Preparation method of gel-state polymer sodium ion battery and sodium ion battery

By adsorbing black phosphorus quantum dots into the porous PMMA membrane, forming gel electrolytes, the problems of poor dispersion and insufficient performance in the battery are solved, the high-rate performance and cycling performance of sodium ion batteries are improved, and the more Highly efficient battery performance.

CN119009098APending Publication Date: 2024-11-22ZHUHAI SMOOTHWAY ELECTRONICS MATERIALS
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411158818.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

When black phosphorus is used as an auxiliary material for negative electrodes in chemical power supplies, it is difficult to exert its photoelectric and photothermal properties, and its dispersion in the battery is limited, resulting in a large difference in battery performance from commercial batteries and poor quantum effects.

Method used

Using the preparation method of gel polymer sodium ion battery, black phosphorus quantum dots are mixed in liquid electrolyte and adsorbed in PMMA porous membrane to form gel electrolyte to reduce the loss and oxidation of black phosphorus quantum dots Risk, increase its effective component ratio and dispersion in the battery, and reduce impedance during battery circulation.

Benefits of technology

It improves the high-rate performance and cycling performance of sodium ion batteries, reduces the impedance and safety risks of the battery, enhances the quantum effect of black phosphorus quantum dots, and makes up for the low ionic conductivity defect of polymer electrolyte.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005005847640000092
    Figure BDA0005005847640000092
  • Figure BDA0005005847640000121
    Figure BDA0005005847640000121
Patent Text Reader

Abstract

The invention provides a preparation method of a gel-state polymer sodium-ion battery and the sodium-ion battery. The preparation method comprises the following steps: preparing a positive plate; preparing a negative plate; mixing a sodium salt, a non-aqueous organic solvent and the black phosphorus quantum dots to obtain a liquid electrolyte; the preparation method comprises the following steps: preparing a membrane casting solution containing polymethyl methacrylate, a pore-foaming agent and a solvent, pouring, sequentially removing the solvent, soaking in a coagulating bath to remove the pore-foaming agent, and removing the coagulating bath to obtain a PMMA porous membrane; and separating the positive plate and the negative plate at intervals by adopting a PMMA (Polymethyl Methacrylate) porous membrane, assembling the positive plate and the negative plate into a naked battery cell, packaging the naked battery cell, filling the liquid electrolyte, sealing and forming to obtain the gel-state polymer sodium ion battery. According to the preparation method of the gel-state polymer sodium ion battery, the effect of the black phosphorus in the battery can be effectively exerted, and the impedance of the battery in the cycle process can be reduced, so that the high-rate performance of the sodium ion battery is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of new energy batteries, in particular to solid-state batteries, and more particularly to a preparation method of a gel polymer sodium ion battery and a sodium ion battery. Background Art

[0002] Black phosphorus is a new type of direct bandgap two-dimensional material. Its bandgap can be adjusted from 0.3eV (bulk state) to 1.5eV (monolayer) by the number of layers. Therefore, it can absorb light with wavelengths ranging from visible light to infrared for communication. In addition, its high carrier mobility (up to 1000cm when the thickness is 10nm) 2 ˙v -1 ˙s -1 ) and a higher on-off ratio (104), which shows great potential advantages in the fields of semiconductors, optoelectronics, and photothermal energy.

[0003] Attempts to use black phosphorus in chemical power sources include using it as an auxiliary negative electrode material to improve the energy density of lithium batteries. In practical applications, black phosphorus needs to be stripped into single-layer, few-layer or multi-layer black phosphorus (i.e., phosphorene) to exert its excellent photoelectric and photothermal properties. However, when used in the negative electrode, it is difficult to exert the effect of black phosphorus because black phosphorus exists in the negative electrode. Some researchers have tried to use black phosphorus in the electrolyte of chemical power sources, mixing black phosphorus nanosheets and liquid electrolytes into methyl methacrylate monomers for polymerization to obtain a black phosphorus nanosheet polymer composite film, and then using this composite film and the electrode to assemble into a button battery. Although this method based on the electrode can better exert the effect of black phosphorus, the performance of the battery itself is quite different from that of commercial batteries. However, even if the composite film is used to assemble a commercial battery, the dispersion of black phosphorus nanosheets in the battery is limited, and its quantum effect is not well exerted. Summary of the invention

[0004] Based on the above problems, the object of the present invention is to provide a method for preparing a gel polymer sodium ion battery and a sodium ion battery, which can effectively exert the effect of black phosphorus in the battery, reduce the impedance of the battery during the cycle process, and effectively improve the high-rate performance of the sodium ion battery.

[0005] To achieve the above object, the present invention provides a method for preparing a gel polymer sodium ion battery, comprising the steps of:

[0006] (1) preparing a positive electrode sheet;

[0007] (2) preparing a negative electrode sheet;

[0008] (3) mixing sodium salt, non-aqueous organic solvent and black phosphorus quantum dots to obtain a liquid electrolyte;

[0009] (4) first preparing a casting solution comprising polymethyl methacrylate, a porogen and a solvent, and after casting, successively removing the solvent, removing the porogen by immersion in a coagulation bath, and removing the coagulation bath to obtain a PMMA porous membrane;

[0010] (5) The positive electrode sheet and the negative electrode sheet are separated by a PMMA porous membrane and assembled into a bare cell and then packaged, and the liquid electrolyte is poured into the cell and sealed to obtain a gel polymer sodium ion battery.

