole is disposed in the center of the first inner partition plate 11.
[0051] The first body 1 further includes a first rib 15. The first rib 15 is fixed to the first bottom plate 12, the first top plate 14 and the first web 13 by welding. The first rib 15 is also welded and fixed between adjacent first inner partitions 11. The cross-sectional shape of the first rib 15 is "T" shaped.
[0052] The present application proposes a box-type column manufacturing process, including a box-type column, and further comprising the following steps: S100, material preparation: The purpose is to pre-process the materials that make up the box column, including: 1) Cutting: A 30 mm machining allowance is set along the length direction of the first bottom plate, the first web plate and the first top plate.
[0053] 2) Bevel processing: Use semi-automatic flame cutting machine for processing.
[0054] 3) Processing of special-shaped parts: Special-shaped parts are cut by flame CNC cutting or plasma cutting. The allowable deviation of the parts after cutting is shown in Table 1: 4) Splicing requirements: The butt length between the first bottom plate, the first top plate and the first web plate is greater than or equal to 600mm, the butt welds between the first bottom plate, the first top plate and the first web plate are staggered by at least 200mm, and the butt welds and the first inner partition plate and stiffening plate are staggered by at least 200mm.
[0055] 5) Processing of the first rib: T-shaped ribs can be cut from I-beams along the axis.
[0056] 6) Processing of the first inner partition: Assemble the welding backing plate according to the requirements of the inner partition weld, control the width and diagonal size of the inner partition, the length of the positioning weld on the inner partition is 40-60mm, and the spacing of the positioning weld is 200-300mm.
[0057] The first main body part of the box column is processed after the material is prepared.
[0058] S110, Inner partition positioning and assembly: Figure 6 As shown, the inner partition is vertically arranged on the first bottom plate according to a preset spacing, and the first rib plate longitudinally arranged on the first bottom plate is assembled and welded.
[0059] S120, assemble the first web: Figure 5 As shown, the first bottom plate, the first web plate and the inner partition plate are pressed against each other, and the verticality of the first web plate and the edge of the first bottom plate is checked to ensure that the first web plate is aligned with the end of the first bottom plate. After passing the test, positioning welding is performed.
[0060] S130, welding the first inner baffle: welding the first inner baffle and the first web and the first bottom plate to form a full penetration weld, and performing ultrasonic testing after welding.
[0061] S140, welding the first rib located on the first web: Figure 4 As shown, the double-sided fillet welds between the first rib and the first web and the first inner partition are welded. When welding, welding is first performed at a position parallel to the first web. The positions that require overhead welding are welded inside the box after the box is turned over.
[0062] S150, first top plate assembly: Figure 3 As shown, if the first top plate is provided with a first rib plate, the first rib plate is welded on the first top plate in advance. Then the first top plate is covered on the first web plates on both sides, and a 2-3mm welding shrinkage margin is added in the cross-sectional height direction when covering the plate. The first top plate is pressed tightly against the first web plate and the first inner partition plate, and the cross-sectional dimensions are confirmed, and the first web plate is aligned with the first bottom plate and the corner of the first top plate. After the distortion is qualified, positioning welding is performed.
[0063] S160. Perform base welding and reinforcement on the main weld of the first main body: turn the first main body over so that the first top plate is located at the bottom of the first main body. At this time, the welder enters the first main body to weld the full penetration weld between the first inner partition and the first top plate, and welds the welds between the first rib plate and the first top plate, the first bottom plate, the first web plate and the inner partition.
[0064] S170, welding the first main body weld, the main weld of the box body is welded by gas shielded welding for base and submerged arc welding for cover. The specific operation is as follows: 1) The welding method adopts CO2 gas shielded welding (GMAW) and submerged arc welding (SAW).
[0065] 2) Welding wire selection is shown in Table 2: Table 2: Welding wire selection table 3) Welding process parameters: a. Gas shielded welding parameters: welding current 200-290 (A), voltage 26-32 (V), welding speed 30-45cm / min; b. Submerged arc welding parameters: welding current 600-750 (A), voltage 34-40 (V), welding speed 27-40cm / min.
