Lithium ion battery electrolyte and lithium ion battery
By using compound A with cyano structure and compound B with silicon-based structure in lithium-ion battery electrolyte, the alkalinity and oxidation problems of high-nickel positive electrode materials are solved, the high-temperature and low-temperature performance of lithium-ion batteries are improved, and the high-temperature and low-temperature performance of lithium-ion batteries is controlled. The internal resistance growth improves the safety and cycle stability of the battery.
Patent Information
- Application Number
- CN202411143796.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-22
AI Technical Summary
The use of high nickel positive electrode materials in lithium-ion batteries has problems such as high alkalinity, strong oxidation and poor thermal stability, which leads to poor electrochemical and safety performance, and increases internal resistance, affecting the endurance of lithium-ion batteries.
Using a lithium-ion battery electrolyte, including lithium salts, non-aqueous organic solvents and specific additives, Compound A and Compound B, the cyano structure in Compound A can complex transition metal cations, and Compound B can reduce by-product accumulation and protection. The integrity of the positive electrode material, combining silicon groups to improve high- and low-temperature performance.
It effectively improves the high-temperature circulation and low-temperature discharge performance of lithium-ion batteries, and controls the internal resistance growth during the high-temperature circulation, enhancing the safety and cycle stability of the battery.
Smart Images

Figure CN119009130A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of lithium ion batteries, and in particular relates to a lithium ion battery electrolyte and a lithium ion battery. Background Art
[0002] Lithium-ion batteries have broad application prospects in consumer electronics, power vehicle batteries and energy storage power supplies due to their high energy density, long cycle life and no pollution. With the development of the lithium-ion battery industry, people have put forward higher requirements for the endurance of lithium-ion batteries. In order to improve the energy density of lithium-ion batteries, developing lithium-ion battery positive electrode materials with high specific capacity is one of the effective ways.
[0003] At present, high-nickel cathode materials have become a hot topic of research due to their higher theoretical specific capacity than other cathode materials. However, the use of high-nickel cathode materials in batteries still faces many problems, mainly reflected in: (1) The high-nickel cathode materials have high alkalinity and will react chemically with some additives in the electrolyte to produce a large number of by-products. The by-products will not only occupy the active material space of the battery, but also block the micropores, affect the migration of lithium ions, and thus increase the internal resistance; (2) The high nickel content in high-nickel cathode materials makes them highly oxidizing, causing the electrolyte to easily undergo electrochemical oxidation reactions on the cathode surface, while causing changes in the structure of the high-nickel cathode materials, resulting in reduction reactions and dissolution of transition metal ions such as nickel and cobalt; (3) The thermal stability of high-nickel cathode materials is poor. The above problems will deteriorate the electrochemical performance and safety performance of lithium-ion batteries containing high-nickel cathode materials.
[0004] Therefore, there is an urgent need for a lithium ion battery electrolyte and a lithium ion battery to solve the deficiencies of the existing technical problems. Summary of the invention
[0005] In view of the above problems, the purpose of the present invention is to provide a lithium ion battery electrolyte and a lithium ion battery, which can not only improve the high temperature cycle performance and low temperature discharge performance of the lithium ion battery, but also effectively control the internal resistance growth during the high temperature cycle process.
[0006] To achieve the above objectives, the present invention provides a lithium ion battery electrolyte in a first aspect, comprising a lithium salt, a non-aqueous organic solvent and an additive, wherein the additive comprises a compound A and a compound B, wherein the structure of the compound A is as shown in Formula 1, the structure of the compound B is as shown in Formula 2 or Formula 3, and the mass percentage of the compound B in the lithium ion battery electrolyte is 0.05-1%.
[0007]
[0008] wherein R1 is selected from an alkyl group, an alkyl halide phenyl group, a diaryl alkyl group or an ester group, R2 to R4 are each independently selected from an alkyl group, an alkoxy group, an alkynyl group, an alkenyl group, a phenyl group or a halogen group, X is selected from N or O, R5 is selected from an alkyl group, and R 6~ R7 is independently selected from alkyl or phenyl, R8 is selected from alkyl, alkenyl, phenyl or norbornene, and m, n, p is independently selected from 0 or 1.
