Preparation method of gel-state polymer sodium ion battery and sodium ion battery

By using gel polymers and black phosphorus quantum dots in sodium ion batteries, the problem of poor dispersion of black phosphorus in the battery is solved, the battery impedance is reduced, the high-rate performance and safety is improved, and the black phosphorus is achieved. Excellent photoelectric and photothermal performance.

CN119009097APending Publication Date: 2024-11-22ZHUHAI SMOOTHWAY ELECTRONICS MATERIALS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411158814.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

When black phosphorus is used as a negative electrode material in chemical power supplies, it is difficult to exert its photoelectric and photothermal properties, and its dispersion in the battery is limited, resulting in poor quantum effects and affecting battery performance.

Method used

Using the preparation method of gel polymer sodium ion battery, the gel electrolyte precursor is prepared and cured in the battery cell, and the black phosphorus quantum dots are dispersed in the gel polymer, reducing the impedance during the battery cycle, and through The low-impedance SEI and CEI films are formed in situ to improve the high-rate performance of the battery.

Benefits of technology

It effectively reduces the cyclic impedance of the battery, improves the high-rate performance and safety performance of sodium ion batteries, and enhances the quantum effect of black phosphorus quantum dots, improves stability, and significantly improves battery performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005005847260000081
    Figure BDA0005005847260000081
  • Figure BDA0005005847260000091
    Figure BDA0005005847260000091
  • Figure BDA0005005847260000092
    Figure BDA0005005847260000092
Patent Text Reader

Abstract

The invention provides a preparation method of a gel-state polymer sodium-ion battery and the sodium-ion battery. The preparation method comprises the following steps: preparing a positive plate; preparing a negative plate; mixing sodium salt, a non-aqueous organic solvent, a monomer, a cross-linking agent, an initiator and the black phosphorus quantum dots to obtain a gel electrolyte precursor; separating the positive plate and the negative plate at an interval by using an isolating membrane, assembling into a naked battery cell, packaging, pouring a gel electrolyte precursor, sealing, and forming to obtain a battery cell; and curing the battery cell and carrying out post-treatment. The black phosphorus quantum dots are attached to the surfaces of the positive electrode and the negative electrode, impedance in the circulation process can be reduced, and the rate performance of the sodium-ion battery is improved. In addition, the ionic conductivity of the polymer can be improved, so that the defect of low ionic conductivity of the polymer serving as an electrolyte is overcome. Meanwhile, the electrolyte adopts an in-situ cured gel electrolyte, so that the contact between the positive electrode and the isolating membrane interface and between the negative electrode and the isolating membrane interface can be improved, the growth of sodium dendrites is inhibited, and the safety performance of the battery is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of new energy batteries, in particular to solid-state batteries, and more particularly to a preparation method of a gel polymer sodium ion battery and a sodium ion battery. Background Art

[0002] Black phosphorus is a new type of direct bandgap two-dimensional material. Its bandgap can be adjusted from 0.3eV (bulk state) to 1.5eV (monolayer) by the number of layers. Therefore, it can absorb light with wavelengths ranging from visible light to infrared for communication. In addition, its high carrier mobility (up to 1000cm when the thickness is 10nm) 2 ˙v -1 ˙s -1 ) and a higher on-off ratio (104), which shows great potential advantages in the fields of semiconductors, optoelectronics, and photothermal energy.

[0003] Attempts to use black phosphorus in chemical power sources include using it as an auxiliary negative electrode material to improve the energy density of lithium batteries. In practical applications, black phosphorus needs to be stripped into single-layer, few-layer or multi-layer black phosphorus (i.e., phosphorene) to exert its excellent photoelectric and photothermal properties. However, when used in the negative electrode, it is difficult to exert the effect of black phosphorus because black phosphorus exists in the negative electrode. Some researchers have tried to use black phosphorus in the electrolyte of chemical power sources, mixing black phosphorus nanosheets and liquid electrolytes into methyl methacrylate monomers for polymerization to obtain a black phosphorus nanosheet polymer composite film, and then using this composite film and the electrode to assemble into a button battery. Although this method based on the electrode can better exert the effect of black phosphorus, the performance of the battery itself is quite different from that of commercial batteries. However, even if the composite film is used to assemble a commercial battery, the dispersion of black phosphorus nanosheets in the battery is limited, and its quantum effect is not well exerted. Summary of the invention

[0004] Based on the above problems, the object of the present invention is to provide a method for preparing a gel polymer sodium ion battery and a sodium ion battery, which can effectively exert the effect of black phosphorus in the battery, reduce the impedance of the battery during the cycle process, and effectively improve the high-rate performance of the sodium ion battery.

