Copolymer, rubber composition, tire, and method for producing copolymer

By using copolymers of specific proportions and structures in rubber, combined with copolymerization and graft polymerization processes, the problem of insufficient deterioration resistance characteristics in the existing rubber technology is solved, and the high deterioration resistance characteristics of rubber components and rubber compositions are achieved and low loss, improving tire performance.

CN119013322APending Publication Date: 2024-11-22BRIDGESTONE CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380033544.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-05-10
Filing Date
2023-01-12
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing rubber technology cannot achieve sufficient deterioration resistance, and the deterioration resistance of rubber still needs to be further improved.

Method used

By using copolymers containing ethylene, α-olefin units with more than 6 carbon atoms, non-conjugated diene units and aromatic vinyl units, novel rubber components with excellent deterioration resistance, and by specific copolymerization The product manufacturing method includes a copolymerization step and a graft polymerization step to prepare a copolymer having a weight average molecular weight of 200,000 or more for preparing a rubber composition and a tire.

Benefits of technology

The excellent deterioration resistance and low loss properties of the rubber components and rubber composition are achieved, and the performance stability of the tire is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005078722390000101
    Figure BDA0005078722390000101
  • Figure BDA0005078722390000161
    Figure BDA0005078722390000161
  • Figure BDA0005078722390000191
    Figure BDA0005078722390000191
Patent Text Reader

Abstract

The present invention provides a rubber component having excellent degradation resistance characteristics. This copolymer is characterized by comprising: ethylene units; an alpha-olefin unit having 6 or more carbon atoms; a non-conjugated diene unit; and an aromatic vinyl unit.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to copolymers, rubber compositions, tires, and methods of making the copolymers. Background Art

[0002] For rubber products such as tires, efforts are being made to develop elastomers (rubber components) having excellent degradation resistance characteristics in order to suppress the degradation of performance over time. For example, a technology for reducing the amount of double bonds in a polymer by changing the monomer ratio when synthesizing EPDM (ethylene-propylene-diene rubber) or a hydrogenation technology for reducing the amount of double bonds after synthesizing a diene copolymer has been studied.

[0003] For example, PTL 1 discloses that a rubber composition having excellent heat aging resistance can be obtained by using a predetermined copolymer rubber and a diene rubber in a predetermined ratio.

[0004] Citation List

[0005] PTL1: JPH08-337694A Summary of the invention

[0006] Problem that the invention aims to solve

[0007] However, the above conventional rubber technologies cannot achieve sufficient anti-degradation properties, and there is still a need to further improve the anti-degradation properties.

[0008] Therefore, an object of the present disclosure is to solve the above-mentioned problems of the prior art and to provide a rubber component having excellent anti-degradation characteristics and a method for producing the same.

[0009] Furthermore, another object of the present disclosure is to provide a rubber composition and a tire having excellent anti-deterioration characteristics including such a rubber component.

[0010] Solutions for solving problems

[0011] As a result of intensive studies to solve the above-mentioned problems, the present inventors found that a novel elastomer (rubber component) having excellent anti-degradation characteristics can be obtained by synthesis using predetermined monomers, and thus completed the present disclosure.

[0012] The main configuration of the present disclosure to solve the above-mentioned problems is as follows.

[0013] [1] A copolymer comprising an ethylene unit, an α-olefin unit having 6 or more carbon atoms, a non-conjugated diene unit, and an aromatic vinyl unit.

[0014] [2] The copolymer according to [1], wherein the proportion of ethylene units is 75 mol% or less, the proportion of α-olefin units is 20 mol% or more, the proportion of non-conjugated diene units is 1.0 mol% or more, and the proportion of aromatic vinyl units is 0.5 mol% or more.

[0015] [3] The copolymer according to [1] or [2], comprising:

[0016] A main chain portion having an ethylene unit, an α-olefin unit having 6 or more carbon atoms, a non-conjugated diene unit and an aromatic vinyl unit, and

[0017] A branched chain portion having a conjugated diene unit bonded to the main chain portion.