[0011] In the technical solution adopted by the present invention, black phosphorus quantum dots are first mixed in a liquid electrolyte, and then adsorbed in the pore structure of a PMMA porous membrane with the liquid electrolyte. Compared with the method of first preparing black phosphorus quantum dots into a gel electrolyte membrane and then assembling them into a battery, the loss of black phosphorus quantum dots in the preparation process is reduced, the oxidation risk of black phosphorus quantum dots is reduced, and the effective component ratio of black phosphorus in the gel electrolyte is increased. The cycle performance of the prepared battery is better and it is not easy to precipitate sodium. The present invention uses black phosphorus quantum dots to be dispersed in a PMMA porous membrane. Black phosphorus quantum dots are zero-dimensional materials. Compared with two-dimensional materials such as black phosphorus nanosheets, their quantum effects are stronger and they are easier to disperse in a PMMA porous membrane. Black phosphorus itself has a high carrier mobility. It is attached to the surface of the positive and negative electrodes, which can reduce the impedance during the cycle. During the battery cycle, the black phosphorus quantum dots decompose and form fluorinated phosphides in situ. The impedance of the formed SEI and CEI films is also low, which can improve the high rate performance of sodium ion batteries. In addition, black phosphorus quantum dots can improve the ionic conductivity of polymers to make up for the defect of low ionic conductivity of polymers as electrolytes. The present invention prepares polymethyl methacrylate and porogens into a casting solution first, and removes the solvent, porogen and coagulation bath in sequence after casting to obtain a PMMA porous membrane with a high liquid absorption rate. The PMMA porous membrane prepared by this phase inversion method can adsorb liquid electrolytes containing black phosphorus quantum dots, which can reduce the flow of liquid electrolytes and improve the safety of batteries. The PMMA porous membrane has a high liquid absorption rate and can also reduce the amount of liquid electrolyte used, thereby further improving the safety of sodium ion batteries.

[0012] As a technical solution of the present invention, the positive electrode active material, the positive electrode conductive agent and the positive electrode binder are mixed to form a positive electrode slurry, which is then coated on an aluminum foil, dried and rolled to obtain the positive electrode sheet.

[0013] As a technical solution of the present invention, the negative electrode active material, the negative electrode conductive agent and the negative electrode binder are mixed to form a negative electrode slurry, which is then coated on a copper foil, dried and rolled to obtain the negative electrode sheet.

[0014] As a technical solution of the present invention, the positive electrode active material includes α-NaFeO2, NaCoO2, Na 0.7 [Fe 0.7 Mn 0.3]O2、Na(Mn 0.25 Fe 0.25 Co 0.25 Ni 0.25 )O2, NaMnO2, Na 0.5 [Fe 1 / 2 Mn 1 / 2 ]O2、Na 0.67 [Fe 1 / 2 Mn 1 / 2 ]O2, Na[Ni 0.35 Fe 0.40 Mn 0.25 ]O2, Na[Ni 0.30 Fe 0.45 Mn 0.25 ]O2, Na[Ni 0.25 Fe 0.50 Mn 0.25 ]O2, Na[Ni 0.20 Fe 0.55 Mn 0.25 ]O2、Na 0.67 [Mn 0.60 Ni 0.15 Fe 0.25 ]O2、Na[Li 0.05 (Ni 0.25 Fe 0.25 Mn 0.5 ) 0.95 ]O2, Na2FePO4F, Na4Fe2(CN)6, NaNi 0.33 Fe 0.33 Mn 0.33 At least one of O2, NaFePO4, Na2FeP2O7, Na2MnPO4F, NaCoPO4, Na3V2(PO4)3, NaCrO2 and Na2Fe2(SO4)3.

[0015] As a technical solution of the present invention, the positive electrode conductive agent includes at least one of conductive carbon black, conductive graphite, carbon fiber, carbon nanotube and graphene.

[0016] As a technical solution of the present invention, the positive electrode binder includes polyvinylidene fluoride.

[0017] As a technical solution of the present invention, the negative electrode active material includes at least one negative electrode material selected from soft carbon, hard carbon, sodium titanate, MoS2, Fe2O3, Fe3O4, ZnS, Sb and SbSn.

[0018] As a technical solution of the present invention, the negative electrode conductive agent includes at least one of conductive carbon black, conductive graphite, carbon fiber, carbon nanotube and graphene.

[0019] As a technical solution of the present invention, the negative electrode binder includes sodium carboxymethyl cellulose and / or styrene-butadiene rubber.

[0020] As a technical solution of the present invention, the sodium salt includes at least one of sodium hexafluorophosphate, sodium difluorooxalatoborate, sodium tetrafluoroborate, sodium bisoxalatoborate, sodium perchlorate, sodium hexafluoroarsenate, sodium bis(fluorosulfonyl)imide, sodium trifluoromethylsulfonate and sodium bis(trifluoromethylsulfonyl)imide.

[0021] As a technical solution of the present invention, the non-aqueous organic solvent includes at least one of a carbonate organic solvent, a carboxylate organic solvent and an ether organic solvent.

[0022] As a technical solution of the present invention, the weight average molecular weight of the polymethyl methacrylate is 3000-150000, and the concentration of the polymethyl methacrylate in the casting solution is 10-20wt.%.