[0005] To achieve the above object, the present invention provides a method for preparing a gel polymer sodium ion battery, comprising the steps of:

[0006] (1) preparing a positive electrode sheet;

[0007] (2) preparing a negative electrode sheet;

[0008] (3) mixing sodium salt, non-aqueous organic solvent, monomer, cross-linking agent, initiator and black phosphorus quantum dots to obtain a gel electrolyte precursor;

[0009] (4) using an isolation film to separate the positive electrode sheet and the negative electrode sheet, assembling them into a bare cell and then packaging them, pouring the gel electrolyte precursor and sealing them to form a cell;

[0010] (5) Curing and post-processing the battery cell.

[0011] In the technical solution adopted by the present invention, a gel electrolyte precursor is first prepared, then infused and cured after formation, and a gel electrolyte can be obtained by in-situ polymerization. Compared with the method of first preparing a gel electrolyte membrane and then assembling it into a battery, the interface impedance and interface integrity are better, the cycle performance of the obtained battery is better, and it is not easy to precipitate sodium. The present invention uses black phosphorus quantum dots dispersed in a gel polymer. Black phosphorus quantum dots are zero-dimensional materials. Compared with two-dimensional materials such as black phosphorus nanosheets, their quantum effect is stronger, and they are easier to disperse in gel polymers to form a stable system. Therefore, it is relatively stable during the storage of gel electrolytes. Black phosphorus itself has a high carrier mobility. It is attached to the surface of the positive and negative electrodes, which can reduce the impedance during the cycle. During the battery cycle, the black phosphorus quantum dots decompose and form fluorinated phosphides in situ. The impedance of the formed SEI and CEI films is also low, which can improve the high-rate performance of sodium ion batteries. In addition, black phosphorus quantum dots can improve the ionic conductivity of polymers to make up for the defect of low ionic conductivity of polymers as electrolytes. At the same time, the electrolyte of the present invention adopts an in-situ solidified gel electrolyte, which can improve the contact between the positive electrode and the isolation membrane interface and the negative electrode and the isolation membrane interface, inhibit the growth of sodium dendrites, adsorb liquid electrolyte (lithium salt, etc.) in gel electrolysis, reduce free electrolyte, and improve the safety performance of the battery.

[0012] As a technical solution of the present invention, the positive electrode active material, the positive electrode conductive agent and the positive electrode binder are mixed to form a positive electrode slurry, which is then coated on an aluminum foil, dried and rolled to obtain the positive electrode sheet.

[0013] As a technical solution of the present invention, the negative electrode active material, the negative electrode conductive agent and the negative electrode binder are mixed to form a negative electrode slurry, which is then coated on a copper foil, dried and rolled to obtain the negative electrode sheet.

[0014] As a technical solution of the present invention, the positive electrode active material includes α-NaFeO2, NaCoO2, Na 0.7 [Fe 0.7 Mn 0.3 ]O2、Na(Mn 0.25 Fe 0.25 Co 0.25 Ni 0.25 )O2, NaMnO2, Na 0.5 [Fe 1 / 2 Mn 1 / 2 ]O2、Na 0.67 [Fe 1 / 2 Mn 1 / 2]O2, Na[Ni 0.35 Fe 0.40 Mn 0.25 ]O2, Na[Ni 0.30 Fe 0.45 Mn 0.25 ]O2, Na[Ni 0.25 Fe 0.50 Mn 0.25 ]O2, Na[Ni 0.20 Fe 0.55 Mn 0.25 ]O2、Na 0.67 [Mn 0.60 Ni 0.15 Fe 0.25 ]O2、Na[Li 0.05 (Ni 0.25 Fe 0.25 Mn 0.5 ) 0.95 ]O2, Na2FePO4F, Na4Fe2(CN)6, NaNi 0.33 Fe 0.33 Mn 0.33 At least one of O2, NaFePO4, Na2FeP2O7, Na2MnPO4F, NaCoPO4, Na3V2(PO4)3, NaCrO2 and Na2Fe2(SO4)3.

