Positive sodium-supplementing additive applied to sodium-ion battery, preparation method of positive sodium-supplementing additive, positive plate and battery

By combining and modifying sodium oxalate with nickel nanoparticles, the positive sodium supplement additive for sodium ion batteries was prepared, which solved the decomposition voltage and utilization of sodium oxalate in commercial batteries, and significantly improved the energy density of sodium ion batteries and Cyclic stability.

CN119009180APending Publication Date: 2024-11-22HUNAN DESAY BATTERY CO LTD +1
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411130205.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The application of sodium oxalate in commercial sodium ion batteries is limited by its high decomposition voltage and low decomposition utilization, resulting in insufficient energy density and cycling stability.

Method used

By combining sodium oxalate with ethanol and nickel nanoparticles, micron-scale sodium oxalate particles are prepared, and modified by nickel-based catalysts to reduce the decomposition voltage of sodium oxalate, and combine the layer oxygen positive electrode or polyanion positive electrode to achieve effective positive sodium supplementation effect. Enhance the battery's first and cycle performance.

Benefits of technology

It significantly improves the energy density and cycle life of sodium ion batteries, achieves more than 90% of the first-round decomposition efficiency, and maintains good stability, and is suitable for commercial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119009180A_ABST
    Figure CN119009180A_ABST
Patent Text Reader

Abstract

The invention discloses a positive sodium supplement additive applied to a sodium ion battery, a preparation method, a positive plate and a battery. The preparation method comprises the following steps: adding a sodium oxalate saturated solution into ethanol to obtain sodium oxalate particles; the method comprises the following steps: reacting a solution containing ethanol, anhydrous nickel chloride and triethanolamine in the presence of inert gas to obtain Ni molecular catalyst powder; and stirring ethanol, the Ni molecular catalyst and the sodium oxalate particles, drying by distillation, and calcining to obtain the positive sodium supplement additive for the sodium ion battery. A small amount of nickel-based catalyst in the anode sodium supplementing additive has good catalytic performance, can catalyze decomposition of sodium oxalate and can reduce the decomposition potential of sodium oxalate, so that the composite sodium supplementing agent has the first-circle decomposition efficiency of 90% or above under the cut-off voltage of 4.25 V.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of sodium ion batteries, and in particular relates to a positive electrode sodium supplement additive applied to sodium ion batteries, a preparation method thereof, a positive electrode sheet and a battery. Background Art

[0002] Lithium-ion batteries have been used more and more widely in recent years. However, with the sharp rise in the price of lithium carbonate, the cost of batteries has become higher. At the same time, the limited reserves of metallic lithium in the earth also pose certain challenges to its large-scale application in the future. Sodium-ion batteries have abundant raw material resources and are relatively cheap. They are increasingly attracting attention from the industry and have shown good potential in large-scale energy storage applications. Since the solid electrolyte interface (SEI) film generated at the negative electrode consumes the active sodium ions released from the positive electrode, the first efficiency of the battery is reduced, thereby reducing the energy density and cycle stability of the battery. The first irreversible capacity loss has become one of the bottlenecks restricting the development of sodium-ion batteries. Researchers have found that sodium supplementation technology can effectively supplement the first irreversible capacity loss of sodium-ion batteries, thereby improving the energy density and cycle life of sodium-ion batteries. According to the different locations of sodium ion release, it can be divided into positive electrode sodium supplementation, negative electrode sodium supplementation and third electrode sodium supplementation. Negative electrode sodium supplementation usually requires the use of metallic sodium powder, which has a relatively harsh operating environment, is difficult to apply on a large scale and is very costly, and is generally used in laboratory research; third electrode sodium supplementation is to supplement the battery with sodium through a metallic sodium electrode as the third electrode, and its operating environment is also relatively harsh. At the same time, this method has the problems of non-uniform diffusion of sodium ions and a relatively complex operating process, and its industrial application is also relatively limited; positive electrode sodium supplementation technology generally refers to the addition of sodium supplementation additives during the positive electrode homogenization process. The sodium supplementation has good uniformity and is compatible with the existing battery homogenization coating process, and has good application prospects. Sodium oxalate, as a positive electrode sodium supplementation additive, has the advantages of low cost and high capacity. However, the higher decomposition voltage and lower decomposition utilization rate of commercial sodium oxalate limit its application in commercial sodium-ion batteries. Summary of the invention