[0066] 4) Preparation before welding: Before welding, the oxides and cutting slag within 100mm on both sides of the groove must be cleaned.
[0067] 5) The welding sequence of the first main weld is as follows: a. Use CO2 gas shielded welding to weld the weld between the web and the bottom plate to 1 / 3 of the groove depth, and turn it upside down; b. Use CO2 gas shielded welding and submerged arc welding to weld the welds of the web and top plate to 1 / 2 of the groove depth, and then turn it upside down. For example, first weld the weld to 1 / 3 of the groove by CO2 gas shielded welding, and then weld the weld to 1 / 2 of the groove by submerged arc welding; c. Use submerged arc welding to weld the remaining 2 / 3 of the groove depth of the weld between the web and the bottom plate, and turn it upside down; d. Use submerged arc welding to weld the remaining 1 / 2 of the groove depth of the weld between the web and the top plate.
[0068] Due to the principle of thermal expansion and contraction, when welding the box, the welding heat introduced causes the box weld to expand. Therefore, in the traditional method, after welding one side of the weld completely, the other side of the weld is turned over and welded, which will cause the box weld to expand unevenly, resulting in welding deformation of the box.
[0069] In this embodiment, when welding the main body weld, the weld groove is divided into two layers. The inner layer of the weld groove is welded first each time, and then the outer layer of the weld groove is welded. This makes the welding heat input of the welds on the upper and lower sides almost equal, thereby reducing or avoiding deformation problems during the box welding process.
[0070] When welding the weld groove, in this embodiment, it is divided into two layers and four welding times. When the box thickness is thick, the groove can also be divided into more levels, such as four layers and eight welding times, eight layers and sixteen welding times.
[0071] In this embodiment, when welding the inner layer of the weld groove, CO2 gas shielded welding is used for welding, and when welding the outer layer of the weld groove, submerged arc welding is used for welding. When submerged arc welding is used, the welding current is large, and it is easy to break through the liner during welding. Therefore, this problem can be avoided by first performing CO2 gas shielded welding and then performing submerged arc welding.
[0072] 6) Preheating requirements and temperature selection are shown in Table 3. This embodiment takes Q345 steel as an example: Table 3: Preheating temperature table S180, Correction: Flame correction of bending and twisting deformation of the box.
[0073] S190, face milling: Place the first body on the end milling machine platform, the first body is perpendicular to the end milling equipment, and the first body is pressed against the working platform. Milling plane requirements: flatness is less than 0.3mm, and the verticality between the milling plane and the first body is less than or equal to 1.5h / 1000.
[0074] S200, assembly of the first box column corbel and box column foot plate, such as Figure 2 As shown, the specific steps are as follows: 1) Make the first box column corbel: The first box column corbel includes the wing plates on both sides and the web plate between the wing plates. Double-sided fillet welds are used between the web plate and the wing plates of the H-shaped steel corbel. After welding, the angular deformation of the wing plates is flame corrected, and the stiffening plates on the web plates are assembled and welded. The wing plates and the first main body are fully melted through, and the web plates and the box body are partially melted through.
[0075] 2) Shot blasting and rust removal are performed on the first main body, the first box column corbel, and the box column foot plate.
[0076] 3) Fixed length of the first main body: According to the drawing dimensions, the added margin of the first main body is marked and cut by a semi-automatic cutting machine, the groove of the welding part of the box column foot plate is processed, and the groove is polished after completion.
[0077] 4) Place the first body on the assembly platform, establish a horizontal reference, and draw lines on the first body according to the size and position of each component external to the first body on the drawing. The lines include the center line and the reference line, and the part position is marked with double lines; The components of the multi-layer corbels are made by the method of drawing wires and erecting poles, and the corbels and connecting plates are based on the milling plane of the column top; 5) Assembly box column base: Figure 1 As shown, the weld between the box column foot plate and the first main body is required to be fully penetrated to the first level; the stiffening plate, the first rib plate and the box column foot plate are tightly pressed against each other without welding; 6) Painting: After sandblasting and rust removal, the box-type columns that have been manufactured and inspected are sprayed according to the spraying positions in the drawings.