[0009] Compared with the prior art, the additive of the present invention comprises compound A and compound B, wherein the cyano structure in compound A can complex the transition metal cations dissolved in the positive electrode material of the lithium ion battery, and prevent the cations from entering the electrolyte to catalyze and intensify the decomposition and gas production of the electrolyte, thereby improving the safety performance of the battery, and the cyano structure has high oxidation stability to ensure the stability of the lithium ion battery in a high-voltage working environment, and the cyano structure is a highly polar functional group, which is conducive to the dissociation of lithium salts, thereby improving the cycle performance and low-temperature discharge performance of the lithium ion battery and reducing the internal resistance of the battery; however, the cyano structure has a low boiling point characteristic, which leads to the instability of the lithium ion battery in a high-temperature working environment, so a non-flammable and thermally stable silicon group is also introduced into compound A to improve the stability of the lithium ion battery in a high-temperature working environment, and the low-bond rotation of the silicon group can make it have a highly flexible skeleton and a lower glass transition temperature and a lower viscosity, so the silicon group can improve the high-temperature cycle of the lithium ion battery while improving its low-temperature discharge performance to a certain extent. In addition, compound B can not only significantly reduce the increase in internal resistance caused by the accumulation of byproducts during the battery charge and discharge cycle by reacting with the alkaline substances on the surface of the positive electrode material, but also protect the integrity of the positive electrode material to further improve the high temperature cycle and low temperature discharge performance of the lithium ion battery. Therefore, the present invention uses compound A and compound B as additives together, and utilizes the synergistic effect of the two, so that the lithium ion battery electrolyte can not only improve the high temperature cycle performance and low temperature discharge performance of the lithium ion battery, but also effectively control the internal resistance growth during the high temperature cycle.
[0010] Further, R1 of the present invention is selected from C1-C6 alkyl, C1-C4 alkyl halophenyl, diaryl C1-C4 alkyl or C2-C5 alkyl ester, R2-R4 are each independently selected from C1-C6 alkyl, C1-C6 alkoxy, C2-C6 alkenyl, phenyl or halogen, X is selected from N or O, R5 is selected from C1-C4 alkyl, R6-R7 are each independently selected from C1-C6 alkyl or phenyl, R8 is selected from C1-C4 alkyl, C2-C4 alkenyl, phenyl or norbornene. Specifically, the alkyl group can be straight chain, branched chain or cyclic, such as alkyl group can be but not limited to methyl, ethyl, propyl, isopropyl, butyl, sec-butyl, tert-butyl, pentyl and cyclohexyl, etc., more specifically, the hydrogen on the cyclic alkyl ring can also be substituted by an alkyl group. Specifically, the alkenyl group can be but not limited to vinyl, propenyl, butenyl, isobutenyl, etc. Specifically, C1~C6 alkoxy can be but not limited to methoxy, ethoxy, n-propoxy, isopropoxy, n-butoxy, sec-butoxy, tert-butoxy, pentyloxy or hexyloxy. Specifically, diaryl C1~C4 alkyl refers to two aryl groups (benzene ring or other aromatic ring) connected by a carbon chain, and the length of this carbon chain ranges from 1 to 4 carbon atoms. Alkyl halophenyl refers to the hydrogen atoms on the benzene ring being replaced by an alkyl chain and a halogen, respectively, such as the two hydrogen atoms on the benzene ring can be replaced by an ethyl group and a fluorine atom, respectively. Specifically, halogen includes but is not limited to fluorine (F), chlorine (Cl), bromine (Br), iodine (I), etc., preferably, the halogen is fluorine (F). It can be understood that R2, R3, and R4 can be the same or different, and are not limited here; at the same time, R6 and R7 can also be the same or different.