[0003] In order to overcome the problem in the prior art that sodium oxalate cannot be used in commercial sodium ion batteries due to its high decomposition voltage and low decomposition utilization rate, the purpose of the present invention is to propose a positive electrode sodium supplement additive for sodium ion batteries, a preparation method, a positive electrode sheet, and a battery. The preparation method modifies sodium oxalate and changes its performance, so that the positive electrode sodium supplement additive has better stability, can supplement the sodium loss caused by the formation of the negative electrode SEI film and the irreversible reaction, and greatly improve the energy density of the sodium ion full battery.

[0004] To achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0005] A method for preparing a positive electrode sodium supplement additive for a sodium ion battery comprises the following steps:

[0006] adding a saturated sodium oxalate solution into ethanol to obtain sodium oxalate particles;

[0007] A solution containing ethanol, anhydrous nickel chloride and triethanolamine is reacted under an inert gas to obtain a Ni molecular catalyst powder;

[0008] The ethanol, Ni molecular catalyst and sodium oxalate particles are mixed and stirred, evaporated to dryness, and calcined to obtain a positive electrode sodium supplement additive for sodium ion batteries.

[0009] Furthermore, when preparing the sodium oxalate particles, the volume ratio of the saturated sodium oxalate solution to ethanol is 10-20 mL: 100-200 mL.

[0010] Furthermore, when preparing the Ni molecular catalyst powder, the usage ratio of ethanol and anhydrous nickel chloride is 150-300 mL: 5-10 mg.

[0011] Furthermore, when preparing the Ni molecular catalyst powder, the usage ratio of anhydrous nickel chloride and triethanolamine is 5-10 mg: 1-2 mL.

[0012] Furthermore, the reaction temperature is 70-78°C and the reaction time is 30-40 min.

[0013] Furthermore, when preparing the positive electrode sodium supplement additive for sodium ion batteries, the usage ratio of ethanol to sodium oxalate particles is 20-40mL:1-2g.

[0014] Furthermore, when preparing the positive electrode sodium supplement additive for sodium ion batteries, the mass ratio of Ni molecular catalyst to small particle sodium oxalate is 0.4-0.5:1; the calcination temperature is 300-350°C and the time is 4-5 hours.

[0015] A positive electrode sodium supplement additive for sodium ion batteries comprises sodium oxalate modified with nickel nanoparticles, wherein the particle size of the sodium oxalate is 0.5-10 microns.

[0016] A positive electrode sheet comprises a positive electrode sodium supplement additive prepared by the method.

[0017] A sodium ion battery, comprising the positive electrode sodium supplement additive prepared by the method and / or the positive electrode material.

[0018] Compared with the prior art, the present invention has the following beneficial effects:

[0019] The present invention prepares micron-sized sodium oxalate particles, which initially reduce the decomposition voltage of sodium oxalate; then, the decomposition voltage of sodium oxalate is greatly reduced by surface modification of nickel-based catalysts, and a better positive electrode sodium supplementation effect can be achieved by coupling with a layered oxygen positive electrode or a polyanion positive electrode, thereby compensating for the loss of active sodium caused by SEI growth on the surface of the hard carbon negative electrode, improving the first efficiency and cycle performance of the battery, and at the same time, the battery can be charged at 4.25V (vs. Na + / Na) to achieve a first-cycle decomposition efficiency of more than 90%. The original ion catalysis coupled size control effect of this invention greatly improves the sodium supplementation performance of sodium oxalate. After being applied to the battery system, it effectively improves the first efficiency and cycle performance of the battery, showing good commercial application prospects. When used, the positive electrode sodium supplement additive of the present invention is added directly when the positive electrode is stirred, which is compatible with the existing slurry coating process and does not require the modification of the battery production process.