[0078] Embodiment 2 For a long box column, it is divided into multiple parts and the box columns are manufactured separately before being assembled. The multiple parts of the box columns are manufactured according to the manufacturing sequence in the first embodiment. When multiple box columns are combined and assembled, the butt welds of the first main bodies of adjacent box columns are staggered by at least 200mm, and the butt welding process is welded by submerged arc welding. For example, if the standard length is 10m and a 40m long box column is required, it is divided into four parts and manufactured separately before being combined.
[0079] By decomposing a long box column into multiple parts, the inner partition in each part is closer to the port of the box column. Therefore, when workers enter the box column to perform welding, the safety factor of the operation is higher.
[0080] Embodiment 3 Refer to the attached drawings of the specification, such as Figure 7-Figure 15 As shown, a box-type column proposed in the present application includes a second main body 3, a protrusion 4 is arranged on the side of the second main body 3, and a variable-section box 5 is arranged at the end of the second main body 3. The second main body 3 includes a second bottom plate 32, a second top plate 34 corresponding to the second bottom plate 32, and a second web 33 connecting the second bottom plate 32 and the second top plate 34. A plurality of second inner partitions 31 are arranged at intervals inside the second main body 3, and a through hole is arranged in the center of the second inner partition 31. The second main body 3 also includes a second rib 35, and the second rib 35 is arranged on the second bottom plate 32, the second web 33 and the second top plate 34. The cross-sectional shape of the second rib 35 is a "T" shape.
[0081] The protrusion 4 includes a protruding bottom plate 41 integrally formed with the second bottom plate 32, a protruding top plate 42 integrally formed with the second top plate 34, a protruding web 44 connecting the protruding bottom plate 41 and the protruding top plate 42, a protruding stiffening plate 43 located between the protruding bottom plate 41 and the protruding top plate 42, and a sealing plate 45 arranged at the end opening of the protrusion 4.
[0082] The variable cross-section box 5 includes a box bottom plate 51, a box top plate 53 corresponding to the box bottom plate 51, and a box web 52 connecting the box top plate 53 and the box bottom plate 51. The box top plate 53 and the box bottom plate 51 are formed by splicing a plurality of flat plates or bent plates at a preset angle to form a variable cross-section box 5 with a variable box cross-section. A plurality of second inner partitions 31 are arranged inside the variable cross-section box 5 at preset intervals.
[0083] The present application proposes a box-type column manufacturing process, including a box-type column, and further comprising the following steps: S300, material preparation: Process the materials for assembling box columns according to relevant processes; S310, manufacturing a variable cross-section box: The variable cross-section box is manufactured separately from the second main body, and the manufacturing of the variable cross-section box includes the following processes: 1) Install the second inner partition on the bottom plate of the box; 2) Install the box belly plate and box top plate, and weld them after installation; 3) Perform end milling on the welded variable-section box.
[0084] S320, such as Fig.15As shown, the second bottom plate and the protruding bottom plate are integrally formed, the second inner partition plate and the second bottom plate are assembled, and the second rib plate located on the second bottom plate is assembled and welded at the same time. The groove of the second inner partition plate faces the second main body port on the closer side, which is convenient for workers to enter the box body for welding.
[0085] S330, such as Fig.14 As shown, assemble the second webs on both sides, weld the welds between the second inner partition and the second web and the second bottom plate, and perform ultrasonic testing after welding. The groove of the second web located on one side of the protrusion is divided into two cases, one is that when the second web is located at the protrusion, the second web has a single-sided groove of 45°, and the other is that the groove of the second web is 45° except for the part located at the protrusion.
[0086] S340, such as Fig.13 As shown, the second rib located on the second web is assembled and welded by fillet welds.
[0087] S350, such as Fig.12 As shown, the second top plate is assembled and welding shrinkage allowance is added to the box cross section; before the second top plate is installed, a concealed inspection is performed on the other three sides of the box.
[0088] S360, flip the second top plate and the second bottom plate, at which point the second top plate is located at the bottom of the second main body, weld the weld between the second inner partition plate and the second top plate, and perform ultrasonic testing 24 hours after welding.