[0011] Furthermore, the compound A of the present invention is at least one selected from compounds 1 to 8:
[0012]
[0013]
[0014] The preparation of compound 3 includes: reacting 4-fluoroacetophenone (CAS: 403-42-9) and trimethylsilyl cyanide (CAS: 7677-24-9) under heating conditions to obtain compound 3.
[0015] The preparation of compound 7 includes: reacting 1,1-diphenylacetone (CAS: 781-35-1) and trimethylsilyl cyanide (CAS: 7677-24-9) under heating conditions to obtain compound 7.
[0016] Furthermore, the compound B of the present invention is selected from at least one of compounds 9 to 15:
[0017]
[0018]
[0019] Further, the mass percentage of compound A of the present invention in the lithium ion battery electrolyte is 0.05-5%. For example, the mass percentage of compound A in the lithium ion battery electrolyte may be, but is not limited to, 0.05%, 0.1%, 0.5%, 0.8%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%. Specifically, the mass percentage of compound A of the present invention in the lithium ion battery electrolyte is 0.05-1%.
[0020] Furthermore, the mass percentage of compound B of the present invention in the lithium-ion battery electrolyte is 0.05-1%; for example, the mass percentage of compound B in the electrolyte may be but is not limited to 0.05%, 0.1%, 0.5%, 0.8%, 1%.
[0021] Further, the mass ratio of compound A to compound B of the present invention is 0.1 to 8: 1. Preferably, the mass ratio of compound A to compound B of the present invention is 1:1.
[0022] Furthermore, the lithium salt of the present invention is selected from lithium hexafluorophosphate (LiPF 6) , lithium perchlorate (LiClO4), lithium tetrafluoroborate (LiBF4), lithium trifluoromethanesulfonate (LiCF3SO3), lithium bistrifluoromethanesulfonyl imide (LiTFSI), lithium bisoxalatoborate (LiBOB), lithium difluorophosphate (LiPO2F2), lithium fluorosulfonate (LiSO2F), lithium bisoxalatoborate (LiBC4O8), lithium difluorooxalatoborate, lithium difluorobisoxalatophosphate and lithium bisfluorosulfonyl imide. As an example, the lithium salt is lithium hexafluorophosphate (LiPF6), but is not limited thereto.
[0023] The mass percentage of the lithium salt in the lithium ion battery electrolyte of the present invention is 5-25%. The mass percentage of the lithium salt in the lithium ion battery electrolyte can be but not limited to 5%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 19%, 21%, 22%, 23%, 25%.
[0024] Further, the non-aqueous organic solvent of the present invention includes at least one of carboxylic acid esters, carbonates and ether compounds. Specifically, carboxylic acid esters include but are not limited to γ-butyrolactone, γ-valerolactone, δ-valerolactone, methyl acetate (MA), ethyl acetate (EA), ethyl propionate (EP), butyl acetate (n-Ba), propyl propionate (n-PP), butyl propionate. Carbonates include but are not limited to ethylene carbonate (EC), propylene carbonate, butylene carbonate (BC), pentylene carbonate, vinylene carbonate (VC), dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), propylene carbonate (PC). Ether compounds include, but are not limited to, 1,3-dioxolane (DOL), 1,4-dioxolane (DX), crown ether, tetrahydrofuran (THF), 2-methyltetrahydrofuran (2-CH3-THF), 2-trifluoromethyltetrahydrofuran (2-CF3-THF), dimethoxymethane, diethoxymethane, ethoxymethoxymethane, ethylene glycol di-n-propyl ether, ethylene glycol di-n-butyl ether, and diethylene glycol dimethyl ether.
[0025] Furthermore, the mass percentage of the non-aqueous organic solvent of the present invention in the lithium-ion battery electrolyte is 65-90%; preferably, the mass percentage of the non-aqueous organic solvent of the present invention in the lithium-ion battery electrolyte is 75-89%. As an example, the mass percentage of the non-aqueous organic solvent of the present invention in the lithium-ion battery electrolyte may be, but is not limited to, 78%, 80%, 81%, 82%, 83%, 84%, 85%, 86%, 87%, 88%, 89%.