[0015] As a technical solution of the present invention, the positive electrode conductive agent includes at least one of conductive carbon black, conductive graphite, carbon fiber, carbon nanotube and graphene.

[0016] As a technical solution of the present invention, the positive electrode binder includes polyvinylidene fluoride.

[0017] As a technical solution of the present invention, the negative electrode active material includes at least one negative electrode material selected from soft carbon, hard carbon, sodium titanate, MoS2, Fe2O3, Fe3O4, ZnS, Sb and SbSn.

[0018] As a technical solution of the present invention, the negative electrode conductive agent includes at least one of conductive carbon black, conductive graphite, carbon fiber, carbon nanotube and graphene.

[0019] As a technical solution of the present invention, the negative electrode binder includes sodium carboxymethyl cellulose and / or styrene-butadiene rubber.

[0020] As a technical solution of the present invention, the sodium salt includes at least one of sodium hexafluorophosphate, sodium difluorooxalatoborate, sodium tetrafluoroborate, sodium bisoxalatoborate, sodium perchlorate, sodium hexafluoroarsenate, sodium bis(fluorosulfonyl)imide, sodium trifluoromethylsulfonate and sodium bis(trifluoromethylsulfonyl)imide.

[0021] As a technical solution of the present invention, the non-aqueous organic solvent includes at least one of a carbonate organic solvent, a carboxylate organic solvent and an ether organic solvent.

[0022] As a technical solution of the present invention, the monomer includes at least one of methyl methacrylate, methyl acrylate and triacrylate of phosphate.

[0023] As a technical solution of the present invention, the cross-linking agent includes at least one of ethylene glycol dimethacrylate, pentaerythritol tetraacrylate and pentaerythritol triacrylate.

[0024] As a technical solution of the present invention, the initiator includes one or more of azobisisoheptanenitrile, azobisisobutyronitrile, azobisisobutyramidine hydrochloride, azobisisobutylimidazoline hydrochloride, benzoyl peroxide, potassium persulfate, ammonium persulfate, tert-butyl benzoyl peroxide and methyl ethyl ketone peroxide.

[0025] As a technical solution of the present invention, the black phosphorus quantum dots can be prepared by ball-milling blocky black phosphorus in a solvent to obtain a black scale dispersion, and then performing ultrasonication, centrifugation and drying.

[0026] As a technical solution of the present invention, the particle size of the black phosphorus quantum dots is 3 to 20 nm, and the black phosphorus quantum dots account for 0.005 to 0.200% of the total mass of the monomer and the cross-linking agent.

[0027] As a technical solution of the present invention, the curing conditions are a temperature of 40 to 70° C. and a time of 4 to 24 hours, and the post-treatment includes volume separation.

[0028] On the other hand, the present invention provides a gel polymer sodium ion battery prepared by a preparation method of a gel polymer sodium ion battery, comprising a positive electrode active material, a negative electrode active material and a gel electrolyte, wherein the gel electrolyte comprises a gel polymer, a sodium salt and black phosphorus quantum dots, and the gel polymer accounts for 3 to 90% of the mass of the gel electrolyte. DETAILED DESCRIPTION

[0029] The gel polymer sodium ion battery of the present invention comprises a positive electrode active material, a negative electrode active material and a gel electrolyte. The gel electrolyte comprises a gel polymer, a sodium salt and black phosphorus quantum dots. The sodium salt and the black phosphorus quantum dots are dispersed in the gel polymer, and the gel polymer accounts for 3 to 90% of the mass of the gel electrolyte, preferably 5 to 70%, more preferably 7 to 50%, and further preferably 9 to 5%. As an example, the gel polymer accounts for 3% to 90% of the mass of the gel electrolyte, but is not limited to 3%, 5%, 10%, 20%, 30%, 40%, 50%, 60%, 70%, 80%, 90%. The gel polymer is polymerized by monomers under the action of an initiator and a crosslinking agent. The monomer comprises at least one of methyl methacrylate, methyl acrylate and triacrylate of phosphoric acid. The crosslinking agent comprises at least one of ethylene glycol dimethacrylate, pentaerythritol tetraacrylate and pentaerythritol triacrylate. The initiator includes one or more of azobisisoheptanonitrile, azobisisobutyronitrile, azobisisobutyramidine hydrochloride, azobisisobutylimidazoline hydrochloride, benzoyl peroxide, potassium persulfate, ammonium persulfate, tert-butyl peroxide benzoyl and methyl ethyl ketone peroxide. The sodium salt includes at least one of sodium hexafluorophosphate, sodium difluorooxalate borate, sodium tetrafluoroborate, sodium bisoxalate borate, sodium perchlorate, sodium hexafluoroarsenate, sodium bis(fluorosulfonyl)imide, sodium trifluoromethylsulfonate and sodium bis(trifluoromethylsulfonyl)imide. The particle size of the black phosphorus quantum dots is 3 to 20 nm. As an example, the particle size can be, but is not limited to, 3 nm, 5 nm, 7 nm, 9 nm, 11 nm, 13 nm, 15 nm, 17 nm, 19 nm, and 20 nm.