[0089] S370, assemblers and welders enter the box, assemble the second rib plate at the bottom of the second bottom plate in the box, and weld it.
[0090] S380, welding of the main body welds of the box body: manual welding for base welding, submerged arc welding for filling and covering.
[0091] S390, protrusion assembly: Fig.11 As shown, the main weld of the protrusion is subjected to hidden inspection and ultrasonic testing, and the protruding stiffening plate located between the protruding top plate and the protruding bottom plate is assembled. Single-sided backing welding is adopted, and the groove is facing the side with larger space, which can increase the supporting structure to prevent deformation.
[0092] S400, assembly of protruding web: Fig.10 As shown, single-sided groove full penetration welding is adopted between the protruding web and the second top plate and the second bottom plate; single-sided groove backing welding is adopted between the protruding web and the protruding stiffening plate, and ultrasonic testing is performed after welding.
[0093] S410, Sealing plate welding: Fig.10 As shown, the sealing plate weld adopts single-sided groove backing welding.
[0094] S420, such as Figure 8As shown, the variable cross-section box body that has been made is connected to the main box body. The connection is welded with a single-sided liner for full penetration welding to control the misalignment. After the box body connection is completed, the weld is tested by ultrasonic wave and then shot blasted for rust removal. Figure 7 As shown, the prefabricated second box column bracket is first shot blasted and then assembled and welded with the second main body.
[0095] S430, the second box column bracket assembly: Figure 7 As shown, the manufactured second box column bracket is assembled and welded to the second main body, ultrasonic testing is performed after welding, the second main body is cut for the second time, the groove is cut at the bottom of the column, and ear plates are installed on both side ends of the second main body.
[0096] S440. When the second main body is formed by splicing multiple sections of box-type columns, the requirements for the bottom groove of the box-type columns are: groove angle 35°, gap 6mm, full welding of the inner lining plate and the column wall plate, and weld foot 6mm.
[0097] S450, check: box column distortion, end section and diagonal; corbel layer height, adjacent corbel diagonal, corbel eccentricity column center; S460, Rust removal and painting: Sandblast and remove rust on the box-type columns that have been manufactured and tested to be qualified; the painting requirements and non-painted areas shall be implemented in accordance with the instructions and weld drawings.
[0098] Embodiment 4 Refer to the attached drawings of the specification, such as Figure 16-Figure 20 As shown, a box-type column proposed in the present application includes a third main body 7 and a plurality of third box column corbels 8 welded to the surface of the third main body 7, and the third main body 7 includes a third inner partition plate 71, a third bottom plate 72, a third top plate 74, a third web plate 73 and a third rib plate 75.
[0099] Compared with the box-type column in the first embodiment, the box-type column in this embodiment has a larger main cross-sectional size, and its manufacturing process and processing sequence are the same as those of the box-type column in the first embodiment.
[0100] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by any technician familiar with the technical field within the technical scope disclosed by the present invention should be covered within the protection scope of the present invention.
Claims
1. A box column, characterized in that: include: The box column body comprises an inner partition plate located inside the box column body, a bottom plate, a top plate corresponding to the bottom plate, and a web connecting the bottom plate and the top plate; the box column body further comprises a rib plate, which is fixed to the bottom plate, the top plate, and the web surface; An external connection part is fixed to the box column body, and the external connection part includes a box column corbel.
2. A box-type column according to claim 1, characterized in that: The box column can be composed of multiple box column bodies connected in sequence by welding.
3. A box-type column according to claim 1, characterized in that: The box column body also includes a box column foot plate, and the box column foot plate is located at the end of the box column body.
4. A box-type column according to claim 1, characterized in that: The box column body also includes a protruding portion, which includes a protruding bottom plate, a protruding top plate, a protruding stiffening plate, a protruding web plate and a sealing plate; the protruding bottom plate is integrally formed with the bottom plate, and the protruding top plate is integrally formed with the top plate.
5. A box-type column according to claim 1, characterized in that: The external connection part also includes a variable cross-section box, which includes a box bottom plate, a box top plate and a box belly plate. The box bottom plate and the box top plate are formed by splicing a plurality of flat plates or bent plates at a preset angle.
