Preparation method of gel-state polymer sodium ion battery and sodium ion battery
By using PMMA-black phosphorus quantum dot composite porous membrane in sodium ion batteries, the problems of poor dispersion and high interface impedance in sodium ion batteries are solved, and the high rate performance and cycle stability of the battery are improved sex.
Patent Information
- Application Number
- CN202411158820.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-22
AI Technical Summary
In the application of black phosphorus in sodium ion batteries, due to poor dispersion and high interface impedance, its quantum effect is poor, affecting the high rate performance and cycle stability of the battery.
The PMMA-black phosphorus quantum dot composite porous membrane is used as the gel electrolyte of the battery. By adsorbing liquid electrolyte in the membrane, the interface impedance is reduced and the cycling performance of the battery is improved.
It effectively improves the high-rate performance and cycle stability of sodium ion batteries, reduces the impedance of the battery during the cycle, and enhances the safety of the battery.
Smart Images

Figure BDA0005005847960000101 
Figure BDA0005005847960000131
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of new energy batteries, in particular to solid-state batteries, and more particularly to a preparation method of a gel polymer sodium ion battery and a sodium ion battery. Background Art
[0002] Black phosphorus is a new type of direct bandgap two-dimensional material. Its bandgap can be adjusted from 0.3eV (bulk state) to 1.5eV (monolayer) by the number of layers. Therefore, it can absorb light with wavelengths ranging from visible light to infrared for communication. In addition, its high carrier mobility (up to 1000cm when the thickness is 10nm) 2 ˙v -1 ˙s -1 ) and a higher on-off ratio (104), which shows great potential advantages in the fields of semiconductors, optoelectronics, and photothermal energy.
[0003] Attempts to use black phosphorus in chemical power sources include using it as an auxiliary negative electrode material to improve the energy density of lithium batteries. In practical applications, black phosphorus needs to be stripped into single-layer, few-layer or multi-layer black phosphorus (i.e., phosphorene) to exert its excellent photoelectric and photothermal properties. However, when used in the negative electrode, it is difficult to exert the effect of black phosphorus because black phosphorus exists in the negative electrode. Some researchers have tried to use black phosphorus in the electrolyte of chemical power sources, mixing black phosphorus nanosheets and liquid electrolytes into methyl methacrylate monomers for polymerization to obtain a black phosphorus nanosheet polymer composite film, and then using this composite film and the electrode to assemble into a button battery. Although this method based on the electrode can better exert the effect of black phosphorus, the performance of the battery itself is quite different from that of commercial batteries. However, even if the composite film is used to assemble a commercial battery, the dispersion of black phosphorus nanosheets in the battery is limited, and its quantum effect is not well exerted. Summary of the invention
[0004] Based on the above problems, the object of the present invention is to provide a method for preparing a gel polymer sodium ion battery and a sodium ion battery, which can effectively exert the effect of black phosphorus in the battery, reduce the impedance of the battery during the cycle process, and effectively improve the high-rate performance of the sodium ion battery.
[0005] To achieve the above object, the present invention provides a method for preparing a gel polymer sodium ion battery, comprising the steps of:
[0006] (1) preparing a positive electrode sheet;
[0007] (2) preparing a negative electrode sheet;
[0008] (3) preparing a liquid electrolyte;
[0009] (4) first preparing a casting solution comprising polymethyl methacrylate, a water-soluble porogen, black phosphorus quantum dots and an organic solvent, and after forming a thin layer, sequentially drying to remove the organic solvent, soaking in water to remove the water-soluble porogen, and baking to remove the water to obtain a PMMA-black phosphorus quantum dot composite porous membrane;
[0010] (5) The positive electrode sheet and the negative electrode sheet are separated by a PMMA-black phosphorus quantum dot composite porous membrane and assembled into a bare cell and then packaged, and the liquid electrolyte is poured into the cell and sealed to obtain a gel polymer sodium ion battery.
[0011] In the technical solution adopted by the present invention, the liquid electrolyte is adsorbed in the pore structure of the PMMA-black phosphorus quantum dot composite porous membrane. Compared with the method of first preparing the black phosphorus quantum dots and the liquid electrolyte into a gel electrolyte membrane and then assembling it into a battery, the interface impedance and interface integrity are better, the cycle performance of the obtained battery is better, and it is not easy to precipitate sodium. The black phosphorus quantum dots of the present invention are dispersed in the PMMA-black phosphorus quantum dot composite porous membrane. The black phosphorus quantum dots are zero-dimensional materials. Compared with two-dimensional materials such as black phosphorus nanosheets, their quantum effect is stronger and easier to disperse in the PMMA-black phosphorus quantum dot composite porous membrane. The high carrier mobility of black phosphorus itself is attached to the surface of the positive and negative electrodes, which can reduce the impedance during the cycle. During the battery cycle, the black phosphorus quantum dots decompose and form fluorinated phosphides in situ. The impedance of the formed SEI and CEI films is also low, which can improve the high rate performance of sodium ion batteries. In addition, black phosphorus quantum dots can improve the ionic conductivity of polymers to make up for the defect of low ionic conductivity of polymers as electrolytes. The present invention prepares polymethyl methacrylate, a water-soluble porogen and black phosphorus quantum dots into a casting solution first, and then removes the water-soluble porogen by washing with water to obtain a PMMA-black phosphorus quantum dot composite porous membrane with a high liquid absorption rate. The PMMA-black phosphorus quantum dot composite porous membrane can better absorb liquid electrolyte, reduce the flow of liquid electrolyte, and improve the safety of the battery.