[0030] The preparation method of the gel polymer sodium ion battery of the present invention comprises the steps of:

[0031] (1) preparing a positive electrode sheet;

[0032] (2) preparing a negative electrode sheet;

[0033] (3) mixing sodium salt, non-aqueous organic solvent, monomer, cross-linking agent, initiator and black phosphorus quantum dots to obtain a gel electrolyte precursor;

[0034] (4) using an isolation film to separate the positive electrode sheet and the negative electrode sheet and assemble them into a bare cell and then package them, and then pouring a gel electrolyte precursor and sealing them to form a cell;

[0035] (5) Curing and post-processing the battery cell.

[0036] In step (1), the positive electrode active material, the positive electrode conductive agent and the positive electrode binder are mixed to form a positive electrode slurry, which is then coated on an aluminum foil, dried, and rolled to obtain a positive electrode sheet. The positive electrode sheet can be prepared using conventional processes. The positive electrode active materials include α-NaFeO2, NaCoO2, Na 0.7 [Fe 0.7 Mn0.3 ]O2、Na(Mn 0.25 Fe 0.25 Co 0.25 Ni 0.25 )O2, NaMnO2, Na 0.5 [Fe 1 / 2Mn 1 / 2 ]O2、Na 0.67 [Fe 1 / 2 Mn 1 / 2 ]O2, Na[Ni 0.35 Fe 0.40 Mn 0.25 ]O2, Na[Ni 0.30 Fe 0.45 Mn 0.25 ]O2, Na[Ni 0.25 Fe 0.50 Mn 0.25 ]O2, Na[Ni 0.20 Fe 0.55 Mn 0.25 ]O2、Na 0.67 [Mn 0.60 Ni 0.15 Fe 0.25 ]O2、Na[Li 0.05 (Ni 0.25 Fe 0.25 Mn 0.5 ) 0.95 ]O2, Na2FePO4F, Na4Fe2(CN)6, NaNi 0.33 Fe 0.33 Mn 0.33 At least one of O2, NaFePO4, Na2FeP2O7, Na2MnPO4F, NaCoPO4, Na3V2(PO4)3, NaCrO2 and Na2Fe2(SO4)3. The positive electrode active material includes not only the above materials but also the corresponding coating and doping materials. The positive electrode active material is preferably Na[Ni 0.35 Fe 0.40 Mn 0.25 ]O2, Na[Ni 0.30 Fe 0.45 Mn 0.25 ]O2, Na[Ni 0.25 Fe 0.50 Mn 0.25 ]O2, Na[Ni 0.20 Fe 0.55 Mn 0.25 ]O2、Na 0.67 [Mn 0.60 Ni 0.15 Fe 0.25]O2、NaNi 0.33 Fe 0.33 Mn 0.33 O2 and other nickel iron manganese sodium positive electrode materials (NaNMF). The positive electrode conductive agent includes at least one of conductive carbon black, conductive graphite, carbon fiber, carbon nanotubes and graphene. The positive electrode binder includes polyvinylidene fluoride. The positive electrode slurry is prepared using NMP as a solvent. The mass ratio of the positive electrode active material, the positive electrode conductive agent and the positive electrode binder can be 90-98:0.5-5.0:0.5-5.0.