[0018] [4] The copolymer according to [3], wherein in the main chain portion, the proportion of ethylene units is 75 mol% or less, the proportion of α-olefin units is 20 mol% or more, the proportion of non-conjugated diene units is 1.0 mol% or more, and the proportion of aromatic vinyl units is 0.5 mol% or more.

[0019] [5] The copolymer according to [3] or [4], wherein the weight average molecular weight of the copolymer is 200,000 or more, and the proportion of the branched portion in the copolymer is 1% by mass or more.

[0020] [6] The copolymer according to any one of [1] to [5], which has a weight average molecular weight of 200,000 or more.

[0021] [7] The copolymer according to any one of [1] to [6], wherein the aromatic vinyl unit includes a 4-methylstyrene unit.

[0022] [8] The copolymer according to any one of [1] to [7], which has a molecular weight distribution of 4.0 or less.

[0023] [9] A rubber composition comprising the copolymer according to any one of [1] to [8].

[0024]

[10] A tire comprising the rubber composition according to [9].

[0025]

[11] A method for producing a copolymer according to any one of [1] to [8], comprising the following steps:

[0026] Ethylene, an α-olefin compound having 6 or more carbon atoms, a non-conjugated diene compound and an aromatic vinyl compound are copolymerized.

[0027]

[12] A method for producing a copolymer according to any one of [3] to [5], comprising:

[0028] A step A of copolymerizing ethylene, an α-olefin compound having 6 or more carbon atoms, a non-conjugated diene compound, and an aromatic vinyl compound to obtain a prepolymer corresponding to a main chain portion; and

[0029] A step B is to graft-polymerize the prepolymer obtained in the step A with a conjugated diene compound to introduce a branched portion.

[0030] Effects of the Invention

[0031] According to the present disclosure, a rubber component having excellent anti-degradation characteristics and a method for producing the same can be provided.

[0032] Furthermore, according to the present disclosure, using such a rubber component, a rubber composition and a tire having excellent anti-degradation characteristics can be provided. DETAILED DESCRIPTION

[0033] Hereinafter, the copolymer, the rubber composition, the tire, and the method for producing the copolymer of the present disclosure are described in detail with reference to the embodiments of the present disclosure.

[0034] In the present specification, regarding a copolymer or the like, unless otherwise specified, "X unit" means a unit derived from a compound "X" as a monomer.

[0035] The compounds described in this specification may be partially or completely derived from fossil resources, biological resources such as plant resources, or renewable resources such as used tires, etc. They may also be derived from a mixture of two or more of fossil resources, biological resources or renewable resources.

[0036] <Copolymer>

[0037] The copolymer of one embodiment of the present disclosure (hereinafter sometimes referred to as "copolymer A of the present embodiment") includes ethylene units, α-olefin units having 6 or more carbon atoms, non-conjugated diene units, and aromatic vinyl units. Since the copolymer A of the present embodiment contains at least 4 predetermined monomer units in this way, it can exhibit high anti-degradation characteristics.

[0038] The copolymer A of the present embodiment can be produced according to the following method for producing a copolymer.

[0039] As described above, the copolymer A of the present embodiment has at least ethylene units. These ethylene units are units derived from ethylene as a monomer.

[0040] The proportion of ethylene units in the copolymer A is preferably 75 mol% or less. When the proportion of ethylene units in the copolymer A is 75 mol% or less, the flexibility as a rubber is not impaired. From the same viewpoint, the proportion of ethylene units in the copolymer A is more preferably 70 mol% or less, and even more preferably 65 mol% or less. The proportion of ethylene units in the copolymer A is not particularly limited, but may be 10 mol% or more, 15 mol% or more, or 20 mol% or more.