[0012] As a technical solution of the present invention, the positive electrode active material, the positive electrode conductive agent and the positive electrode binder are mixed to form a positive electrode slurry, which is then coated on an aluminum foil, dried and rolled to obtain the positive electrode sheet.
[0013] As a technical solution of the present invention, the negative electrode active material, the negative electrode conductive agent and the negative electrode binder are mixed to form a negative electrode slurry, which is then coated on a copper foil, dried and rolled to obtain the negative electrode sheet.
[0014] As a technical solution of the present invention, the positive electrode active material includes α-NaFeO2, NaCoO2, Na 0.7 [Fe 0.7 Mn 0.3 ]O2、Na(Mn 0.25 Fe 0.25 Co0.25 Ni 0.25 )O2, NaMnO2, Na 0.5 [Fe 1 / 2 Mn 1 / 2 ]O2、Na 0.67 [Fe 1 / 2 Mn 1 / 2 ]O2, Na[Ni 0.35 Fe 0.40 Mn 0.25 ]O2, Na[Ni 0.30 Fe 0.45 Mn 0.25 ]O2, Na[Ni 0.25 Fe 0.50 Mn 0.25 ]O2, Na[Ni 0.20 Fe 0.55 Mn 0.25 ]O2、Na 0.67 [Mn 0.60 Ni 0.15 Fe 0.25 ]O2、Na[Li 0.05 (Ni 0.25 Fe 0.25 Mn 0.5 ) 0.95 ]O2, Na2FePO4F, Na4Fe2(CN)6, NaNi 0.33 Fe 0.33 Mn 0.33 At least one of O2, NaFePO4, Na2FeP2O7, Na2MnPO4F, NaCoPO4, Na3V2(PO4)3, NaCrO2 and Na2Fe2(SO4)3.
[0015] As a technical solution of the present invention, the positive electrode conductive agent includes at least one of conductive carbon black, conductive graphite, carbon fiber, carbon nanotube and graphene.
[0016] As a technical solution of the present invention, the positive electrode binder includes polyvinylidene fluoride.
[0017] As a technical solution of the present invention, the negative electrode active material includes at least one negative electrode material selected from soft carbon, hard carbon, sodium titanate, MoS2, Fe2O3, Fe3O4, ZnS, Sb and SbSn.
[0018] As a technical solution of the present invention, the negative electrode conductive agent includes at least one of conductive carbon black, conductive graphite, carbon fiber, carbon nanotube and graphene.
[0019] As a technical solution of the present invention, the negative electrode binder includes sodium carboxymethyl cellulose and / or styrene-butadiene rubber.
[0020] As a technical solution of the present invention, the sodium salt includes at least one of sodium hexafluorophosphate, sodium difluorooxalatoborate, sodium tetrafluoroborate, sodium bisoxalatoborate, sodium perchlorate, sodium hexafluoroarsenate, sodium bis(fluorosulfonyl)imide, sodium trifluoromethylsulfonate and sodium bis(trifluoromethylsulfonyl)imide.
[0021] As a technical solution of the present invention, the non-aqueous organic solvent includes at least one of a carbonate organic solvent, a carboxylate organic solvent and an ether organic solvent.
[0022] As a technical solution of the present invention, the weight average molecular weight of the polymethyl methacrylate is 3,000 to 150,000.
[0023] As a technical solution of the present invention, the mass ratio of the polymethyl methacrylate to the water-soluble porogen is 1:1-9.
[0024] As a technical solution of the present invention, the water-soluble porogen includes at least one of polyethylene glycol, polypropylene alcohol and polyacrylic acid, and the weight average molecular weight of the water-soluble porogen is 400-1600.
[0025] As a technical solution of the present invention, the solid content of the casting solution is 0.5-3.0%.
[0026] As a technical solution of the present invention, the thickness of the thin layer is 10 to 250 μm.
[0027] As a technical solution of the present invention, the organic solvent includes at least one of tetrahydrofuran, formamide, N,N-dimethylformamide, N,N-dimethylacetamide, 1,4-dioxane, 1,3-dioxolane, dimethyl sulfoxide, acetone, acetaldehyde, pyridine, ethyl acetate, dibutyl phthalate, dioxane and aromatic compounds.
[0028] As a technical solution of the present invention, the drying temperature is 40 to 60° C., and the drying time is 1 to 4 hours.
[0029] As a technical solution of the present invention, the baking temperature is 90-120° C., and the baking time is 20-36 hours.
[0030] As a technical solution of the present invention, the thickness of the PMMA-black phosphorus quantum dot composite porous membrane is 1 to 5 μm.
[0031] As a technical solution of the present invention, the porosity of the PMMA-black phosphorus quantum dot composite porous membrane is 70-85%.
[0032] As a technical solution of the present invention, the black phosphorus quantum dots can be prepared by ball-milling blocky black phosphorus in an organic solvent to obtain a black phosphorus dispersion, and then performing ultrasonication, centrifugation and drying.