[0023] As a technical solution of the present invention, the concentration of the porogen in the casting solution is 40-75 wt.%, and the porogen includes at least one of white oil, polyethylene glycol and glycerol.

[0024] As a technical solution of the present invention, the solvent includes at least one of tetrahydrofuran, formamide, N,N-dimethylformamide, N,N-dimethylacetamide, 1,4-dioxane, 1,3-dioxolane, dimethyl sulfoxide, acetone, acetaldehyde, pyridine, ethyl acetate, dibutyl phthalate, dioxane and aromatic compounds.

[0025] As a technical solution of the present invention, the solvent is removed by heating and the heating temperature is 50-70°C, the coagulation bath includes at least one of dichloromethane, ethanol and water, the immersion treatment temperature is 10-25°C, and the coagulation bath is removed by heating and the heating temperature is 50-85°C.

[0026] As a technical solution of the present invention, the liquid absorption rate of the PMMA porous membrane is 200 to 450 wt.%.

[0027] As a technical solution of the present invention, the black phosphorus quantum dots can be prepared by ball-milling blocky black phosphorus in a solvent to obtain a black phosphorus dispersion, and then performing ultrasonication, centrifugation and drying.

[0028] As a technical solution of the present invention, the particle size of the black phosphorus quantum dots is 3 to 20 nm, and the black phosphorus quantum dots account for 0.005 to 0.200% of the mass of the polymethyl methacrylate.

[0029] On the other hand, the present invention provides a gel polymer sodium ion battery prepared by a preparation method of a gel polymer sodium ion battery, comprising a positive electrode active material, a negative electrode active material and a gel electrolyte, wherein the gel electrolyte comprises a PMMA porous membrane and a liquid electrolyte adsorbed in the pores of the PMMA porous membrane, wherein the liquid electrolyte comprises a sodium salt, a non-aqueous organic solvent and black phosphorus quantum dots. DETAILED DESCRIPTION

[0030] The gel polymer sodium ion battery of the present invention comprises a positive electrode active material, a negative electrode active material and a gel electrolyte. The gel electrolyte comprises a PMMA porous membrane and a liquid electrolyte adsorbed in the pores of the PMMA porous membrane, and the liquid electrolyte comprises a sodium salt, a non-aqueous organic solvent and black phosphorus quantum dots. The sodium salt, the non-aqueous organic solvent and the black phosphorus quantum dots are dispersed in the pores of the PMMA porous membrane. The liquid absorption rate of the PMMA porous membrane is 200 to 450wt.%, as an example, the liquid absorption rate can be but not limited to 200wt.%, 230wt.%, 250wt.%, 280wt.%, 300wt.%, 330wt.%, 350wt.%, 370wt.%, 400wt.%, 430wt.%, 450wt.%. The sodium salt includes at least one of sodium hexafluorophosphate, sodium difluorooxalatoborate, sodium tetrafluoroborate, sodium bisoxalatoborate, sodium perchlorate, sodium hexafluoroarsenate, sodium bis(fluorosulfonyl)imide, sodium trifluoromethylsulfonate and sodium bis(trifluoromethylsulfonyl)imide. The non-aqueous organic solvent is selected from at least one of a carbonate organic solvent, a carboxylate organic solvent and an ether organic solvent. Specifically, the non-aqueous solvent may be, but is not limited to, at least one of ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), pentylene carbonate, vinylene carbonate (VC), dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), propylene carbonate (PC), butyl acetate (n-Ba), γ-butyrolactone (γ-Bt), propyl propionate (n-PP), ethyl propionate (EP), ethyl butyrate (Eb), ethylene glycol dimethyl ether (DME), ethylene glycol diethyl ether (ECS), diethylene glycol dimethyl ether (DEGME), triethylene glycol dimethyl ether (TEGDME), tetraethylene glycol dimethyl ether (TEGDME), 1,3-dioxolane (DOL), tetrahydrofuran (THF), methyltetrahydrofuran (MTHF), diphenyl ether and crown ether (CE). The particle size of black phosphorus quantum dots is 3 to 20 nm. As an example, the particle size can be but is not limited to 3 nm, 5 nm, 7 nm, 9 nm, 11 nm, 13 nm, 15 nm, 17 nm, 19 nm, and 20 nm.

[0031] The preparation method of the gel polymer sodium ion battery of the present invention comprises the steps of:

[0032] (1) preparing a positive electrode sheet;

[0033] (2) preparing a negative electrode sheet;

[0034] (3) mixing sodium salt, non-aqueous organic solvent and black phosphorus quantum dots to obtain a liquid electrolyte;

[0035] (4) first preparing a casting solution comprising polymethyl methacrylate, a porogen and a solvent, and after casting, successively removing the solvent, removing the porogen by immersion in a coagulation bath, and removing the coagulation bath to obtain a PMMA porous membrane;

[0036] (5) The positive electrode sheet and the negative electrode sheet are separated by a PMMA porous membrane and assembled into a bare cell and then packaged, and the liquid electrolyte is poured into the cell and sealed to obtain a gel polymer sodium ion battery.