6. A method for manufacturing a box-type column, characterized in that: The method for producing the box-type column according to any one of claims 1 to 3 comprises the following steps: S10, material preparation: pre-process the parts that make up the box column; S11. Positioning and assembling the inner baffles: vertically arranging the inner baffles on the bottom plate at a preset spacing, and assembling and welding the ribs longitudinally arranged on the bottom plate; S12. Assemble the web: press the bottom plate, web and inner partition together, check the verticality of the web and bottom plate edges, ensure that the ends of the web and bottom plates are aligned, and perform positioning welding after passing the test; S13, welding inner diaphragm: welding the full penetration weld between the inner diaphragm and the web and bottom plate, and conducting ultrasonic testing after welding; S14. Welding of ribs on the web: Weld double-sided fillet welds between the ribs and the web and inner partitions. When welding, first weld in parallel with the web. For positions that require overhead welding, wait until the box is turned over before welding inside the box. S15. Top plate assembly: When ribs are provided on the top plate, the ribs are welded to the top plate in advance, and then the top plate is covered on the webs on both sides. When covering the plate, a 2-3mm welding shrinkage allowance is added in the direction of the cross-sectional height, and the top plate is pressed against the web and inner partition, and the cross-sectional dimensions and the alignment of the web, bottom plate and top plate corners are confirmed. Positioning welding is performed after the distortion is qualified. S16. Perform base welding and reinforcement on the main welds of the box column body: After turning over the box column body, the welder enters the interior of the box column body to weld the full penetration welds between the inner partition and the top plate, and welds the welds between the rib plate and the top plate, bottom plate, web plate and inner partition. S17, welding the main weld of the box column, the welding sequence is as follows: a. Use CO2 gas shielded welding to weld the weld between the web and the bottom plate to 1 / 3 of the groove depth, and turn it upside down; b. Use CO2 gas shielded welding and submerged arc welding to weld the welds between the web and the top plate to 1 / 2 of the groove depth, and turn it upside down; c. Use submerged arc welding to weld the remaining 2 / 3 of the groove depth of the weld between the web and the bottom plate, and turn it upside down; d. Use submerged arc welding to weld the remaining 1 / 2 of the groove depth of the weld between the web and the top plate. S18, Correction: Flame correction is performed on the bending and twisting deformation of the box. S19, end milling: Place the box column body on the end milling machine platform, the box column body is perpendicular to the end milling equipment, and press the box column body on the working platform. Milling plane requirements: flatness is less than 0.3mm, and the verticality of the milling plane and the first body is less than or equal to 1.5h / 1000. S20. Assembling the box column corbel and the box column foot plate, and obtaining a box column as claimed in claim 1 or 3 after assembly.
7. A method for manufacturing a box-type column according to claim 6, characterized in that: The material preparation process in step S10 includes: 1) Cutting: Set a 30mm machining allowance along the length direction of the bottom plate, web plate and top plate; 2) Bevel processing: semi-automatic flame cutting machine is used for processing; 3) Processing of special-shaped parts: Special-shaped parts are processed by flame CNC cutting or plasma cutting; 4) Splicing requirements: The butt length between the bottom plate, top plate and web plate is greater than or equal to 600mm, the butt welds between the bottom plate, top plate and web plate are staggered by at least 200mm, and the butt welds and the inner partition and stiffening plate are staggered by at least 200mm; 5) Processing of the first rib: T-shaped ribs can be cut from I-beams along the axis; 6) Processing of the first inner partition: assemble the welding backing plate according to the requirements of the inner partition weld, control the width and diagonal size of the inner partition, the length of the positioning weld on the inner partition is 40-60mm, and the spacing of the positioning weld is 200-300mm; In step S17, welding the box column body also includes the following process: 1) The welding method adopts CO2 gas shielded welding and submerged arc welding; 2) During the welding process, the welding wire for CO2 gas shielded welding is Q355 steel, model ER50-6, type solid wire, diameter 1.2mm; the welding wire for submerged arc welding is Q355 steel, model H 10 Mn2, type is solid wire, diameter is 4.0mm, flux is CHF101; 3) Welding process parameters: a. Gas shielded welding parameters: welding current 200-290 (A), voltage 26-32 (V), welding