[0033] As a technical solution of the present invention, the particle size of the black phosphorus quantum dots is 3 to 20 nm, and the black phosphorus quantum dots account for 0.005 to 0.200% of the mass of the liquid electrolyte.
[0034] On the other hand, the present invention provides a gel polymer sodium ion battery prepared by a preparation method of a gel polymer sodium ion battery, comprising a positive electrode active material, a negative electrode active material and a gel electrolyte, wherein the gel electrolyte comprises a PMMA-black phosphorus quantum dot composite porous membrane and a liquid electrolyte adsorbed in the pores of the PMMA-black phosphorus quantum dot composite porous membrane, wherein the liquid electrolyte comprises a sodium salt and a non-aqueous organic solvent. DETAILED DESCRIPTION
[0035] The gel polymer sodium ion battery of the present invention comprises a positive electrode active material, a negative electrode active material and a gel electrolyte. The gel electrolyte comprises a PMMA-black phosphorus quantum dot composite porous membrane and a liquid electrolyte adsorbed in the pores of the PMMA-black phosphorus quantum dot composite porous membrane, and the liquid electrolyte comprises a sodium salt and a non-aqueous organic solvent. The sodium salt and the non-aqueous organic solvent are dispersed in the pores of the PMMA-black phosphorus quantum dot composite porous membrane. The thickness of the PMMA-black phosphorus quantum dot composite porous membrane is 1 to 5 μm. As an example, the thickness can be but not limited to 1 μm, 2 μm, 3 μm, 4 μm, and 5 μm. The porosity of the PMMA-black phosphorus quantum dot composite porous membrane is 70 to 85%. As an example, the porosity can be but not limited to 70%, 73%, 75%, 78%, 80%, 82%, 84%, and 85%. The particle size of the black phosphorus quantum dots is 3 to 20 nm. As an example, the particle size can be, but is not limited to, 3 nm, 5 nm, 7 nm, 9 nm, 11 nm, 13 nm, 15 nm, 17 nm, 19 nm, and 20 nm. The sodium salt includes at least one of sodium hexafluorophosphate, sodium difluorooxalatoborate, sodium tetrafluoroborate, sodium bisoxalatoborate, sodium perchlorate, sodium hexafluoroarsenate, sodium bis(fluorosulfonyl)imide, sodium trifluoromethylsulfonate, and sodium bis(trifluoromethylsulfonyl)imide. The non-aqueous organic solvent is selected from at least one of a carbonate organic solvent, a carboxylate organic solvent, and an ether organic solvent. Specifically, the non-aqueous organic solvent may be, but is not limited to, at least one of ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), pentylene carbonate, vinylene carbonate (VC), dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), propylene carbonate (PC), butyl acetate (n-Ba), γ-butyrolactone (γ-Bt), propyl propionate (n-PP), ethyl propionate (EP), ethyl butyrate (Eb), ethylene glycol dimethyl ether (DME), ethylene glycol diethyl ether (ECS), diethylene glycol dimethyl ether (DEGME), triethylene glycol dimethyl ether (TEGDME), tetraethylene glycol dimethyl ether (TEGDME), 1,3-dioxolane (DOL), tetrahydrofuran (THF), methyltetrahydrofuran (MTHF), diphenyl ether and crown ether (CE).
[0036] The preparation method of the gel polymer sodium ion battery of the present invention comprises the steps of:
[0037] (1) preparing a positive electrode sheet;
[0038] (2) preparing a negative electrode sheet;
[0039] (3) preparing a liquid electrolyte;
[0040] (4) first preparing a casting solution comprising polymethyl methacrylate, a water-soluble porogen, black phosphorus quantum dots and an organic solvent, and after forming a thin layer, sequentially drying to remove the organic solvent, soaking in water to remove the water-soluble porogen, and baking to remove the water to obtain a PMMA-black phosphorus quantum dot composite porous membrane;
[0041] (5) The positive electrode sheet and the negative electrode sheet are separated by a PMMA-black phosphorus quantum dot composite porous membrane and assembled into a bare cell and then packaged, and the liquid electrolyte is poured into the cell and sealed to obtain a gel polymer sodium ion battery.