[0037] In step (1), the positive electrode active material, the positive electrode conductive agent and the positive electrode binder are mixed to form a positive electrode slurry, which is then coated on an aluminum foil, dried, and rolled to obtain a positive electrode sheet. The positive electrode sheet can be prepared using conventional processes. The positive electrode active materials include α-NaFeO2, NaCoO2, Na 0.7 [Fe 0.7 Mn 0.3 ]O2、Na(Mn 0.25 Fe 0.25 Co 0.25 Ni 0.25 )O2, NaMnO2, Na 0.5 [Fe 1 / 2Mn 1 / 2 ]O2、Na 0.67 [Fe 1 / 2 Mn 1 / 2 ]O2, Na[Ni 0.35 Fe 0.40 Mn 0.25 ]O2, Na[Ni 0.30 Fe 0.45 Mn 0.25 ]O2, Na[Ni 0.25 Fe 0.50 Mn 0.25 ]O2, Na[Ni 0.20 Fe 0.55 Mn 0.25 ]O2、Na 0.67 [Mn 0.60 Ni 0.15 Fe 0.25 ]O2、Na[Li 0.05 (Ni 0.25 Fe 0.25 Mn 0.5 ) 0.95 ]O2, Na2FePO4F, Na4Fe2(CN)6, NaNi0.33 Fe 0.33 Mn 0.33 At least one of O2, NaFePO4, Na2FeP2O7, Na2MnPO4F, NaCoPO4, Na3V2(PO4)3, NaCrO2 and Na2Fe2(SO4)3. The positive electrode active material includes not only the above materials but also the corresponding coating and doping materials. The positive electrode active material is preferably Na[Ni 0.35 Fe 0.40 Mn 0.25 ]O2, Na[Ni 0.30 Fe 0.45 Mn 0.25 ]O2, Na[Ni 0.25 Fe 0.50 Mn 0.25 ]O2, Na[Ni 0.20 Fe 0.55 Mn 0.25 ]O2、Na 0.67 [Mn 0.60 Ni 0.15 Fe 0.25 ]O2、NaNi 0.33 Fe 0.33 Mn 0.33 O2 and other nickel iron manganese sodium positive electrode materials (NaNMF). The positive electrode conductive agent includes at least one of conductive carbon black, conductive graphite, carbon fiber, carbon nanotubes and graphene. The positive electrode binder includes polyvinylidene fluoride. The positive electrode slurry is prepared using NMP as a solvent. The mass ratio of the positive electrode active material, the positive electrode conductive agent and the positive electrode binder can be 90-98:0.5-5.0:0.5-5.0.

[0038] In step (2), the negative electrode active material, the negative electrode conductive agent and the negative electrode binder are mixed to form a negative electrode slurry, which is then coated on a copper foil, dried and rolled to obtain a negative electrode sheet. The negative electrode sheet can be prepared by conventional processes. The negative electrode active material includes a negative electrode material selected from at least one of soft carbon, hard carbon, sodium titanate, MoS2, Fe2O3, Fe3O4, ZnS, Sb and SbSn. As an example, the negative electrode active material of the present invention is hard carbon. The negative electrode conductive agent includes at least one of conductive carbon black, conductive graphite, carbon fiber, carbon nanotubes and graphene. The negative electrode binder includes sodium carboxymethyl cellulose and / or styrene-butadiene rubber. The negative electrode slurry is prepared using NMP or water as a solvent. The mass ratio of the negative electrode active material, the negative electrode conductive agent and the negative electrode binder can be 95-99:0.5-3.0:0.5-3.0.

[0039] In step (3), the sodium salt is selected from at least one of sodium hexafluorophosphate (NaPF6), sodium difluorooxalate borate (NaDFOP), sodium tetrafluoroborate (NaBF4), sodium bis(oxalate borate) (NaBOB), sodium perchlorate (NaClO), sodium hexafluoroarsenate (NaAsF6), sodium bis(fluorosulfonyl) imide (NaFSI), sodium trifluoromethylsulfonate (NaCF3SO3) and sodium bis(trifluoromethylsulfonyl) imide (NaTFSI). As an example, the sodium salt is sodium hexafluorophosphate (NaPF6). In some embodiments, the sodium salt is a mixture of sodium dioxalate borate (NaDFOP) and sodium hexafluorophosphate (NaPF6). The mass percentage of the sodium salt in the liquid electrolyte is 8 to 20%, specifically but not limited to 8%, 10%, 12%, 14%, 15%, 16%, 18%, 20%, preferably 10% to 15%, and further preferably, the mass percentage of the sodium salt in the liquid electrolyte is 14%.

[0040] The non-aqueous solvent is selected from at least one of carbonate organic solvents, carboxylate organic solvents and ether organic solvents. Specifically, the non-aqueous solvent may be, but is not limited to, ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), pentylene carbonate, vinylene carbonate (VC), dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), propylene carbonate (PC), butyl acetate (n-Ba), γ-butyrolactone (γ-Bt), propyl propionate (n-PP), ethyl propionate (EP), ethyl butyrate (Eb), ethylene glycol dimethyl ether (DME), ethylene glycol diethyl ether (ECS), diethylene glycol dimethyl ether (DEGME), triethylene glycol dimethyl ether (TEGDME), tetraethylene glycol dimethyl ether (TEGDME), 1,3-dioxolane (DOL), tetrahydrofuran (THF), methyltetrahydrofuran (MTHF), diphenyl ether and crown ether (CE). The mass percentage of the non-aqueous solvent in the liquid electrolyte is 60-90%, and may be but is not limited to 60%, 65%, 70%, 72%, 74%, 75%, 76%, 78%, 80%, 82%, 84%, 86%, 88%, 90%, and is preferably 75-88%.