[0020] Furthermore, the sodium oxalate prepared by the anti-solvent crystallization method based on solvent ratio control in the present invention has a particle size smaller than that of ordinary recrystallized sodium oxalate, has a shorter sodium ion and electron transmission path, and has better electrical conductivity, so that the decomposition potential of sodium oxalate is further reduced, thereby having better decomposition performance.

[0021] The positive electrode sodium supplement additive of the present invention is stable in the air and has significant effects. It can supplement the sodium loss caused by the formation of the negative electrode SEI film and irreversible reactions, greatly improving the energy density of the sodium ion full battery. The positive electrode sodium supplement additive of the present invention can be oxidized and provide sodium ions during the first charging process. At the same time, the residual components are converted into gas and can be removed by the degassing process after high-temperature formation during the battery production process. The high decomposition rate ensures that it will not continue to produce gas in subsequent cycles. A small amount of nickel-based catalyst in the positive electrode sodium supplement additive has good catalytic performance, can catalyze the decomposition of sodium oxalate, and can reduce the decomposition potential of sodium oxalate, so that the composite sodium supplement has a first-cycle decomposition efficiency of more than 90% at a cut-off voltage of 4.25V. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 Schematic diagram of the structure of Ni-modified Na2C2O4;

[0023] Figure 2 SEM element distribution map of Na2C2O4 composite additive modified for Ni-based catalyst;

[0024] Figure 3 These are the charge and discharge curves of Na2C2O4 / Ni(8%)-Na3V2(PO4)3 and Na3V2(PO4)3. DETAILED DESCRIPTION

[0025] In order to facilitate the understanding of the present invention, the present invention will be described more fully below with reference to the relevant drawings. The preferred embodiments of the present invention are given in the drawings. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present invention more thoroughly and comprehensively understood.

[0026] In an ordinary sodium ion full battery, part of the sodium ions released from the positive electrode during the first charging process will be used to form an SEI film on the surface of the negative electrode, thereby reducing the number of sodium ions available for deintercalation in the full battery, resulting in a decrease in the capacity and energy density of the full battery. The sodium supplement additive added to the positive electrode requires that it can undergo electro-oxidative decomposition during the first charging process and provide sodium ions to supplement the deintercalation sodium ions in the full battery. At the same time, the additive is irreversible after decomposition, that is, it will not react with sodium ions in the subsequent cycle process. Secondly, the additive is also required to have good stability in the air and during the electrode preparation process, which is conducive to simplifying the operation and reducing costs. The positive electrode sodium supplement additive in the present invention has good stability and can be directly mixed and stirred with active materials, conductive agents and adhesives in the air to prepare positive electrodes. Therefore, the use of the additive will not affect the existing sodium ion battery production process. After assembling the battery, the additive undergoes irreversible decomposition during the first charging process, providing sodium ions to supplement the sodium loss caused by the negative electrode side reaction, and the residual part becomes gas, which can be removed by the degassing step after hot pressing during the battery production process, and will not affect the electrochemical performance of the battery. The composite sodium supplement additive of the present invention can, on the one hand, effectively supplement the loss of active sodium in the first cycle and improve the energy density of the battery; on the other hand, more active sodium can be pre-stored by appropriately excessive sodium supplementation for the first time to supplement the loss of active sodium in the cycle, thereby enhancing the cycle life of the battery.

[0027] A method for preparing a positive electrode sodium supplement additive for a sodium ion battery of the present invention comprises the following steps:

[0028] 1) Weigh 5-10g of commercial sodium oxalate, disperse it in 50-100mL of water, stir for 1-2 hours, filter to remove insoluble impurities, and obtain a saturated sodium oxalate solution. Slowly add (1 second / drop) 10-20mL of saturated sodium oxalate solution to 100-200mL of ethanol through a dropping funnel, and a precipitate will be generated. Centrifuge and dry to obtain the precipitated solid powder small particles of sodium oxalate.

[0029] 2) Add 5-10 mg of anhydrous nickel chloride and 1-2 mL of triethanolamine to 150-300 mL of ethanol, stir evenly, reflux with N2 for 30 minutes, and centrifuge and dry to obtain a light blue Ni molecular catalyst powder.