speed 30-45cm / min; b. Submerged arc welding parameters: welding current 600-750 (A), voltage 34-40 (V), welding speed 27-40cm / min; 4) Preparation before welding: Before welding, the oxides and cutting slag within 100mm on both sides of the groove need to be cleaned; 5) Welding preheating; In step S20, the process of assembling the box column corbel and the box column foot plate includes: 1) Make the box column corbel: The box column corbel includes the wing plates on both sides and the web plate between the wing plates. Double-sided fillet welds are used between the web plate and the wing plates of the H-shaped steel corbel. After welding, the angular deformation of the wing plates is flame corrected, and the stiffening plates on the web plates are assembled and welded. The wing plates and the main body are fully melted to the first level, and the web plates and the box body are partially melted; 2) Shot blasting and rust removal on the box column corbels. 3) Main body fixed length: according to the drawing size, the added margin of the main body is marked and cut by a semi-automatic cutting machine, the groove of the welding part of the box column foot plate is processed, and the groove is polished after completion; 4) Place the main body on the assembly platform, establish a horizontal reference, and draw lines on the main body according to the size and position of each component external to the main body on the drawing. The lines include the center line and the reference line, and the part position is marked with double lines; The components of the multi-layer corbels are made by the method of drawing wires and erecting poles, and the corbels and connecting plates are based on the milling plane of the column top; 5) Assemble the box column foot plate: The weld between the box column foot plate and the main body is required to be fully penetrated to the first level; the stiffening plate and rib plate set on the box column foot plate are tightly pressed against the box column foot plate without welding; 6) Painting: After sandblasting and rust removal, the box-type columns that have been manufactured and inspected are sprayed according to the spraying positions in the drawings.
8. A method for manufacturing a box-type column according to claim 6, characterized in that: The box column can be made by connecting multiple box column bodies in sequence by welding. The production method is as follows: The box-type column is divided into multiple parts, and the box-type columns are manufactured separately and then assembled. When multiple box-type columns are combined and assembled, the direct butt welds of the first main bodies of adjacent box-type columns are staggered by at least 200mm, and submerged arc welding is used in the butt welding process.
9. A method for manufacturing a box-type column according to claim 6, characterized in that: The box column body also includes a protruding portion, which includes a protruding bottom plate, a protruding top plate, a protruding stiffening plate, a protruding web plate and a sealing plate; the protruding bottom plate is integrally formed with the bottom plate, and the protruding top plate is integrally formed with the top plate. The manufacturing steps are as follows: S21, the protruding bottom plate and the bottom plate, the protruding top plate and the top plate are integrally formed; S22. Conduct concealed inspection and ultrasonic inspection on the main weld of the protruding part, assemble the protruding stiffening plate between the protruding top plate and the protruding bottom plate, and adopt single-sided backing welding; S23. Assemble the protruding web, use single-sided groove full penetration welding between the protruding web and the top plate and bottom plate, and use single-sided groove backing welding between the protruding web and the protruding stiffening plate, and perform ultrasonic testing after welding; S24. Sealing plate welding: The sealing plate weld adopts single-sided groove backing welding.
10. A method for manufacturing a box-type column according to claim 6, characterized in that: The external connection part also includes a variable cross-section box, which includes a box bottom plate, a box top plate and a box belly plate. The box bottom plate and the box top plate are formed by splicing a plurality of flat plates or bent plates at a preset angle. The production of the variable cross-section box includes the following process: S25, installing the inner partition plate on the bottom plate of the box; S26, install the box body belly plate and the box body top plate, and weld them after installation; S27, performing end milling on the welded variable cross-section box to complete the production of the variable cross-section box; S28. The variable-section box body is connected to the main box body. The connection point is welded with a single-sided liner for full penetration welding to control the misalignment. After the connection is completed, the weld is ultrasonically inspected and shot blasted for rust removal.