[0042] In step (1), the positive electrode active material, the positive electrode conductive agent and the positive electrode binder are mixed to form a positive electrode slurry, which is then coated on an aluminum foil, dried, and rolled to obtain a positive electrode sheet. The positive electrode sheet can be prepared using conventional processes. The positive electrode active materials include α-NaFeO2, NaCoO2, Na 0.7 [Fe 0.7 Mn 0.3 ]O2、Na(Mn 0.25 Fe 0.25 Co 0.25 Ni 0.25 )O2, NaMnO2, Na 0.5 [Fe 1 / 2Mn 1 / 2 ]O2、Na 0.67 [Fe 1 / 2 Mn 1 / 2 ]O2, Na[Ni 0.35 Fe 0.40 Mn 0.25 ]O2, Na[Ni 0.30 Fe 0.45 Mn 0.25 ]O2, Na[Ni 0.25 Fe 0.50 Mn 0.25 ]O2, Na[Ni 0.20 Fe 0.55 Mn 0.25 ]O2、Na 0.67 [Mn 0.60 Ni 0.15 Fe 0.25 ]O2、Na[Li 0.05 (Ni 0.25 Fe 0.25 Mn 0.5 ) 0.95 ]O2, Na2FePO4F, Na4Fe2(CN)6, NaNi 0.33 Fe 0.33 Mn 0.33At least one of O2, NaFePO4, Na2FeP2O7, Na2MnPO4F, NaCoPO4, Na3V2(PO4)3, NaCrO2 and Na2Fe2(SO4)3. The positive electrode active material includes not only the above materials but also the corresponding coating and doping materials. The positive electrode active material is preferably Na[Ni 0.35 Fe 0.40 Mn 0.25 ]O2, Na[Ni 0.30 Fe 0.45 Mn 0.25 ]O2, Na[Ni 0.25 Fe 0.50 Mn 0.25 ]O2, Na[Ni 0.20 Fe 0.55 Mn 0.25 ]O2、Na 0.67 [Mn 0.60 Ni 0.15 Fe 0.25 ]O2、NaNi 0.33 Fe 0.33 Mn 0.33 O2 and other nickel iron manganese sodium positive electrode materials (NaNMF). The positive electrode conductive agent includes at least one of conductive carbon black, conductive graphite, carbon fiber, carbon nanotubes and graphene. The positive electrode binder includes polyvinylidene fluoride. NMP is used as an organic solvent to prepare the positive electrode slurry. The mass ratio of the positive electrode active material, the positive electrode conductive agent and the positive electrode binder can be 90-98:0.5-5.0:0.5-5.0.
[0043] In step (2), the negative electrode active material, the negative electrode conductive agent and the negative electrode binder are mixed to form a negative electrode slurry, which is then coated on a copper foil, dried and rolled to obtain a negative electrode sheet. The negative electrode sheet can be prepared by conventional processes. The negative electrode active material includes a negative electrode material selected from at least one of soft carbon, hard carbon, sodium titanate, MoS2, Fe2O3, Fe3O4, ZnS, Sb and SbSn. As an example, the negative electrode active material of the present invention is hard carbon. The negative electrode conductive agent includes at least one of conductive carbon black, conductive graphite, carbon fiber, carbon nanotubes and graphene. The negative electrode binder includes sodium carboxymethyl cellulose and / or styrene-butadiene rubber. The negative electrode slurry is prepared using NMP or water as an organic solvent. The mass ratio of the negative electrode active material, the negative electrode conductive agent and the negative electrode binder can be 95-99:0.5-3.0:0.5-3.0.
[0044] In step (3), in a glove box filled with nitrogen, the non-aqueous organic solvent is sealed and packaged, frozen, and then taken out, and sodium salt is slowly added to the non-aqueous organic solvent and mixed evenly to obtain a liquid electrolyte.
[0045] The sodium salt is selected from at least one of sodium hexafluorophosphate (NaPF6), sodium difluorooxalate borate (NaDFOP), sodium tetrafluoroborate (NaBF4), sodium bisoxalate borate (NaBOB), sodium perchlorate (NaClO), sodium hexafluoroarsenate (NaAsF6), sodium bis(fluorosulfonyl)imide (NaFSI), sodium trifluoromethylsulfonate (NaCF3SO3) and sodium bis(trifluoromethylsulfonyl)imide (NaTFSI). As an example, the sodium salt is sodium hexafluorophosphate (NaPF6), and in some embodiments, the sodium salt is a mixture of sodium dioxalate borate (NaDFOP) and sodium hexafluorophosphate (NaPF6). The mass percentage of the sodium salt in the liquid electrolyte is 8 to 20%, specifically but not limited to 8%, 10%, 12%, 14%, 15%, 16%, 18%, 20%, preferably 10% to 15%, and further preferably, the mass percentage of the sodium salt in the liquid electrolyte is 14%.
[0046] The non-aqueous organic solvent is selected from at least one of carbonate organic solvents, carboxylate organic solvents and ether organic solvents. Specifically, the non-aqueous organic solvent may be, but is not limited to, ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), pentylene carbonate, vinylene carbonate (VC), dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), propylene carbonate (PC), butyl acetate (n-Ba), γ-butyrolactone (γ-Bt), propyl propionate (n-PP), ethyl propionate (EP), ethyl butyrate (Eb), ethylene glycol dimethyl ether (DME), ethylene glycol diethyl ether (ECS), diethylene glycol dimethyl ether (DEGME), triethylene glycol dimethyl ether (TEGDME), tetraethylene glycol dimethyl ether (TEGDME), 1,3-dioxolane (DOL), tetrahydrofuran (THF), methyltetrahydrofuran (MTHF), diphenyl ether and crown ether (CE). The mass percentage of the non-aqueous organic solvent in the liquid electrolyte is 60-90%, and may be but is not limited to 60%, 65%, 70%, 72%, 74%, 75%, 76%, 78%, 80%, 82%, 84%, 86%, 88%, 90%, and is preferably 75-88%.