[0030] 3) Add 0.5-1g of light blue Ni-based molecular catalyst to 20-40mL of ethanol, then add 1-2g of small-particle sodium oxalate, stir for 30 minutes and evaporate to dryness to obtain solid powder, calcine at 300-350℃ in vacuum for 4-5 hours to obtain positive electrode sodium supplement additive, namely Ni-Na2C2O4. The mass ratio of light blue Ni-based molecular catalyst to small-particle sodium oxalate is 0.4-0.5;

[0031] The present invention provides a positive electrode sodium supplement additive for sodium ion batteries, comprising a composite material of small-particle sodium oxalate modified with ultra-small nickel nanoparticles, such as Figure 1 and Figure 2 As shown. The particle size of small-particle sodium oxalate is 0.5-10 microns, preferably 3-7 microns. It is prepared by anti-solvent crystallization and can be directly used in the positive electrode of sodium ion batteries to play a role in sodium supplementation; nickel ion modified sodium oxalate composite material is mainly prepared by in-situ surface adsorption followed by vacuum high-temperature calcination. The element distribution test under scanning electron microscopy proves the presence of Ni on the surface of sodium oxalate (see Figure 2 ).

[0032] 4) The positive electrode material, the conductive agent (Ketjen Black), the binder and the sodium supplement additive are mixed, a solvent is added to adjust the mixture into a slurry, and then the mixture is coated on the surface of the current collector, and the positive electrode sheet is obtained after vacuum drying.

[0033] The mass ratio of the positive electrode material, the conductive agent, the binder and the sodium supplement additive is 8:1:1:0.3-2.

[0034] The positive electrode material is sodium vanadium fluoride phosphate (Na3V2(PO4)2F3), sodium vanadium phosphate (Na3V2(PO4)3), Prussian blue, or layered oxide Na x Ni a Mn b M c O2, where 0.5≤x≤1, 0.15≤a≤0.33, a+b+c=1, 0.67≥b>0, c>0, and M is Li + Mg 2+ , Ca 2+ 、Al 3+ 、Ti 4+ 、V 3+ , Fe 3+ 、Co 3+ , Cu 2+ 、Zn 2+ 、Zr 4+ , Nb 5+ , W 5+ , Y 3+ ,La 3+ 、Ce 4+ , Er 3+At least one of the above, Ni, Mn and M elements together constitute a transition metal layer, and the transition metal layer and the Na layer are alternately arranged in the middle of the oxygen layer to form a layered composite oxide.

[0035] The negative electrode material of the sodium ion battery is hard carbon, soft carbon, transition metal oxide, transition metal sulfide, transition metal phosphide or alloy (Sn, P, Se, Bi, etc.) material and composite materials thereof.

[0036] The binder is polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), sodium alginate or styrene-butadiene rubber (SBR).

[0037] The solvent is N-methylpyrrolidone, water, toluene or ethanol.

[0038] The current collector is aluminum foil, copper foil, steel wire mesh or nickel foam.

[0039] Preferably, the positive electrode material Na 0.67 Mn 0.67 Ni 0.33 O2, Ketjen black, and PVDF are mixed in a mass ratio of 80:10:10, and then 3-20wt% of Ni-Na2C2O4 of the positive electrode material is added and mixed thoroughly. Then NMP is added to make a slurry, and it is evenly coated on the surface of the Al foil with a scraper, and placed in a vacuum drying oven at 110°C for 10 hours to obtain the Al foil with active materials, and the Al foil with active materials is cut into disc-shaped positive electrode sheets.

[0040] A sodium ion battery, comprising a positive electrode sodium supplement additive and / or the positive electrode sheet.

[0041] The present invention is further described below by way of examples.

[0042] Example 1

[0043] Preparation of a positive electrode sodium supplement additive for sodium ion batteries, namely Ni-Na2C2O4:

[0044] 1) Weigh 10g of commercial sodium oxalate, disperse it in 100mL of water, stir for 2 hours, filter to remove insoluble impurities, and obtain a saturated sodium oxalate solution. Slowly add (1 second / drop) 20mL of saturated sodium oxalate solution to 200mL of ethanol through a dropping funnel, and a precipitate will be generated. Centrifuge and dry to obtain the precipitated solid powder small particles of sodium oxalate.