[0037] In step (2), the negative electrode active material, the negative electrode conductive agent and the negative electrode binder are mixed to form a negative electrode slurry, which is then coated on a copper foil, dried and rolled to obtain a negative electrode sheet. The negative electrode sheet can be prepared by conventional processes. The negative electrode active material includes a negative electrode material selected from at least one of soft carbon, hard carbon, sodium titanate, MoS2, Fe2O3, Fe3O4, ZnS, Sb and SbSn. As an example, the negative electrode active material of the present invention is hard carbon. The negative electrode conductive agent includes at least one of conductive carbon black, conductive graphite, carbon fiber, carbon nanotubes and graphene. The negative electrode binder includes sodium carboxymethyl cellulose and / or styrene-butadiene rubber. The negative electrode slurry is prepared using NMP or water as a solvent. The mass ratio of the negative electrode active material, the negative electrode conductive agent and the negative electrode binder can be 95-99:0.5-3.0:0.5-3.0.

[0038] In step (3), the sodium salt is selected from at least one of sodium hexafluorophosphate (NaPF6), sodium difluorooxalate borate (NaDFOP), sodium tetrafluoroborate (NaBF4), sodium bis(oxalate borate) (NaBOB), sodium perchlorate (NaClO), sodium hexafluoroarsenate (NaAsF6), sodium bis(fluorosulfonyl)imide (NaFSI), sodium trifluoromethylsulfonate (NaCF3SO3) and sodium bis(trifluoromethylsulfonyl)imide (NaTFSI). As an example, the sodium salt is sodium hexafluorophosphate (NaPF6). In some embodiments, the sodium salt is a mixture of sodium dioxalate borate (NaDFOP) and sodium hexafluorophosphate (NaPF6). The mass percentage of the sodium salt in the gel electrolyte precursor is 8 to 20%, specifically but not limited to 8%, 10%, 12%, 14%, 15%, 16%, 18%, 20%, preferably 10% to 15%, and further preferably, the mass percentage of the sodium salt in the gel electrolyte precursor is 14%.

[0039] The non-aqueous solvent is selected from at least one of carbonate organic solvents, carboxylate organic solvents and ether organic solvents. Specifically, the non-aqueous solvent may be, but is not limited to, ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), pentylene carbonate, vinylene carbonate (VC), dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), propylene carbonate (PC), butyl acetate (n-Ba), γ-butyrolactone (γ-Bt), propyl propionate (n-PP), ethyl propionate (EP), ethyl butyrate (Eb), ethylene glycol dimethyl ether (DME), ethylene glycol diethyl ether (ECS), diethylene glycol dimethyl ether (DEGME), triethylene glycol dimethyl ether (TEGDME), tetraethylene glycol dimethyl ether (TEGDME), 1,3-dioxolane (DOL), tetrahydrofuran (THF), methyltetrahydrofuran (MTHF), diphenyl ether and crown ether (CE). The mass percentage of the non-aqueous solvent in the gel electrolyte precursor is 60-90%, and may be but is not limited to 60%, 65%, 70%, 72%, 74%, 75%, 76%, 78%, 80%, 82%, 84%, 86%, 88%, 90%, preferably 75-88%.

[0040] Black phosphorus quantum dots (BPQDs) can exhibit typical quantum size effects, and their optical, electrical and chemical properties will change due to the reduction in size. The particle size of the black phosphorus quantum dots of the present invention is 3 to 20 nm, preferably 5 to 15 nm, and more preferably 6 to 10 nm. As an example, the particle size of the black phosphorus quantum dots may be, but not limited to, 3 nm, 5 nm, 7 nm, 9 nm, 11 nm, 12 nm, 14 nm, 16 nm, 18 nm, and 20 nm. The black phosphorus quantum dots account for 0.005 to 0.200% of the total mass of the monomer and the cross-linking agent, preferably 0.010% to 0.100%. As an example, the proportion of black phosphorus quantum dots may be, but not limited to, 0.005%, 0.010%, 0.020%, 0.040%, 0.080%, 0.100%, 0.120%, 0.140%, 0.160%, 0.180%, and 0.200%. Black phosphorus quantum dots are prepared by ball-milling block black phosphorus in a solvent to obtain a black scale dispersion, and then ultrasonicating, centrifuging and drying. Wherein, the mass ratio of block black phosphorus to solvent is 1 to 3:1000. As an example, the mass ratio of block black phosphorus to solvent may be, but is not limited to, 1:1000, 2:1000, and 3:1000. The solvent is selected from N-methylpyrrolidone (NMP). Ball milling is specifically ball milling in a zirconium oxide ball mill for 3 to 5 hours. Ultrasound is specifically ultrasonicating in an ultrasonicator for 9 to 11 hours. Centrifugation is specifically carried out in a centrifuge. Drying is specifically freeze-drying the supernatant obtained after centrifugation, and freeze-drying can specifically be drying in a cold dryer.