[0047] In step (4), the weight average molecular weight of polymethyl methacrylate is 3000-150000, preferably 20000-100000, or 30000-90000, or 35000-80000, or 40000-70000. As an example, the weight average molecular weight of polymethyl methacrylate may be, but is not limited to, 3000, 5000, 10000, 20000, 30000, 40000, 50000, 60000, 70000, 80000, 90000, 100000, 110000, 120000, 120000, 140000, 150000. When the weight average molecular weight is too low, the adhesion to the substrate during casting may be reduced and the obtained coating film tends to be hard and brittle. When the weight average molecular weight is too high, the time for dissolving the casting solution will be longer. Gel permeation chromatography (GPC) can be used to determine the weight average molecular weight of the resin during operation.
[0048] The water-soluble porogen includes at least one of polyethylene glycol (PEG), polypropylene alcohol (PPG) and polyacrylic acid (PAA). The weight average molecular weight of the water-soluble porogen is 400 to 1600. As an example, the weight average molecular weight may be, but not limited to, 400, 600, 800, 1000, 1200, 1400, 1600. The weight average molecular weight of the water-soluble porogen should not be too low. A water-soluble porogen with a weight average molecular weight that is too small is in liquid form and is easily precipitated with solvent volatilization, making it difficult to form sufficient porosity. However, if the weight average molecular weight is too large, it is difficult to remove and will result in residues in the PMMA-black phosphorus quantum dot composite porous membrane.
[0049] The mass ratio of polymethyl methacrylate to the water-soluble porogen is 1:1-9. As an example, the mass ratio of the two can be but is not limited to 1:1, 1:2, 1:3, 1:4, 1:5, 1:6, 1:7, 1:8, 1:9.
[0050] Black phosphorus quantum dots (BPQDs) can exhibit typical quantum size effects, and their optical, electrical and chemical properties will change due to the reduction in size. The particle size of the black phosphorus quantum dots of the present invention is 3 to 20 nm, preferably 5 to 15 nm, and more preferably 6 to 10 nm. As an example, the particle size of the black phosphorus quantum dots may be, but not limited to, 3 nm, 5 nm, 7 nm, 9 nm, 11 nm, 12 nm, 14 nm, 16 nm, 18 nm, and 20 nm. The mass percentage of black phosphorus quantum dots in polymethyl methacrylate is 0.005 to 0.200%, preferably 0.010% to 0.100%. As an example, the proportion of black phosphorus quantum dots may be, but not limited to, 0.005%, 0.010%, 0.020%, 0.040%, 0.080%, 0.100%, 0.120%, 0.140%, 0.160%, 0.180%, and 0.200%. Black phosphorus quantum dots are prepared by ball-milling block black phosphorus in an organic solvent to obtain a black phosphorus dispersion, and then ultrasonicating, centrifuging and drying. Wherein, the mass ratio of block black phosphorus to organic solvent is 1 to 3:1000. As an example, the mass ratio of block black phosphorus to organic solvent may be, but is not limited to, 1:1000, 2:1000, 3:1000. The organic solvent is selected from N-methylpyrrolidone (NMP). Ball milling is specifically ball milling in a zirconium oxide ball mill for 3 to 5 hours. Ultrasound is specifically ultrasonicating in an ultrasonicator for 9 to 11 hours. Centrifugation is specifically carried out in a centrifuge. Drying is specifically freeze-drying the supernatant obtained after centrifugation, and freeze-drying can specifically be drying in a cold dryer.
[0051] The organic solvent includes at least one of tetrahydrofuran, formamide, N,N-dimethylformamide, N,N-dimethylacetamide, 1,4-dioxane, 1,3-dioxolane, dimethyl sulfoxide, acetone, acetaldehyde, pyridine, ethyl acetate, dibutyl phthalate, dioxane and aromatic compounds. The coagulation bath includes at least one of dichloromethane, ethanol and water.
[0052] The solid content of the casting solution is 0.5-3.0%. As an example, the solid content can be, but not limited to, 0.5%, 1.0%, 1.5%, 2.0%, 2.5%, and 3.0%. The thickness of the thin layer is 10-250 μm. As an example, the thickness can be, but not limited to, 10 μm, 50 μm, 100 μm, 150 μm, 200 μm, 230 μm, and 250 μm. The thin layer can be achieved by scraping, brushing, spraying, and the like. The drying temperature is 40-60°C. As an example, the drying temperature can be, but not limited to, 40°C, 42°C, 45°C, 48°C, 50°C, 53°C, 55°C, 58°C, and 60°C. The drying time is 1-4 hours. As an example, the drying time can be, but not limited to, 1 hour, 2 hours, 3 hours, and 4 hours. The immersion time in water depends on the actual situation, and at least all the porogens need to be leached out and removed. The baking temperature is 90-120° C., and as an example, the baking temperature may be, but not limited to, 90° C., 95° C., 100° C., 105° C., 110° C., 115° C., and 120° C. The baking time is 20-36 hours, and as an example, the baking time may be, but not limited to, 20 hours, 22 hours, 24 hours, 26 hours, 28 hours, 30 hours, 32 hours, 34 hours, and 36 hours.
[0053] In order to better illustrate the purpose, technical scheme and beneficial effects of the present invention, the present invention will be further described below in conjunction with specific embodiments. It should be noted that the following implementation method is a further explanation of the present invention and should not be used as a limitation of the present invention.