[0041] The copolymer A of the present embodiment has at least α-olefin units. These α-olefin units are units derived from α-olefin compounds with more than 6 carbon atoms as monomers. By using α-olefin compounds with more than 6 carbon atoms, the gelation between copolymers and the re-crosslinking of sulfur after vulcanization can be significantly suppressed. The example of α-olefin compounds with more than 6 carbon atoms includes 4-methyl-1-pentene, 3-methyl-1-pentene, 1-hexene, 1-heptene, 1-octene, 1-nonene, 1-decene, 1-undecene, 1-dodecene, 1-tridecene, 1-tetradecene, 1-pentadecene, 1-hexadecene, 1-heptadecene and 1-octadecene. One of α-olefin units (α-olefin compounds) can be used alone, or a combination of two or more of these can be used. The α-olefin compound is not particularly limited, but is preferably an α-olefin compound with less than 20 carbon atoms. In particular, from the viewpoint of more reliably obtaining the desired effect and more easily synthesizing the copolymer, the α-olefin unit preferably includes at least one of 1-octene unit, 1-dodecene unit and 1-octadecene unit, and the α-olefin unit more preferably includes 1-octene unit.

[0042] The ratio of the α-olefin units in the copolymer A of the present embodiment is preferably 20 mol% or more. When the ratio of the α-olefin units in the copolymer A is 20 mol% or more, the above-mentioned gelation and re-crosslinking can be more effectively suppressed. From the same viewpoint, the ratio of the α-olefin units in the copolymer A is more preferably 25 mol% or more, and even more preferably 30 mol% or more. The ratio of the α-olefin units in the copolymer A is not particularly limited, but may be 60 mol% or less, 55 mol% or less, or 50 mol% or less.

[0043] The copolymer A of the present embodiment has at least non-conjugated diene units. These non-conjugated diene units are units derived from non-conjugated diene compounds as monomers. By having such non-conjugated diene units, a carbon-carbon double bond is left per unit in the copolymer, which can become a reaction point with sulfur. Examples of non-conjugated diene compounds include 5-ethylidene-2-norbornene, dicyclopentadiene, 1,4-hexadiene, cyclooctadiene, 5-vinyl-2-norbornene, 4,8-dimethyl-1,4,8-decadiene and 4-ethylidene-8-methyl-1,7-nonadiene. One of the non-conjugated diene units (non-conjugated diene compounds) can be used alone, or a combination of two or more of these can be used. In particular, from the viewpoint of more reliably obtaining the desired effect, the non-conjugated diene unit preferably includes a 5-ethylidene-2-norbornene unit.

[0044] The ratio of the non-conjugated diene units in the copolymer A of the present embodiment is preferably 1.0 mol% or more. When the ratio of the non-conjugated diene units in the copolymer A is 1.0 mol% or more, sulfur vulcanization can be fully promoted. From the same point of view, the ratio of the non-conjugated diene units in the copolymer A is more preferably 1.5 mol% or more, and even more preferably 2.0 mol% or more. The ratio of the non-conjugated diene units in the copolymer A is not particularly limited, but from the viewpoint of further improving the anti-degradation characteristics, it can be 10 mol% or less, 8 mol% or less, or 5 mol% or less.

[0045] The copolymer A of the present embodiment has at least an aromatic vinyl unit. These aromatic vinyl units are units derived from aromatic vinyl compounds as monomers. Aromatic vinyl compounds refer to aromatic compounds substituted with at least vinyl. Examples of aromatic vinyl compounds include styrene, α-methylstyrene, 2-methylstyrene (o-methylstyrene), 3-methylstyrene (m-methylstyrene), 4-methylstyrene (p-methylstyrene), 2,4-dimethylstyrene, 2-ethylstyrene, 3-ethylstyrene and 4-ethylstyrene. One of the aromatic vinyl units (aromatic vinyl compounds) can be used alone, or a combination of two or more of these can be used. From the point of view of more effectively improving the degradation resistance, the aromatic vinyl compound is preferably an aromatic vinyl compound with a substituted vinyl. In addition, from the point of view of more reliably obtaining the desired effect and easily introducing a branched chain during the manufacture of copolymer A1 (described later), the aromatic vinyl compound preferably has an alkyl group (such as methyl, ethyl, propyl, butyl, etc.). From the same point of view, the aromatic vinyl compound preferably does not include styrene. In particular, from the same point of view, the aromatic vinyl unit more preferably includes a 4-methylstyrene unit.