[0045] 2) Add 10 mg of anhydrous nickel chloride and 2 mL of triethanolamine to 300 mL of ethanol, stir evenly, reflux with N2 for 30 minutes, and centrifuge and dry to obtain a light blue Ni molecular catalyst powder.

[0046] 3) In 20 mL of ethanol, 0.5 g of Ni-based molecular catalyst was added, followed by 1 g of small-particle sodium oxalate. After stirring for 30 minutes, the mixture was evaporated to dryness to obtain a solid powder. After calcination at 300 ° C in vacuum for 4 hours, a positive electrode sodium supplement additive for sodium ion batteries, namely Ni-Na2C2O4, was obtained.

[0047] Preparation of positive electrode sheet containing sodium supplement additive: 0.67 Mn 0.67 Ni 0.33 O2, Ketjen Black, and PVDF were mixed in a mass ratio of 80:10:10, and then 5% of the mass of the positive electrode material Ni-Na2C2O4 was added and mixed thoroughly. Then NMP was added to make a slurry, and it was evenly coated on the surface of the Al foil with a scraper. After being placed in a vacuum drying oven at 110°C for 10 hours, the Al foil with active materials was cut into a disc-shaped positive electrode sheet, which was recorded as Na 0.67 Mn 0.67 Ni 0.33 O2-5%Ni-Na2C2O4.

[0048] Half-cell assembly: CR2032 button cells were assembled in an Ar-filled MBRAUN glove box using the prepared Na 0.67 Mn 0.67 Ni 0.33 O2-5% Ni-Na2C2O4 electrode as the positive electrode, 1mol / L NaClO4 propylene carbonate (PC) / 5% fluoroethylene carbonate (FEC) (V / V) as the electrolyte, and Na metal sheet as the negative electrode to assemble 2032 button cells. The button cells were placed in the test system at 2.5-4.25V (vs. Na + / Na, the same below), and charge and discharge at a current density of 20mA / g. 0.67 Mn 0.67 Ni 0.33 The initial charge and discharge capacities of the O2-5% Ni-Na2C2O4 positive electrode are shown in Table 1. The initial charge and discharge capacities are 159mAh / g and 134mAh / g, respectively. The increase in specific capacity comes from the decomposition of Na2C2O4. The first cycle decomposition rate of sodium oxalate is about 97% by calculation. Its cycle performance is shown in Table 1. After 100 cycles, the capacity retention rate is still higher than 90%, which is comparable to that of Na 0.67 Mn 0.67 Ni 0.33 O2 electrode equivalent.

[0049] Assembly of negative electrode sheet: Mix 2% negative electrode binder (SBR:CMC=2:1) ​​with water, stir at a rate of 500rad / min for 30min to obtain glue; mix 97% negative electrode active material (hard carbon), 1% negative electrode conductive agent (carbon black) and water, stir at a speed of 400rad / min for 30min; then add the prepared glue, stir at a speed of 1500rad / min for 120min; after stirring evenly, stir at a speed of 200rad / min for 6h to obtain negative electrode slurry for standby use. The total amount of water is to control the solid content of the entire negative electrode slurry to 44% and the viscosity to 2200CP. The negative electrode slurry is evenly coated on one side of the carbon-coated aluminum foil (16μm), and then heated and dried. After the heating and drying is completed, the negative electrode slurry is evenly coated on the other side of the carbon-coated aluminum foil, and heated and dried to obtain a negative electrode sheet containing a negative electrode active material layer.

[0050] Soft-pack full battery assembly: stack the positive electrode sheet, polypropylene film, and negative electrode sheet in order, so that the polypropylene film is between the positive electrode sheet and the negative electrode sheet to play an isolating role, and then stack the sheets to obtain a bare battery cell; then weld the positive and negative electrode ears, pre-package the aluminum-plastic film, dry, and inject the electrolyte (the electrolyte is NaPF6, the concentration is 1mol / L, and the solvent is EC:DEC:DMC=1:1:1); then seal, form, age, and separate the capacity to finally obtain a soft-pack sodium ion battery; the design capacity of the soft-pack sodium ion battery is 1Ah. The test process of the soft-pack battery is as follows: the first cycle is charged and discharged at a current density of 20mAh / g in the voltage range of 2.5-4.25V, and then from the second cycle, the voltage range of 2.5V-4.0V is charged and discharged at a current density of 60mAh / g, and the cycle is repeated for 300 cycles, and the capacity retention rate is recorded.