[0041] Black phosphorus quantum dots (BPQDs) can exhibit typical quantum size effects, and their optical, electrical and chemical properties will change due to the reduction in size. The particle size of the black phosphorus quantum dots of the present invention is 3 to 20 nm, preferably 5 to 15 nm, and more preferably 6 to 10 nm. As an example, the particle size of the black phosphorus quantum dots may be, but not limited to, 3 nm, 5 nm, 7 nm, 9 nm, 11 nm, 12 nm, 14 nm, 16 nm, 18 nm, and 20 nm. The mass percentage of black phosphorus quantum dots in polymethyl methacrylate is 0.005 to 0.200%, preferably 0.010% to 0.100%. As an example, the proportion of black phosphorus quantum dots may be, but not limited to, 0.005%, 0.010%, 0.020%, 0.040%, 0.080%, 0.100%, 0.120%, 0.140%, 0.160%, 0.180%, and 0.200%. Black phosphorus quantum dots are prepared by ball-milling block black phosphorus in a solvent to obtain a black phosphorus dispersion, and then ultrasonicating, centrifuging and drying. Wherein, the mass ratio of block black phosphorus to solvent is 1 to 3:1000. As an example, the mass ratio of block black phosphorus to solvent may be, but is not limited to, 1:1000, 2:1000, and 3:1000. The solvent is selected from N-methylpyrrolidone (NMP). Ball milling is specifically ball milling in a zirconium oxide ball mill for 3 to 5 hours. Ultrasound is specifically ultrasonicating in an ultrasonicator for 9 to 11 hours. Centrifugation is specifically carried out in a centrifuge. Drying is specifically freeze-drying the supernatant obtained after centrifugation, and freeze-drying can specifically be drying in a cold dryer.

[0042] In step (4), the weight average molecular weight of polymethyl methacrylate is 3000-150000, preferably 20000-100000, or 30000-90000, or 35000-80000, or 40000-70000. As an example, the weight average molecular weight of polymethyl methacrylate may be, but not limited to, 3000, 5000, 10000, 20000, 30000, 40000, 50000, 60000, 70000, 80000, 90000, 100000, 110000, 120000, 120000, 140000, 150000. When the weight average molecular weight is too low, the adhesion to the substrate during casting may be reduced and the obtained coating film tends to be hard and brittle. When the weight average molecular weight is too high, the time for dissolving and preparing the casting solution will be relatively long. Gel permeation chromatography (GPC) can be used to determine the weight average molecular weight of the resin during operation. The concentration of polymethyl methacrylate in the casting solution is 10-20wt.%. Methyl methacrylate serves as a polymer framework, and forms a gel electrolyte after adsorbing the electrolyte. Its content in the casting solution can control the pore structure and porosity in the porous structure of the polymer. Only 10wt.% of methyl methacrylate can obtain a porous polymer with a porosity of about 90%. As an example, the concentration can be, but is not limited to, 10wt.%, 11wt.%, 12wt.%, 13wt.%, 14wt.%, 15wt.%, 16wt.%, 17wt.%, 18wt.%, 19wt.%, 20wt.%. The concentration of the porogen in the casting solution is 40-75wt.%, and as an example, the concentration of the porogen can be, but is not limited to, 40wt.%, 45wt.%, 50wt.%, 55wt.%, 60wt.%, 65wt.%, 70wt.%, 75wt.%. The porogen includes at least one of white oil, polyethylene glycol and glycerol. The weight average molecular weight of polyethylene glycol is 400-1600, and as an example, it can be, but is not limited to, 400, 500, 600, 700, 800, 900, 1000, 1100, 1200, 1300, 1400, 1500, 1600. The solvent includes at least one of tetrahydrofuran, formamide, N,N-dimethylformamide, N,N-dimethylacetamide, 1,4-dioxane, 1,3-dioxolane, dimethyl sulfoxide, acetone, acetaldehyde, pyridine, ethyl acetate, dibutyl phthalate, dioxane and aromatic compounds. The coagulation bath includes at least one of dichloromethane, ethanol and water. The selection of the porogen and the coagulation bath is corresponding. The coagulation bath needs to select a substance that can dissolve the porogen. For example, when the porogen is white oil, the coagulation bath can be dichloromethane; when the porogen is polyethylene glycol, the coagulation bath can be water or a mixture of water and ethanol; when the porogen is glycerol, the coagulation bath can be ethanol or a mixture of ethanol and water.The solvent is removed by heating and the heating temperature is 50-70°C. As an example, the heating temperature can be but not limited to 50°C, 52°C, 54°C, 56°C, 58°C, 60°C, 62°C, 64°C, 66°C, 68°C, 70°C, and the heating temperature needs to be higher than the boiling point of the corresponding solvent. The temperature of the immersion treatment is 10-25°C. As an example, the immersion temperature can be but not limited to 10°C, 13°C, 15°C, 18°C, 20°C, 23°C, 25°C. The temperature of the immersion treatment needs to be moderate. If the temperature is high, the molecular diffusion of the porogen is faster, which can improve the preparation efficiency of the PMMA porous membrane and the residual porogen is lower. However, when the temperature is high, the volatilization degree of the coagulation bath is aggravated, and the production safety is reduced during industrialization. Of course, the temperature of the coagulation bath should not be too low, otherwise there will be more porogen residues, which will affect the electrochemical performance of the subsequent battery. The coagulation bath is removed by heating and the heating temperature is 50-85°C. As an example, the heating temperature can be but not limited to 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, 80°C, 85°C, and the heating temperature must not be lower than the boiling point of the corresponding coagulation bath. Polymethyl methacrylate and porogen are first prepared into a casting solution. After casting, the solvent, porogen and coagulation bath are removed in sequence to obtain a PMMA porous membrane with a high liquid absorption rate. The liquid absorption rate of this PMMA porous membrane is 200-450wt.%. As an example, the liquid absorption rate can be but not limited to 200wt.%, 250wt.%, 300wt.%, 350wt.%, 400wt.%, 450wt.%.