[0026] Furthermore, the lithium-ion battery electrolyte of the present invention also includes an auxiliary agent, which includes at least one of fluoroethylene carbonate (FEC), vinyl sulfite, 1,3-propane sultone (PS), 1,3-propene sultone, 1,4-butane sultone, vinyl sulfate (DTD) and succinic anhydride.
[0027] To achieve the above objectives, the second aspect of the present invention further provides a lithium ion battery, comprising a positive electrode material, a negative electrode material and the lithium ion battery electrolyte mentioned above.
[0028] Compared with the prior art, the lithium ion battery electrolyte of the present invention uses compound A and compound B together as additives, so the lithium ion battery of the present invention has better high-temperature cycle performance, low-temperature discharge performance and lower internal resistance growth rate.
[0029] Furthermore, the positive electrode material of the present invention is selected from lithium transition metal oxide LiNi x Co y Mn z L 1-x-y-zO2, wherein L is selected from at least one of Al, Sr, Mg, Ti, Ca, Zr, Zn, Si or Fe, 0≤x≤1, 0≤y≤1, 0≤z≤1, 0<x+y+z≤1.
[0030] Furthermore, the negative electrode material of the present invention is selected from at least one of artificial graphite, natural graphite, lithium titanate, silicon-carbon composite material and silicon monoxide. DETAILED DESCRIPTION
[0031] The present invention will be further described below in conjunction with specific embodiments, but this should not limit the protection scope of the present invention.
[0032] Example 1
[0033] (1) Preparation of lithium-ion battery electrolyte
[0034] In a glove box filled with argon (O2 <1ppm, H2O <1ppm), ethylene carbonate (EC), ethyl methyl carbonate (EMC) and diethyl carbonate (DEC) were mixed in a weight ratio of EC:EMC:DEC=2:3:5 to obtain 85g of a non-aqueous organic solvent, followed by adding 0.5g of compound 1 and 0.5g of compound 9 as additives, dissolving and stirring well, then adding 14g of lithium hexafluorophosphate and mixing well to obtain a non-aqueous electrolyte.
[0035] (2) Preparation of positive electrode
[0036] LiNi 9.2 Co 0.3 Mn 0.5 O2 (NCM92), adhesive PVDF and conductive agent SuperP are mixed evenly in a mass ratio of 95:1:4 to form a lithium-ion battery positive electrode slurry with a certain viscosity. The mixed slurry is coated on both sides of an aluminum foil, and then dried and rolled to obtain a positive electrode sheet.
[0037] (3) Preparation of negative electrode sheet
[0038] Artificial graphite, conductive agent SuperP, thickener CMC, and adhesive SBR (styrene-butadiene rubber latex) are made into slurry in a mass ratio of 95:1.5:1.0:2.5, mixed evenly, coated on both sides of copper foil with the mixed slurry, and then dried and rolled to obtain a negative electrode sheet.
[0039] (4) Preparation of lithium-ion batteries
[0040] The positive electrode, the separator and the negative electrode are wound into a soft-pack battery cell, which is packaged with a polymer aluminum-plastic film and filled with the prepared lithium-ion battery non-aqueous electrolyte. After the processes of formation and capacity separation, a lithium-ion battery with a capacity of 1000 mAh is manufactured.
[0041] The formulas of the lithium ion battery electrolytes of Examples 2 to 14 and Comparative Examples 1 to 4 are shown in Table 1. The steps of preparing the lithium ion battery electrolytes and preparing the lithium ion batteries are the same as those of Example 1.
[0042] Table 1 Lithium-ion battery electrolyte formula
[0043]
[0044]
[0045]
[0046] The lithium ion batteries prepared in Examples 1 to 14 and Comparative Examples 1 to 4 were subjected to high temperature cycle tests, low temperature discharge tests and cycle internal resistance tests according to the following test conditions. The test results are shown in Table 2.