[0051] Example 2

[0052] The same as Example 1, except that the ratio of Ni-Na2C2O4 is 3%, and the others are the same as Example 1.

[0053] Example 3

[0054] The same as Example 1, except that the ratio of Ni-Na2C2O4 is 10%, and the others are the same as Example 1.

[0055] Example 4

[0056] The same as Example 1, except that the ratio of Ni-Na2C2O4 is 15%, and the others are the same as Example 1.

[0057] Example 5

[0058] The same as Example 1, except that the positive electrode material is replaced with Na3V2(PO4)3, and the content of the sodium supplement additive is adjusted to 8%, thereby obtaining a Na3V2(PO4)3-8% Ni-Na2C2O4 positive electrode sheet and battery.

[0059] Example 6

[0060] 1) Weigh 5g of commercial sodium oxalate, disperse it in 50mL of water, stir for 2 hours, filter to remove insoluble impurities, and obtain a saturated sodium oxalate solution. Slowly add (1 second / drop) 10mL of saturated sodium oxalate solution to 100mL of ethanol through a dropping funnel, and a precipitate will be generated. Centrifuge and dry to obtain the precipitated solid powder small particles of sodium oxalate.

[0061] 2) Add 10 mg of anhydrous nickel chloride and 2 mL of triethanolamine to 300 mL of ethanol, stir evenly, reflux with N2 for 30 minutes, and centrifuge and dry to obtain a light blue Ni molecular catalyst powder.

[0062] 3) In 20 mL of ethanol, 0.5 g of Ni-based molecular catalyst was added, followed by 1 g of small-particle sodium oxalate. After stirring for 30 minutes, the mixture was evaporated to dryness to obtain a solid powder. After vacuum calcination at 350° C. for 4 hours, a positive electrode sodium supplement additive for sodium ion batteries, namely Ni-Na2C2O4, was obtained.

[0063] Example 7

[0064] 1) Weigh 7g of commercial sodium oxalate, disperse it in 70mL of water, stir for 2 hours, filter to remove insoluble impurities, and obtain a saturated sodium oxalate solution. Slowly add (1 second / drop) 20mL of saturated sodium oxalate solution to 200mL of ethanol through a dropping funnel, and a precipitate will be generated. Centrifuge and dry to obtain the precipitated solid powder small particles of sodium oxalate.

[0065] 2) Add 5 mg of anhydrous nickel chloride and 1 mL of triethanolamine to 1500 mL of ethanol, stir evenly, reflux with N2 for 30 minutes, and centrifuge and dry to obtain a light blue Ni molecular catalyst powder.

[0066] 3) In 40 mL of ethanol, add 1 g of light blue Ni-based molecular catalyst, then add 2 g of small-particle sodium oxalate, stir for 40 minutes and evaporate to dryness to obtain a solid powder. After vacuum calcination at 320°C for 4.5 hours, a positive electrode sodium supplement additive for sodium ion batteries, namely Ni-Na2C2O4, is obtained.

[0067] Example 8

[0068] 1) Weigh 8g of commercial sodium oxalate, disperse it in 80mL of water, stir for 2 hours, filter to remove insoluble impurities, and obtain a saturated sodium oxalate solution. Slowly add (1 second / drop) 15mL of saturated sodium oxalate solution to 150mL of ethanol through a dropping funnel, and a precipitate will be generated. Centrifuge and dry to obtain the precipitated solid powder small particles of sodium oxalate.

[0069] 2) Add 5 mg of anhydrous nickel chloride and 1 mL of triethanolamine to 150 mL of ethanol, stir evenly, reflux with N2 for 30 minutes, and centrifuge and dry to obtain a light blue Ni molecular catalyst powder.