[0041] The monomer used in the polymerization includes at least one of methyl methacrylate, methyl acrylate and triacrylate of phosphate. The initiator includes one or more of azobisisoheptanenitrile (ABVN), azobisisobutyronitrile (AIBN), azobisisobutyramidine hydrochloride (AIBA), azobisisobutylimidazoline hydrochloride (AIBI), benzoyl peroxide (BPO), potassium persulfate, ammonium persulfate, tert-butyl peroxide benzoyl and methyl ethyl ketone peroxide. The crosslinking agent includes at least one of ethylene glycol dimethacrylate (EDMA), pentaerythritol tetraacrylate and pentaerythritol triacrylate. Wherein, the mass ratio of the monomer to the crosslinking agent is 1 to 10:1 to 10. As an example, the mass ratio of the two can be, but is not limited to, 1:9, 2:8, 3:7, 4:6, 5:5, 6:4, 7:3, 8:2, 9:1. The initiator is 0.1-0.5% of the mass of the monomer. As an example, the initiator can be, but is not limited to, 0.1%, 0.2%, 0.3%, 0.4%, or 0.5%.

[0042] In step (4), the curing conditions are a temperature of 40 to 70° C. and a time of 4 to 24 hours. As an example, the curing temperature may be, but is not limited to, 40° C., 45° C., 50° C., 55° C., 60° C., 65° C., 70° C. As an example, the curing time may be, but is not limited to, 4 hours, 8 hours, 12 hours, 16 hours, 20 hours, 24 hours. Post-processing includes volume separation.

[0043] In order to better illustrate the purpose, technical scheme and beneficial effects of the present invention, the present invention will be further described below in conjunction with specific embodiments. It should be noted that the following implementation method is a further explanation of the present invention and should not be used as a limitation of the present invention.

[0044] Example 1

[0045] (1) Preparation of positive electrode sheet

[0046] The highest charging voltage is 4.2V. 0.33 Fe 0.33 Mn 0.33 O2, adhesive PVDF and conductive agent SuperP are evenly mixed in a mass ratio of 95:1:4 to form a positive electrode slurry with a certain viscosity. The mixed positive electrode slurry is coated on both sides of an aluminum foil, and then dried and rolled to obtain a positive electrode sheet.

[0047] (2) Preparation of negative electrode

[0048] Hard carbon, conductive agent SuperP, and adhesive PVDF are prepared into negative electrode slurry in a mass ratio of 97:1:2, and mixed evenly. The mixed negative electrode slurry is coated on both sides of an aluminum foil, and then dried and rolled to obtain a negative electrode sheet.

[0049] (3) Preparation of gel electrolyte precursor

[0050] In a glove box filled with nitrogen (O2≤5ppm, H2O≤5ppm), ethylene carbonate (EC), diethyl carbonate (DEC) and ethyl methyl carbonate (EMC) were mixed in a mass ratio of 1:2:1 to obtain 76g of non-aqueous solvent, and then 8g of methyl methacrylate (MMA), 2g of ethylene glycol dimethacrylate (EDMA) and 0.02g of azobisisobutyronitrile (AIBN) were added, and then 0.02g of black phosphorus quantum dots (BPQDs) were added to obtain a mixed solution. The mixed solution was sealed and packaged and placed in a quick freezer (-4℃) for 2h before being taken out. In a glove box filled with nitrogen (O2≤5ppm, H2O≤5ppm), 14g of sodium hexafluorophosphate was slowly added to the mixed solution, and the gel electrolyte precursor was obtained after mixing evenly.

[0051] Among them, the preparation method of black phosphorus quantum dots is: put 200 mg of block black phosphorus and 100 ml of NMP into a zirconia ball mill, and obtain a black phosphorus dispersion after ball milling for 4 hours; put the black phosphorus dispersion into a PP centrifuge tube, ultrasonicate it with an ultrasonicator for 10 hours, centrifuge it, and take the supernatant to obtain a black phosphorus quantum dot dispersion; dry the black phosphorus quantum dot dispersion in a freeze dryer to obtain black phosphorus quantum dots.