[0047] High temperature cycle performance test:
[0048] Place the lithium-ion battery in a 45℃ constant temperature box and let it stand for 30 minutes to make the lithium-ion battery reach a constant temperature. Charge it at a constant current of 1C to a voltage of 4.2V, then charge it at a constant voltage of 4.2V to a current of 0.05C, and then discharge it at a constant current of 1C to a voltage of 3.0V. Record the first discharge capacity of the battery as C0, which is a charge and discharge cycle. Then charge and discharge at 1C / 1C for 300 cycles at 45℃, record the discharge capacity as C1, and use the following formula to calculate the capacity retention rate of the lithium-ion battery.
[0049] Capacity retention rate = (C1 / C0) × 100%
[0050] Low temperature discharge performance test:
[0051] At a constant temperature of 25°C, charge the formed battery to 4.2V (NCM92) at 1C constant current and constant voltage, with a cut-off current of 0.05C. After standing for 5 minutes, discharge it to 3.0V (NCM92) at 0.5C constant current and constant voltage, record the initial discharge capacity C0 of the battery, charge it to 4.2V (NCM92) at 1C constant current and constant voltage, with a cut-off current of 0.05C, and then stand the battery at -20°C for 5 hours, discharge it to 3.0V (NCM92) at 0.33C constant current, record the discharge capacity C1 of the battery. Use the following formula to calculate the capacity retention rate of lithium-ion batteries.
[0052] Capacity retention rate = (C1 / C0) × 100%
[0053] Cyclic internal resistance growth rate test:
[0054] At 45°C, the divided battery is charged at room temperature at 0.5C constant current and constant voltage to a cut-off voltage of 4.2V, then discharged at constant current and constant voltage until the capacity drops to 50% SOC, the internal resistance of the battery is tested, and then charged at 1C constant current to 4.2V, and then cycled 300 times in this way, recording the internal resistance of the battery after the first full charge and the internal resistance of the battery after the last full charge. The following formula is used to calculate the internal resistance growth rate of lithium-ion batteries after 300 cycles of high-temperature cycling.
[0055] Internal resistance growth rate = (battery internal resistance after the last full charge - battery internal resistance after the first full charge) / battery internal resistance after the first full charge × 100%.
[0056] Table 2 Performance test results of lithium-ion batteries
[0057]
[0058] As can be seen from Table 1, the performance of the lithium ion batteries of all embodiments is better than that of Comparative Example 1, which shows that the additives of the present invention include compound A and compound B, wherein the cyano structure in compound A can complex the transition metal cations dissolved in the positive electrode material of the lithium ion battery, prevent it from entering the electrolyte to catalyze and aggravate the decomposition and gas production of the electrolyte, thereby improving the safety performance of the battery, and the cyano structure has high oxidation stability to ensure the stability of the lithium ion battery in a high-voltage working environment, and the cyano structure is a highly polar functional group, which helps the dissociation of lithium salts, thereby improving the cycle performance, low-temperature discharge performance and reducing the internal resistance of the lithium ion battery; however, the cyano structure has a low boiling point characteristic, which leads to the instability of the lithium ion battery in a high-temperature working environment, so the compound A is also introduced with a non-flammable and excellent thermally stable silicon group to improve the stability of the lithium ion battery in a high-temperature working environment. In addition, compound B can not only significantly reduce the increase in internal resistance caused by the accumulation of byproducts during the battery charge and discharge cycle, but also protect the integrity of the positive electrode material, thereby further improving the high-temperature cycle and low-temperature discharge performance of the lithium ion battery. Therefore, the present invention uses compound A and compound B as additives to improve the ring performance and low-temperature discharge performance, and can also effectively control the internal resistance growth during the high-temperature cycle process.
[0059] By comparing Example 1 with Example 12, it can be seen that the introduction of the auxiliary agent can further improve various performances of the lithium-ion battery.
[0060] By comparing Example 1 with Comparative Examples 2 to 3, it can be seen that compound A and compound B are used together as additives, and the synergistic effect of the two is utilized to make the lithium ion battery electrolyte not only improve the high temperature cycle performance and low temperature discharge performance of the lithium ion battery, but also effectively control the internal resistance growth during the high temperature cycle process; that is, removing either compound A or compound B will affect the performance of the lithium ion battery.