[0043] In order to better illustrate the purpose, technical scheme and beneficial effects of the present invention, the present invention will be further described below in conjunction with specific embodiments. It should be noted that the following implementation method is a further explanation of the present invention and should not be used as a limitation of the present invention.

[0044] Part I: Preparation of PMMA porous membrane

[0045] Example 1

[0046] Take 10g of polymethyl methacrylate (weight average molecular weight of 40000), dissolve it in 20g of N,N-dimethylformamide, heat it to 60℃ and stir the solution until it is transparent, then add 20g of white oil and stir for 30min to make a casting solution. Pour the casting solution on a clean glass plate with a thickness of about 200μm, then put it into a 60℃ oven and heat it for 12h to evaporate most of the N,N-dimethylformamide. Then soak it in a 20℃ dichloromethane coagulation bath for 6h to remove the white oil and residual N,N-dimethylformamide. Then heat it at 60℃ to evaporate the dichloromethane to obtain a dry PMMA porous membrane for standby use.

[0047] The preparation parameters of the PMMA porous membranes in Examples 1 to 7 are shown in Table 1, and the rest of Examples 2 to 7 are the same as Example 1. The PMMA porous membranes in Examples 1 to 7 were tested for liquid absorption rate. The test method is as follows, and the test results are shown in Table 1.

[0048] Liquid absorption test: Take about 5g of PMMA porous membrane, weigh its specific mass, record it as m0, immerse it in liquid electrolyte (this liquid electrolyte is the same as the liquid electrolyte in Example 8), wait for 5 minutes, wait for it to be fully infiltrated by the electrolyte, take it out with tweezers, wipe off the electrolyte on its surface with filter paper, weigh its weight, record it as m1.

[0049] Liquid absorption rate

[0050] Table 1 Preparation parameters of PMMA porous membranes in Examples 1 to 7

[0051]

[0052] From the results in Table 2, it can be seen that the molecular weight and concentration of PMMA and the treatment temperature of the coagulation bath have a great influence on the liquid absorption rate of the PMMA porous membrane.

[0053] Comparative Example 1

[0054] Ethylene carbonate (EC), diethyl carbonate (DEC) and ethyl methyl carbonate (EMC) were mixed in a mass ratio of 1:2:1 to obtain 76g of non-aqueous solvent, and then 8g of methyl methacrylate (MMA), 2g of ethylene glycol dimethacrylate (EDMA) and 0.02g of azobisisobutyronitrile (AIBN) were added, and then 0.02g of black phosphorus quantum dots (BPQDs) were added to obtain a mixed solution. 14g of sodium hexafluorophosphate was slowly added to the mixed solution, mixed evenly, and heated to 85°C to induce the self-polymerization of methyl methacrylate to form a viscous precursor solution. The precursor solution was poured into a clean silicone rubber sealed glass mold, and then quickly transferred to a vacuum drying oven and dried to obtain a PMMA film.

[0055] Among them, the preparation method of black phosphorus quantum dots is: put 200 mg of block black phosphorus and 100 ml of NMP into a zirconia ball mill, and obtain a black phosphorus dispersion after ball milling for 4 hours; put the black phosphorus dispersion into a PP centrifuge tube, ultrasonicate it with an ultrasonicator for 10 hours, centrifuge it, and take the supernatant to obtain a black phosphorus quantum dot dispersion; dry the black phosphorus quantum dot dispersion in a freeze dryer to obtain black phosphorus quantum dots.

[0056] Part II: Preparation of the battery

[0057] Example 8

[0058] (1) Preparation of positive electrode sheet

[0059] The highest charging voltage is 4.2V. 0.33 Fe 0.33 Mn 0.33 O2, adhesive PVDF and conductive agent SuperP are evenly mixed in a mass ratio of 95:1:4 to form a positive electrode slurry with a certain viscosity. The mixed positive electrode slurry is coated on both sides of an aluminum foil, and then dried and rolled to obtain a positive electrode sheet.

[0060] (2) Preparation of negative electrode

[0061] Hard carbon, conductive agent SuperP, and adhesive PVDF are prepared into negative electrode slurry in a mass ratio of 97:1:2, and mixed evenly. The mixed negative electrode slurry is coated on both sides of an aluminum foil, and then dried and rolled to obtain a negative electrode sheet.