[0052] (4) Preparation of sodium ion batteries

[0053] The positive electrode sheet, the isolation film and the negative electrode sheet are stacked in sequence to form a square battery cell, which is packaged with a polymer and filled with the prepared sodium ion battery non-aqueous electrolyte for formation.

[0054] (5) Solidification of sodium ion batteries

[0055] The formed battery is cured at 60°C for 24 hours, and the cured battery is subjected to a capacity division process to produce a sodium ion battery with a capacity of 1000 mAh.

[0056] The formulas of the gel electrolyte precursors of Examples 1 to 9 and Comparative Examples 1 to 3 are shown in Table 1. The preparation of the gel electrolyte precursors, the preparation of the positive electrode sheet, the preparation of the negative electrode sheet, and the preparation and curing of the sodium ion battery of Examples 2 to 9 and Comparative Examples 1 to 3 are the same as those of Example 1.

[0057] Table 1 Formulas of gel electrolyte precursors of various embodiments and comparative examples

[0058]

[0059]

[0060] The gel polymer sodium ion batteries prepared in Examples 1 to 9 and Comparative Examples 1 to 3 were tested for high temperature storage internal resistance change rate and high rate cycle performance, respectively. The test conditions are as follows. The test results are shown in Table 2.

[0061] (1) High temperature storage internal resistance change rate test

[0062] The sodium ion battery was subjected to five charge and discharge cycle tests at room temperature at a charge and discharge rate of 0.5C, and finally charged to a fully charged state at a rate of 1C, and the internal resistance T0 of the sodium ion battery was recorded. The fully charged battery was stored at 60°C for 15 days, and the internal resistance T of the sodium ion battery was recorded. The experimental data such as the battery internal resistance change rate were calculated, and the recorded results are shown in Table 2.

[0063] Internal resistance change rate = (T-T0) / T*100%

[0064] (2) Cyclic performance test

[0065] The sodium ion battery was charged at 45°C at a constant current of 0.5C to 4.2V, then charged at a constant voltage until the current dropped to 0.05C, and then discharged at a constant current of 0.5C to 1.5V. This cycle was repeated, and the discharge capacity of the first cycle and the discharge capacity of the last cycle were recorded. The capacity retention rate was calculated according to the following formula.

[0066] Capacity retention rate = (discharge capacity of the last cycle / discharge capacity of the first cycle) × 100%

[0067] Table 2 Performance of sodium ion batteries in various embodiments and comparative examples

[0068]

[0069]

[0070] As can be seen from the results in Table 2, the performance of Examples 1 to 9 is better than that of Comparative Examples 1 to 3. This may be because the present invention uses black phosphorus quantum dots dispersed in gel polymers. Black phosphorus quantum dots are zero-dimensional materials. Compared with two-dimensional materials such as black phosphorus nanosheets, their quantum effects are stronger and easier to disperse in gel polymers to form a stable system. Therefore, they are relatively stable during the storage of gel electrolytes. Black phosphorus itself has a high carrier mobility. It is attached to the surface of the positive and negative electrodes, which can reduce the impedance during the cycle. During the battery cycle, the black phosphorus quantum dots decompose and form fluorinated phosphides in situ. The impedance of the SEI and CEI films formed is also low, which can improve the high-rate performance of sodium ion batteries. In addition, black phosphorus quantum dots can improve the ionic conductivity of polymers to make up for the defect of low ionic conductivity of polymers as electrolytes. At the same time, the electrolyte of the present invention uses an in-situ cured gel electrolyte, which can improve the contact between the positive electrode and the isolation membrane interface and the negative electrode and the isolation membrane interface, inhibit the growth of sodium dendrites, and adsorb liquid electrolytes (lithium salts, etc.) in gel electrolysis, reduce free electrolytes, and improve the safety performance of batteries.

[0071] Comparative Example 1 does not contain black phosphorus quantum dots, and its impedance is high and its rate performance is poor. In Comparative Example 2, the solid electrolyte without non-aqueous organic solvents such as carbonate has low ionic conductivity and large polarization during charge and discharge, resulting in decreased battery performance. Comparative Example 3 uses black phosphorus nanosheets, which lack quantum effects and are poorly dispersed in the gel polymer, limiting the improvement in battery performance.