[0061] By comparing Example 1 with Comparative Example 4, it can be seen that the performance of the lithium ion battery of Comparative Example 4 is inferior to that of Example 1. This is because Compound B, as an acid anhydride additive, generates products containing open-chain diacid products containing active hydrogen. Too much of such products will affect the electrical properties of the lithium ion battery, so it is necessary to control the content of Compound B to not exceed 1%.
[0062] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A lithium ion battery electrolyte, characterized in that: The invention comprises a lithium salt, a non-aqueous organic solvent and an additive, wherein the additive comprises a compound A and a compound B, wherein the structure of the compound A is shown in Formula 1, the structure of the compound B is shown in Formula 2 or Formula 3, and the mass percentage of the compound B in the lithium ion battery electrolyte is 0.05-1%. wherein R1 is selected from an alkyl group, an alkyl halide phenyl group, a diaryl alkyl group or an ester group, R2 to R4 are each independently selected from an alkyl group, an alkoxy group, an alkynyl group, an alkenyl group, a phenyl group or a halogen group, X is selected from N or O, R5 is selected from an alkyl group, and R 6~ R7 is independently selected from alkyl or phenyl, R8 is selected from alkyl, alkenyl, phenyl or norbornene, and m, n, p is independently selected from 0 or 1.
2. The lithium ion battery electrolyte according to claim 1, characterized in that R1 is selected from C1~C6 alkyl, C1~C4 alkyl halophenyl, diaryl C1~C4 alkyl or C2~C5 alkyl ester, R2~R4 are each independently selected from C1~C6 alkyl, C1~C6 alkoxy, C2~C6 alkenyl, phenyl or halogen, X is selected from N or O, R5 is selected from C1~C4 alkyl, R6~R7 are each independently selected from C1~C6 alkyl or phenyl, R8 is selected from C1~C4 alkyl, C2~C4 alkenyl, phenyl or norbornene.
3. The lithium ion battery electrolyte according to claim 1, characterized in that The compound A is selected from at least one of compounds 1 to 8:
4. The lithium ion battery electrolyte according to claim 1, characterized in that The compound B is selected from at least one of compounds 9 to 15:
5. The high nickel lithium ion battery electrolyte according to claim 1, characterized in that: The mass percentage of the compound A in the lithium-ion battery electrolyte is 0.05-5%.
6. The lithium ion battery electrolyte according to claim 1, characterized in that The lithium salt is selected from at least one of lithium hexafluorophosphate, lithium perchlorate, lithium tetrafluoroborate, lithium trifluoromethanesulfonate, lithium bistrifluoromethanesulfonyl imide, lithium bisoxalatoborate, lithium difluorophosphate, lithium fluorosulfonate, lithium bisoxalatoborate, lithium difluorooxalatoborate, lithium difluorobisoxalatophosphate and lithium bisfluorosulfonyl imide.
7. The lithium ion battery electrolyte according to claim 1, characterized in that: The non-aqueous organic solvent includes at least one of carboxylic acid esters, carbonate esters and ether compounds.
8. The lithium ion battery electrolyte according to claim 1, characterized in that The invention also includes an auxiliary agent, which includes at least one of fluoroethylene carbonate, vinyl sulfite, 1,3-propane sultone, 1,3-propene sultone, 1,4-butane sultone, vinyl sulfate, and succinic anhydride.
9. A lithium ion battery, characterized in that: The invention comprises a positive electrode material, a negative electrode material and a lithium ion battery electrolyte as claimed in any one of claims 1 to 8.
10. The lithium ion battery according to claim 9, characterized in that The positive electrode material is selected from lithium transition metal oxide LiNi x Co y Mn z L 1-x-y-z O2, wherein L is selected from at least one of Al, Sr, Mg, Ti, Ca, Zr, Zn, Si or Fe, 0≤x≤1, 0≤y≤1, 0≤z≤1, 0<x+y+z≤1.