[0062] (3) Preparation of liquid electrolyte

[0063] In a glove box filled with nitrogen (O2≤5ppm, H2O≤5ppm), ethylene carbonate (EC), diethyl carbonate (DEC) and ethyl methyl carbonate (EMC) were mixed in a mass ratio of 1:2:1 to obtain 76g of a mixed solution. The mixed solution was sealed and packaged and placed in a quick freezer (-4°C) for 2h before being taken out. In a glove box filled with nitrogen (O2≤5ppm, H2O≤5ppm), 14g of sodium hexafluorophosphate and 0.01g of black phosphorus quantum dots were slowly added to the mixed solution and mixed evenly to obtain a liquid electrolyte.

[0064] Among them, the preparation method of black phosphorus quantum dots is: put 200 mg of block black phosphorus and 100 ml of NMP into a zirconia ball mill, and obtain a black phosphorus dispersion after ball milling for 4 hours; put the black phosphorus dispersion into a PP centrifuge tube, ultrasonicate it with an ultrasonicator for 10 hours, centrifuge it, and take the supernatant to obtain a black phosphorus quantum dot dispersion; dry the black phosphorus quantum dot dispersion in a freeze dryer to obtain black phosphorus quantum dots.

[0065] (4) Preparation of sodium ion batteries

[0066] The positive electrode sheet and the negative electrode sheet were separated by the PMMA porous membrane of Example 1 and assembled into a bare cell and then packaged. The prepared liquid electrolyte was filled and subjected to formation and capacity separation steps to produce a sodium ion battery 1# with a capacity of 1000 mAh.

[0067] The PMMA porous membranes prepared in Examples 2 to 7 were used to replace the PMMA porous membranes in Example 8 to prepare sodium ion batteries 2# to 7#. 0.02g of black phosphorus quantum dots were used to replace 0.01g of black phosphorus quantum dots in Example 8 to prepare sodium ion battery 8#. 0.04g of black phosphorus quantum dots were used to replace 0.01g of black phosphorus quantum dots in Example 8 to prepare sodium ion battery 9#. On the basis of Example 8, no black phosphorus quantum dots were added to prepare sodium ion battery 10#. On the basis of Example 8, black phosphorus quantum dots were replaced with black phosphorus nanosheets to prepare sodium ion battery 11#.

[0068] Comparative Example 2

[0069] (1) Preparation of positive electrode sheet

[0070] The highest charging voltage is 4.2V. 0.33 Fe 0.33 Mn 0.33 O2, adhesive PVDF and conductive agent SuperP are evenly mixed in a mass ratio of 95:1:4 to form a positive electrode slurry with a certain viscosity. The mixed positive electrode slurry is coated on both sides of an aluminum foil, and then dried and rolled to obtain a positive electrode sheet.

[0071] (2) Preparation of negative electrode

[0072] Hard carbon, conductive agent SuperP, and adhesive PVDF are prepared into negative electrode slurry in a mass ratio of 97:1:2, and mixed evenly. The mixed negative electrode slurry is coated on both sides of an aluminum foil, and then dried and rolled to obtain a negative electrode sheet.

[0073] (3) Preparation of sodium ion batteries

[0074] The positive electrode sheet and the negative electrode sheet were separated by the PMMA porous membrane prepared in Comparative Example 1 and assembled into a bare cell, which was then packaged and sealed. After the formation and capacity division processes, a sodium ion battery 12# with a capacity of 1000mAh was manufactured.

[0075] The prepared sodium ion batteries 1# to 12# were subjected to high-temperature storage internal resistance change rate and high-rate room-temperature cycle performance tests, respectively. The test conditions are as follows and the test results are shown in Table 2.

[0076] (1) High temperature storage internal resistance change rate test

[0077] The sodium ion battery was subjected to five charge and discharge cycle tests at room temperature at a charge and discharge rate of 0.5C, and finally charged to a fully charged state at a rate of 1C, and the internal resistance T0 of the sodium ion battery was recorded. The fully charged battery was stored at 60°C for 15 days, and the internal resistance T of the sodium ion battery was recorded. The experimental data such as the battery internal resistance change rate were calculated, and the recorded results are shown in Table 2.

[0078] Internal resistance change rate = (T-T0) / T*100%

[0079] (2) Normal temperature cycle performance test

[0080] The sodium ion battery was charged at 25°C at a constant current of 0.5C to 4.0V, then charged at a constant voltage until the current dropped to 0.05C, and then discharged at a constant current of 0.5C to 1.5V. This cycle was repeated, and the discharge capacity of the first cycle and the discharge capacity of the last cycle were recorded. The capacity retention rate was calculated according to the following formula.

[0081] Capacity retention rate = (discharge capacity of the last cycle / discharge capacity of the first cycle) × 100%

[0082] Table 2 Performance of sodium ion batteries in various embodiments and comparative examples

[0083]

[0084] From the results in Table 2, it can be seen that the internal resistance change rate of sodium ion batteries 1#~9# is lower than that of sodium ion batteries 10#~12#, and the capacity retention rate at high rate is higher than that of sodium ion batteries 10#~12#. This is because the present invention first prepares a PMMA porous membrane with a higher liquid absorption rate, and then adsorbs a liquid electrolyte containing black phosphorus quantum dots. The black phosphorus quantum dots dispersed in the battery can adhere to the positive and negative electrode surfaces due to their own high carrier mobility, which can reduce the impedance during the cycle process. During the battery cycle, the black phosphorus quantum dots decompose and form fluorophosphide in situ. The impedance of the formed SEI and CEI films is also low, thereby improving the high rate performance of the sodium ion battery.