[0054] Part I: Preparation of PMMA-black phosphorus quantum dots composite porous membrane
[0055] Example 1
[0056] Take 10g of polymethyl methacrylate (PMMA, weight average molecular weight of 40000), 40g of polyethylene glycol (PEG, weight average molecular weight of 600) and 10mg of black phosphorus quantum dots and dissolve them in 1000mL of acetone, stir the solution until transparent, and obtain a casting solution with a solid content of 1%. Use a scraper to scrape the casting solution into a 100μm thick layer on a glass substrate, then put it in a 45℃ oven to dry for 2h to remove acetone, then soak it in water to remove polyethylene glycol, and finally put it in a 100℃ oven to bake for 24h to obtain a PMMA-black phosphorus quantum dot composite porous membrane.
[0057] Among them, the preparation method of black phosphorus quantum dots is: put 200 mg of block black phosphorus and 100 ml of NMP into a zirconia ball mill, and obtain a black phosphorus dispersion after ball milling for 4 hours; put the black phosphorus dispersion into a PP centrifuge tube, ultrasonicate it with an ultrasonicator for 10 hours, centrifuge it, and take the supernatant to obtain a black phosphorus quantum dot dispersion; dry the black phosphorus quantum dot dispersion in a freeze dryer to obtain black phosphorus quantum dots.
[0058] The preparation parameters of the PMMA-black phosphorus quantum dot composite porous membranes in Examples 1 to 13 are shown in Table 1, and the rest of Examples 2 to 13 are the same as Example 1. The PMMA-black phosphorus quantum dot composite porous membranes in Examples 1 to 13 were tested for thickness, porosity, liquid absorption and residual amount, and the test method is as follows, and the test results are shown in Table 1.
[0059] Among them, the thickness is measured by a thickness meter, and the porosity is detected by a porosity meter.
[0060] In addition, the liquid absorption rate test is as follows: take about 5g of PMMA-black phosphorus quantum dot composite porous membrane, weigh its specific mass, record it as m0, immerse it in a liquid electrolyte (this liquid electrolyte is the same as the liquid electrolyte in Example 14), wait for 5 minutes, wait for it to be fully infiltrated by the electrolyte, take it out with tweezers, wipe off the electrolyte on its surface with filter paper, weigh its weight, record it as m1.
[0061] Liquid absorption rate
[0062] Test for residual water-soluble porogen: Take about 5 g of dry PMMA-black phosphorus quantum dot composite porous membrane, accurately measure its weight and record it as m2, put it into a Soxhlet extractor, extract it with methanol for 24 hours, put it into a 45°C vacuum oven until constant weight, record its weight, and record it as m3.
[0063] Residual amount of aqueous porogen
[0064] Table 1 Preparation parameters of PMMA-black phosphorus quantum dot composite porous membrane in Examples 1 to 13
[0065]
[0066] From the results in Table 1, it can be seen that the molecular weight of the water-soluble porogen has a great influence on the performance of the PMMA-black phosphorus quantum dot composite porous membrane. When the weight average molecular weight is too small, the porosity of the composite porous membrane is small and the liquid absorption rate is low; when the weight average molecular weight is too large, it is difficult to remove and will remain in the PMMA-black phosphorus quantum dot composite porous membrane. The molecular weight of the water-soluble porogen is preferably 400-1600. When the water-soluble porogen is PEG, the performance of the PMMA-black phosphorus quantum dot composite porous membrane is better.
[0067] Comparative Example 1
[0068] Ethylene carbonate (EC), diethyl carbonate (DEC) and ethyl methyl carbonate (EMC) were mixed in a mass ratio of 1:2:1 to obtain 76g of non-aqueous organic solvent, and then 8g of methyl methacrylate (MMA), 2g of ethylene glycol dimethacrylate (EDMA) and 0.02g of azobisisobutyronitrile (AIBN) were added, and then 0.02g of black phosphorus quantum dots (BPQDs) were added to obtain a mixed solution. 14g of sodium hexafluorophosphate was slowly added to the mixed solution, mixed evenly, and heated to 85°C to induce the self-polymerization of methyl methacrylate to form a viscous precursor solution. The precursor solution was poured into a clean silicone rubber sealed glass mold, and then quickly transferred to a vacuum drying oven and dried to obtain a PMMA film.
[0069] Among them, the preparation method of black phosphorus quantum dots is: put 200 mg of block black phosphorus and 100 ml of NMP into a zirconia ball mill, and obtain a black phosphorus dispersion after ball milling for 4 hours; put the black phosphorus dispersion into a PP centrifuge tube, ultrasonicate it with an ultrasonicator for 10 hours, centrifuge it, and take the supernatant to obtain a black phosphorus quantum dot dispersion; dry the black phosphorus quantum dot dispersion in a freeze dryer to obtain black phosphorus quantum dots.
[0070] Part II: Preparation of the battery
[0071] Embodiment 14
[0072] (1) Preparation of positive electrode sheet
[0073] The highest charging voltage is 4.2V. 0.33 Fe 0.33 Mn 0.33 O2, adhesive PVDF and conductive agent SuperP are evenly mixed in a mass ratio of 95:1:4 to form a positive electrode slurry with a certain viscosity. The mixed positive electrode slurry is coated on both sides of an aluminum foil, and then dried and rolled to obtain a positive electrode sheet.