[0072] By comparing Examples 1 and 6 to 7, it can be seen that with the increase of the content of black phosphorus quantum dots, the high-temperature storage performance and the cycle performance are improved, but the degree of improvement gradually decreases.

[0073] From the comparison of Examples 1 to 5, it can be seen that the content of the cross-linking agent should not be too high, otherwise the content of the ethylene glycol units contained therein will increase, which will reduce the oxidation resistance of the electrolyte and be detrimental to the high temperature performance of the battery.

[0074] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention is described in detail with reference to the preferred embodiments, it is not limited to those listed in the embodiments. Those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A method for preparing a gel polymer sodium ion battery, characterized in that: Includes steps: (1) preparing a positive electrode sheet; (2) preparing a negative electrode sheet; (3) mixing sodium salt, non-aqueous organic solvent, monomer, cross-linking agent, initiator and black phosphorus quantum dots to obtain a gel electrolyte precursor; (4) using an isolation film to separate the positive electrode sheet and the negative electrode sheet, assembling them into a bare cell and then packaging them, pouring the gel electrolyte precursor and sealing them to form a cell; (5) Curing and post-processing the battery cell.

2. The method for preparing a gel polymer sodium ion battery according to claim 1, characterized in that: The positive electrode active material, positive electrode conductive agent and positive electrode binder are mixed to form positive electrode slurry, which is then coated on aluminum foil, dried and rolled to obtain the positive electrode sheet. The negative electrode active material, negative electrode conductive agent and negative electrode binder are mixed to form negative electrode slurry, which is then coated on copper foil, dried and rolled to obtain the negative electrode sheet.

3. The method for preparing a gel polymer sodium ion battery according to claim 1, characterized in that: The sodium salt includes at least one of sodium hexafluorophosphate, sodium difluorooxalatoborate, sodium tetrafluoroborate, sodium bisoxalatoborate, sodium perchlorate, sodium hexafluoroarsenate, sodium bis(fluorosulfonyl)imide, sodium trifluoromethylsulfonate and sodium bis(trifluoromethylsulfonyl)imide, and the non-aqueous organic solvent includes at least one of a carbonate organic solvent, a carboxylate organic solvent and an ether organic solvent.

4. The method for preparing a gel polymer sodium ion battery according to claim 1, characterized in that: The monomer includes at least one of methyl methacrylate, methyl acrylate and triacrylate of phosphate.

5. The method for preparing a gel polymer sodium ion battery according to claim 1, characterized in that: The crosslinking agent includes at least one of ethylene glycol dimethacrylate, pentaerythritol tetraacrylate and pentaerythritol triacrylate.

6. The method for preparing a gel polymer sodium ion battery according to claim 1, characterized in that: The initiator includes one or more of azobisisoheptanenitrile, azobisisobutyronitrile, azobisisobutyramidine hydrochloride, azobisisobutylimidazoline hydrochloride, benzoyl peroxide, potassium persulfate, ammonium persulfate, tert-butyl benzoyl peroxide and methyl ethyl ketone peroxide.

7. The method for preparing a gel polymer sodium ion battery according to claim 1, characterized in that: The black phosphorus quantum dots can be prepared by ball-milling blocky black phosphorus in a solvent to obtain a black scale dispersion, and then performing ultrasonication, centrifugation and drying.

8. The method for preparing a gel polymer sodium ion battery according to claim 1, characterized in that: The particle size of the black phosphorus quantum dots is 3-20 nm, and the black phosphorus quantum dots account for 0.005-0.200% of the total mass of the monomer and the cross-linking agent.

9. The method for preparing a gel polymer sodium ion battery according to claim 1, characterized in that: The curing conditions are a temperature of 40 to 70° C. and a time of 4 to 24 hours, and the post-treatment includes volume separation.

10. The gel polymer sodium ion battery prepared by the method for preparing a gel polymer sodium ion battery according to any one of claims 1 to 9, characterized in that: The invention comprises a positive electrode active material, a negative electrode active material and a gel electrolyte, wherein the gel electrolyte comprises a gel polymer, a sodium salt and black phosphorus quantum dots, and the gel polymer accounts for 3-90% of the mass of the gel electrolyte.