[0070] 3) In 40 mL of ethanol, add 1 g of light blue Ni-based molecular catalyst, then add 2 g of small-particle sodium oxalate, stir for 40 minutes and evaporate to dryness to obtain a solid powder. After calcining at 300 ° C in vacuum for 5 hours, a positive electrode sodium supplement additive for sodium ion batteries, namely Ni-Na2C2O4, is obtained.

[0071] Comparative Example 1

[0072] Preparation of positive electrode sheet without sodium supplementation additive: 0.67 Mn 0.67 Ni 0.33 O2, Ketjen black, and PVDF were mixed in a mass ratio of 80:10:10. Then N-methylpyrrolidone (NMP) was added to make a slurry, which was evenly coated on the surface of aluminum (Al) foil using a scraper, and dried at 90°C in a vacuum drying oven for 10 hours, and then the Al foil with active materials was cut into disc-shaped positive electrode sheets.

[0073] Except for the positive electrode sheet, the preparation steps of the half-cell and full-cell are the same as in the embodiment. 0.67 Mn 0.67 Ni 0.33 The first charge and discharge capacities of the O2 positive electrode are shown in Table 1, and the first charge and discharge capacities are 147 mAh / g and 133 mAh / g, respectively. The cycle performance is shown in Table 1, and the capacity retention rate of the electrode after 100 cycles is still higher than 90%.

[0074] Comparative Example 2

[0075] The Ni-Na2C2O4 in Example 1 was replaced with small-particle Na2C2O4, and the other conditions remained the same.

[0076] Comparative Example 3

[0077] The Ni-Na2C2O4 in Example 1 was replaced with commercial Na2C2O4, and the other conditions remained the same.

[0078] Comparative Example 4

[0079] The Ni-Na2C2O4 in Example 1 was replaced with a light blue Ni molecular catalyst, and the other conditions remained the same.

[0080] Comparative Example 5

[0081] The Ni-Na2C2O4 in Example 5 was not added, and the other conditions remained the same.

[0082] Table 1 Parameters of half-cells or full-cells assembled in the examples and comparative examples

[0083]

[0084] Specific methods of performance testing:

[0085] First coulombic efficiency: In the battery formation step or the first week of the power-off cycle, record the charging capacity Q1 and the discharging capacity Q2. The value of the first coulombic efficiency = Q2 / Q1×100%.

[0086] Capacity retention rate after 300 cycles: At 25°C, charge and discharge at a current density of 20mAh / g in the voltage range of 2.5-4.25V for the first cycle, and then charge and discharge at a current density of 60mAh / g in the voltage range of 2.5V-4.0V from the second cycle. Cycle 300 cycles and record the capacity retention rate. Calculate the capacity retention rate according to the following formula

[0087] Capacity retention rate = (discharge capacity at the 300th week / initial nominal capacity of the battery) × 100%.

[0088] Result analysis:

[0089] From the results in Table 1, it can be seen that the small-particle sodium oxalate modified with Ni on the surface has good decomposition performance, and the first-cycle decomposition efficiency at 4.25V is above 95%, which proves its good decomposition performance. Through the data of Examples 1-4, it can be found that by increasing the proportion of NiO-Na2C2O4 in the layered oxygen positive electrode | hard carbon negative electrode battery, the charging capacity based on the positive electrode gradually increases, but the decomposition rate is slightly reduced. This may be because as the dosage of the composite sodium supplement increases, the conductivity of the electrode is affected, thereby affecting the decomposition effect of the composite sodium supplement. The capacity retention rate after 300 cycles is close. By comparing the embodiment with comparative example 1, it can be clearly found that the composite sodium supplement can not only improve the first charging capacity of the battery and thus improve the energy density of the battery, but also improve the cycle life of the battery. Through the embodiment and comparative example 2, it can be found that simple small-particle sodium oxalate has poor decomposition performance, which in turn proves the importance of nickel oxide catalysts. By comparing Comparative Example 2 with Comparative Example 3, it can be found that commercial sodium oxalate does not decompose at 4.25V, while small-particle sodium oxalate partially decomposes, proving the good decomposition performance of small particles prepared by the anti-solvent crystallization method, which is mainly due to its relatively good electrical conductivity. By comparing Comparative Example 4 with the embodiment, it can be found that the presence of Ni has basically no effect on the cycle performance of the battery, which may be because the content of Ni in the entire electrode is very low, eliminating the potential adverse effects of possible Ni ion dissolution, and further proving the good application prospects of this solution. In other positive electrode systems, the sodium supplement also exhibits relatively good sodium supplement performance. Figure 3 As shown, it can be found from Example 5 and Comparative Example 5 that the decomposition rate of Na2C2O4 / Ni (8%) sodium supplement reaches 98%, which can significantly improve the charge and discharge capacity and cycle life of Na3V2(PO4)3.