[0074] (2) Preparation of negative electrode
[0075] Hard carbon, conductive agent SuperP, and adhesive PVDF are prepared into negative electrode slurry in a mass ratio of 97:1:2, and mixed evenly. The mixed negative electrode slurry is coated on both sides of an aluminum foil, and then dried and rolled to obtain a negative electrode sheet.
[0076] (3) Preparation of liquid electrolyte
[0077] In a glove box filled with nitrogen (O2≤5ppm, H2O≤5ppm), ethylene carbonate (EC), diethyl carbonate (DEC) and ethyl methyl carbonate (EMC) were mixed in a mass ratio of 1:2:1 to obtain 76g of a mixed solution. The mixed solution was sealed and packaged and placed in a quick freezer (-4°C) for 2h before being taken out. In a glove box filled with nitrogen (O2≤5ppm, H2O≤5ppm), 14g of sodium hexafluorophosphate was slowly added to the mixed solution and mixed evenly to obtain a liquid electrolyte.
[0078] (4) Preparation of sodium ion batteries
[0079] The PMMA-black phosphorus quantum dot composite porous membrane of Example 1 is used to separate the positive electrode sheet and the negative electrode sheet and assemble them into bare cells for packaging. The prepared liquid electrolyte is filled in the cells and the formation and capacity separation steps are performed to produce a sodium ion battery 1# with a capacity of 2.5 mAh.
[0080] The PMMA-black phosphorus quantum dot composite porous membranes prepared in Examples 3 to 4 and 7 to 13 were used to replace the PMMA-black phosphorus quantum dot composite porous membranes in Example 14 to prepare sodium ion batteries 2# to 10#. Based on Example 14, black phosphorus quantum dots were not added to prepare sodium ion battery 11#. Based on Example 14, black phosphorus quantum dots were replaced with black phosphorus nanosheets to prepare sodium ion battery 12#.
[0081] Comparative Example 2
[0082] (1) Preparation of positive electrode sheet
[0083] The highest charging voltage is 4.2V. 0.33 Fe 0.33 Mn 0.33 O2, adhesive PVDF and conductive agent SuperP are evenly mixed in a mass ratio of 95:1:4 to form a positive electrode slurry with a certain viscosity. The mixed positive electrode slurry is coated on both sides of an aluminum foil, and then dried and rolled to obtain a positive electrode sheet.
[0084] (2) Preparation of negative electrode
[0085] Hard carbon, conductive agent SuperP, and adhesive PVDF are prepared into negative electrode slurry in a mass ratio of 97:1:2, and mixed evenly. The mixed negative electrode slurry is coated on both sides of an aluminum foil, and then dried and rolled to obtain a negative electrode sheet.
[0086] (3) Preparation of sodium ion batteries
[0087] The PMMA-black phosphorus quantum dot composite porous membrane prepared in Comparative Example 1 was used to separate the positive electrode sheet and the negative electrode sheet and assembled into a bare cell, which was then packaged and sealed. After the formation and capacity division processes, a sodium ion battery 13# with a capacity of 2.5 mAh was produced.
[0088] The prepared sodium ion batteries 1# to 13# were subjected to high-temperature storage internal resistance change rate and high-rate room-temperature cycle performance tests, respectively. The test conditions are as follows and the test results are shown in Table 2.
[0089] (1) High temperature storage internal resistance change rate test
[0090] The sodium ion battery was subjected to five charge and discharge cycle tests at room temperature at a charge and discharge rate of 0.5C, and finally charged to a fully charged state at a rate of 1C, and the internal resistance T0 of the sodium ion battery was recorded. The fully charged battery was stored at 45°C for 15 days, and the internal resistance T of the sodium ion battery was recorded. The experimental data such as the battery internal resistance change rate were calculated, and the recorded results are shown in Table 2.
[0091] Internal resistance change rate = (T-T0) / T*100%
[0092] (2) Normal temperature cycle performance test
[0093] The sodium ion battery was charged at 25°C at a constant current of 0.5C to 4.0V, then charged at a constant voltage until the current dropped to 0.05C, and then discharged at a constant current of 0.5C to 1.5V. This cycle was repeated, and the discharge capacity of the first cycle and the discharge capacity of the last cycle were recorded. The capacity retention rate was calculated according to the following formula.
[0094] Capacity retention rate = (discharge capacity of the last cycle / discharge capacity of the first cycle) × 100%
[0095] Table 2 Performance of sodium ion batteries in various embodiments and comparative examples
[0096]
[0097] From the results in Table 2, it can be seen that the internal resistance change rate of sodium ion batteries 1#~10# is lower than that of sodium ion batteries 11#~13#, and the capacity retention rate at high rate is higher than that of sodium ion batteries 11#~13#. This is because the present invention first prepares a PMMA-black phosphorus quantum dot composite porous membrane with a higher liquid absorption rate, and then adsorbs the liquid electrolyte. The black phosphorus quantum dots dispersed in the composite porous membrane can adhere to the positive and negative electrode surfaces due to their own high carrier mobility, which can reduce the impedance during the cycle process. During the battery cycle, the black phosphorus quantum dots decompose and form fluorophosphide in situ. The impedance of the formed SEI and CEI films is also low, thereby improving the high rate performance of the sodium ion battery.