[0085] From the comparison between sodium ion battery 1# and sodium ion batteries 8#~9#, it can be seen that with the increase of black phosphorus quantum dot content, the comprehensive performance of sodium ion battery is better.

[0086] Black phosphorus quantum dots were not added to sodium ion battery 10#, so its impedance was high and its rate performance was poor. Sodium ion battery 11# used black phosphorus nanosheets, which lacked quantum effects and were poorly dispersed in gel polymers, limiting the improvement in battery performance. Sodium ion battery 12# polymerized sodium salt, organic solvent, black phosphorus quantum dots and MMA monomers to obtain a gel electrolyte membrane, that is, the gel electrolyte membrane was first prepared and then the sodium ion battery was prepared. This method caused the battery's cycle performance to decay relatively quickly.

[0087] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention is described in detail with reference to the preferred embodiments, it is not limited to those listed in the embodiments. Those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A method for preparing a gel polymer sodium ion battery, characterized in that: Includes steps: (1) preparing a positive electrode sheet; (2) preparing a negative electrode sheet; (3) mixing sodium salt, non-aqueous organic solvent and black phosphorus quantum dots to obtain a liquid electrolyte; (4) first preparing a casting solution comprising polymethyl methacrylate, a porogen and a solvent, and after casting, successively removing the solvent, removing the porogen by immersion in a coagulation bath, and removing the coagulation bath to obtain a PMMA porous membrane; (5) The positive electrode sheet and the negative electrode sheet are separated by a PMMA porous membrane and assembled into a bare cell and then packaged, and the liquid electrolyte is poured into the cell and sealed to obtain a gel polymer sodium ion battery.

2. The method for preparing a gel polymer sodium ion battery according to claim 1, characterized in that: The positive electrode active material, positive electrode conductive agent and positive electrode binder are mixed to form positive electrode slurry, which is then coated on aluminum foil, dried and rolled to obtain the positive electrode sheet. The negative electrode active material, negative electrode conductive agent and negative electrode binder are mixed to form negative electrode slurry, which is then coated on copper foil, dried and rolled to obtain the negative electrode sheet.

3. The method for preparing a gel polymer sodium ion battery according to claim 1, characterized in that: The sodium salt includes at least one of sodium hexafluorophosphate, sodium difluorooxalatoborate, sodium tetrafluoroborate, sodium bisoxalatoborate, sodium perchlorate, sodium hexafluoroarsenate, sodium bis(fluorosulfonyl)imide, sodium trifluoromethylsulfonate and sodium bis(trifluoromethylsulfonyl)imide, and the non-aqueous organic solvent includes at least one of a carbonate organic solvent, a carboxylate organic solvent and an ether organic solvent.

4. The method for preparing a gel polymer sodium ion battery according to claim 1, characterized in that: The weight average molecular weight of the polymethyl methacrylate is 3000-150000, and the concentration of the polymethyl methacrylate in the casting solution is 10-20 wt.%.

5. The method for preparing a gel polymer sodium ion battery according to claim 1, characterized in that: The concentration of the porogen in the casting solution is 40-75 wt.%, and the porogen includes at least one of white oil, polyethylene glycol and glycerol.

6. The method for preparing a gel polymer sodium ion battery according to claim 1, characterized in that: The solvent includes at least one of tetrahydrofuran, formamide, N,N-dimethylformamide, N,N-dimethylacetamide, 1,4-dioxane, 1,3-dioxolane, dimethyl sulfoxide, acetone, acetaldehyde, pyridine, ethyl acetate, dibutyl phthalate, dioxane and aromatic compounds.

7. The method for preparing a gel polymer sodium ion battery according to claim 1, characterized in that: The solvent is removed by heating at a temperature of 50 to 70°C, the coagulation bath comprises at least one of dichloromethane, ethanol and water, the immersion treatment temperature is 10 to 25°C, and the coagulation bath is removed by heating at a temperature of 50 to 85°C.

8. The method for preparing a gel polymer sodium ion battery according to claim 1, characterized in that: The liquid absorption rate of the PMMA porous membrane is 200 to 450 wt.%.

9. The method for preparing a gel polymer sodium ion battery according to claim 1, characterized in that: The particle size of the black phosphorus quantum dots is 3-20nm, and the black phosphorus quantum dots account for 0.005-0.200% of the mass of the polymethyl methacrylate. The black phosphorus quantum dots can be prepared by ball-milling blocky black phosphorus in a solvent to obtain a black phosphorus dispersion, and then performing ultrasound, centrifugation and drying.

10. The gel polymer sodium ion battery prepared by the method for preparing a gel polymer sodium ion battery according to any one of claims 1 to 9, characterized in that: The invention comprises a positive electrode active material, a negative electrode active material and a gel electrolyte, wherein the gel electrolyte comprises a PMMA porous membrane and a liquid electrolyte adsorbed in the pores of the PMMA porous membrane, and the liquid electrolyte comprises a sodium salt, a non-aqueous organic solvent and black phosphorus quantum dots.

Citation Information

Cited By

  • High-temperature polymer lithium ion battery and preparation method thereof

    CN122638597A