[0090] The above description is only for the best embodiment of the present invention, but it should not be understood as limiting the claims. The present invention is not limited to the above embodiments, and its specific structure is allowed to be changed. However, all changes made within the protection scope of the independent claims of the present invention are within the protection scope of the present invention.

[0091] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.

Claims

1. A method for preparing a positive electrode sodium supplement additive for a sodium ion battery, characterized in that: The following steps are involved: adding a saturated sodium oxalate solution into ethanol to obtain micrometer-sized sodium oxalate particles; A solution containing ethanol, anhydrous nickel chloride and triethanolamine is reacted under an inert gas to obtain a Ni molecular catalyst powder; The ethanol, Ni molecular catalyst and sodium oxalate particles are mixed and stirred, evaporated to dryness, and calcined to obtain a positive electrode sodium supplement additive for sodium ion batteries.

2. The method for preparing the positive electrode sodium supplement additive for sodium ion battery according to claim 1, characterized in that: When preparing sodium oxalate particles, the volume ratio of the saturated sodium oxalate solution to ethanol is 10-20 mL: 100-200 mL.

3. The method for preparing the positive electrode sodium supplement additive for sodium ion battery according to claim 1, characterized in that: When preparing Ni molecular catalyst powder, the usage ratio of ethanol and anhydrous nickel chloride is 150-300 mL: 5-10 mg.

4. The method for preparing the positive electrode sodium supplement additive for sodium ion battery according to claim 1, characterized in that: When preparing Ni molecular catalyst powder, the usage ratio of anhydrous nickel chloride and triethanolamine is 5-10 mg:1-2 mL.

5. The method for preparing the positive electrode sodium supplement additive for sodium ion battery according to claim 1, characterized in that: The reaction temperature is 70-78°C and the reaction time is 30-40 minutes.

6. The method for preparing the positive electrode sodium supplement additive for sodium ion battery according to claim 1, characterized in that: When preparing a positive electrode sodium supplement additive for sodium ion batteries, the usage ratio of ethanol to sodium oxalate particles is 20-40 mL: 1-2 g.

7. The method for preparing the positive electrode sodium supplement additive for sodium ion battery according to claim 1, characterized in that: When preparing the positive electrode sodium supplement additive for sodium ion batteries, the mass ratio of Ni molecular catalyst to small particle sodium oxalate is 0.4-0.5:1; the calcination temperature is 300-350°C and the time is 4-5 hours.

8. A positive electrode sodium supplement additive for sodium ion batteries prepared according to the method according to any one of claims 1 to 7, characterized in that: The invention comprises sodium oxalate modified with nickel nanoparticles, and the particle size of the sodium oxalate is 0.5-10 microns.

9. A positive electrode sheet, characterized in that: The positive electrode sodium supplement additive comprises the one prepared by the method according to any one of claims 1 to 7.

10. A sodium ion battery, characterized in that: The sodium ion battery comprises the positive electrode sodium supplement additive prepared by the method according to any one of claims 1 to 7 and / or the positive electrode sheet according to claim 9.

Citation Information

Cited By

  • Method for promoting oxidation of sodium oxalate through coating of conductive polymer, composite sodium supplementing agent and application of composite sodium supplementing agent

    CN119786608A

  • A nanoscale sodium oxalate / carbon composite sodium supplement, a preparation method thereof and application thereof in sodium ion batteries

    CN122907638A