[0098] Sodium ion battery 11# does not contain black phosphorus quantum dots, so its impedance is high and its rate performance is poor. Sodium ion battery 12# uses black phosphorus nanosheets, which lack quantum effects and are poorly dispersed in gel polymers, limiting the improvement of battery performance. Sodium ion battery 13# polymerizes sodium salt, organic solvent, black phosphorus quantum dots and MMA monomers together to obtain a gel electrolyte membrane, that is, the gel electrolyte membrane is first prepared and then the sodium ion battery is prepared. This method will result in high battery impedance and poor cycle.
[0099] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention is described in detail with reference to the preferred embodiments, it is not limited to those listed in the embodiments. Those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A method for preparing a gel polymer sodium ion battery, characterized in that: Includes steps: (1) preparing a positive electrode sheet; (2) preparing a negative electrode sheet; (3) preparing a liquid electrolyte; (4) first preparing a casting solution comprising polymethyl methacrylate, a water-soluble porogen, black phosphorus quantum dots and an organic solvent, and after forming a thin layer, sequentially drying to remove the organic solvent, soaking in water to remove the water-soluble porogen, and baking to remove the water to obtain a PMMA-black phosphorus quantum dot composite porous membrane; (5) The positive electrode sheet and the negative electrode sheet are separated by a PMMA-black phosphorus quantum dot composite porous membrane and assembled into a bare cell and then packaged, and the liquid electrolyte is poured into the cell and sealed to obtain a gel polymer sodium ion battery.
2. The method for preparing a gel polymer sodium ion battery according to claim 1, characterized in that: The positive electrode active material, positive electrode conductive agent and positive electrode binder are mixed to form positive electrode slurry, which is then coated on aluminum foil, dried and rolled to obtain the positive electrode sheet. The negative electrode active material, negative electrode conductive agent and negative electrode binder are mixed to form negative electrode slurry, which is then coated on copper foil, dried and rolled to obtain the negative electrode sheet.
3. The method for preparing a gel polymer sodium ion battery according to claim 1, characterized in that: The liquid electrolyte includes a sodium salt and a non-aqueous organic solvent, wherein the sodium salt includes at least one of sodium hexafluorophosphate, sodium difluorooxalatoborate, sodium tetrafluoroborate, sodium bisoxalatoborate, sodium perchlorate, sodium hexafluoroarsenate, sodium bis(fluorosulfonyl)imide, sodium trifluoromethylsulfonate and sodium bis(trifluoromethylsulfonyl)imide, and the non-aqueous organic solvent includes at least one of a carbonate organic solvent, a carboxylate organic solvent and an ether organic solvent.
4. The method for preparing a gel polymer sodium ion battery according to claim 1, characterized in that: The weight average molecular weight of the polymethyl methacrylate is 3000-150000, the mass ratio of the polymethyl methacrylate to the water-soluble porogen is 1:1-9, the water-soluble porogen includes at least one of polyethylene glycol, polypropylene alcohol and polyacrylic acid, and the weight average molecular weight of the water-soluble porogen is 400-1600.
5. The method for preparing a gel polymer sodium ion battery according to claim 1, characterized in that: The solid content of the casting solution is 0.5-3.0%, and the thickness of the thin layer is 10-250 μm.
6. The method for preparing a gel polymer sodium ion battery according to claim 1, characterized in that: The organic solvent includes at least one of tetrahydrofuran, formamide, N,N-dimethylformamide, N,N-dimethylacetamide, 1,4-dioxane, 1,3-dioxolane, dimethyl sulfoxide, acetone, acetaldehyde, pyridine, ethyl acetate, dibutyl phthalate, dioxane and aromatic compounds.
7. The method for preparing a gel polymer sodium ion battery according to claim 1, characterized in that: The drying temperature is 40-60° C., the drying time is 1-4 hours, the baking temperature is 90-120° C., and the baking time is 20-36 hours.
8. The method for preparing a gel polymer sodium ion battery according to claim 1, characterized in that: The thickness of the PMMA-black phosphorus quantum dot composite porous membrane is 1-5 μm, and the porosity of the PMMA-black phosphorus quantum dot composite porous membrane is 70-85%.
9. The method for preparing a gel polymer sodium ion battery according to claim 1, characterized in that: The particle size of the black phosphorus quantum dots is 3-20nm, and the black phosphorus quantum dots account for 0.005-0.200% of the mass of the polymethyl methacrylate. The black phosphorus quantum dots are obtained by ball-milling blocky black phosphorus in an organic solvent to obtain a black phosphorus dispersion, and then performing ultrasound, centrifugation and drying.
10. The gel polymer sodium ion battery prepared by the method for preparing a gel polymer sodium ion battery according to any one of claims 1 to 9, characterized in that: The invention comprises a positive electrode active material, a negative electrode active material and a gel electrolyte, wherein the gel electrolyte comprises a PMMA-black phosphorus quantum dot composite porous membrane and a liquid electrolyte adsorbed in the pores of the PMMA-black phosphorus quantum dot composite porous membrane, and the liquid electrolyte comprises a sodium salt and a non-aqueous organic solvent.