[0046] The proportion of the aromatic vinyl unit in the copolymer A of the present embodiment is preferably 0.5 mol% or more. When the proportion of the non-conjugated diene unit in the copolymer A is 0.5 mol% or more, the degradation resistance can be further improved. From the same point of view, the proportion of the aromatic vinyl unit in the copolymer A is more preferably 0.8 mol% or more, and even more preferably 1 mol% or more. The proportion of the aromatic vinyl unit in the copolymer A is not particularly limited, but can be 5 mol% or less, 3 mol% or less, or 2 mol% or less.

[0047] The copolymer A of the present embodiment may have other units in addition to the above-mentioned units. However, from the viewpoint of more reliably obtaining the desired effect, the ratio of other units in the copolymer A is preferably 5 mol% or less, more preferably 2 mol% or less, and even more preferably substantially 0 mol% (excluding such other units).

[0048] In a preferred example of this embodiment, in copolymer A, the proportion of ethylene units is 75 mol% or less, the proportion of α-olefin units is 20 mol% or more, the proportion of non-conjugated diene units is 1.0 mol% or more, and the proportion of aromatic vinyl units is 0.5 mol% or more.

[0049] The number average molecular weight (Mn) of the copolymer A in the present embodiment is preferably 100,000 or more. When the number average molecular weight (Mn) of the copolymer A is 100,000 or more, the crosslinking ability is improved. From the same point of view, the number average molecular weight (Mn) of the copolymer A is more preferably 150,000 or more, and even more preferably 200,000 or more. The number average molecular weight (Mn) of the copolymer A is not particularly limited, but is preferably 600,000 or less, and more preferably 500,000 or less.

[0050] The weight average molecular weight (Mw) of copolymer A in the present embodiment is preferably 200,000 or more. When the weight average molecular weight (Mw) of copolymer A is 200,000 or more, the crosslinking ability is improved. From the same point of view, the weight average molecular weight (Mw) of copolymer A is more preferably 400,000 or more. The weight average molecular weight (Mw) of copolymer A is not particularly limited, but is preferably 800,000 or less, more preferably 600,000 or less.

[0051] The molecular weight distribution (Mw / Mn) of copolymer A in the present embodiment is preferably 4.0 or less. When the molecular weight distribution (Mw / Mn) of copolymer A is 4.0 or less, sufficient homogeneity of the physical properties of the copolymer can be achieved. From the same point of view, the molecular weight distribution (Mw / Mn) of copolymer A is more preferably 3.5 or less, and even more preferably 3.0 or less. The molecular weight distribution (Mw / Mn) of copolymer A is not particularly limited, but is preferably 1.5 or more, and more preferably 1.8 or more.

[0052] The above number average molecular weight (Mn), weight average molecular weight (Mw) and molecular weight distribution (Mw / Mn) are determined by gel permeation chromatography (GPC) using polystyrene as a standard substance.

[0053] <Copolymer of a Preferred Aspect>

[0054] Next, a copolymer of a preferred aspect included within the scope of the above-mentioned "Copolymer A of the present embodiment" will be described. This copolymer (hereinafter sometimes referred to as "Copolymer A1") comprises a main chain portion having ethylene units, α-olefin units having 6 or more carbon atoms, non-conjugated diene units and aromatic vinyl units, and a side chain portion having a conjugated diene unit bonded to the main chain portion. In other words, this copolymer A1 can be referred to as a graft polymer. By introducing a side chain having a conjugated diene unit into a main chain having at least four predetermined monomer units, the copolymer A1 of the present embodiment can have excellent low loss properties while exhibiting high degradation resistance.

[0055] The copolymer A1 of the present embodiment can be produced according to the method for producing a copolymer of the present disclosure described below.

[0056] (Main chain part)

[0057] As described above, the main chain portion of the copolymer A1 of the present embodiment has at least ethylene units. These ethylene units are units derived from ethylene as a monomer.

[0058] The ratio of the ethylene units in the main chain portion of the copolymer A1 of the present embodiment is preferably 75mol% or less. When the ratio of the ethylene units in the main chain portion is 75mol% or less, the flexibility as a rubber will not be impaired. From the same viewpoint, the ratio of the ethylene units in the main chain portion is more preferably 70mol% or less, and even more preferably 65mol% or less. The ratio of the ethylene units in the main chain portion is not particularly limited, but it can be more than 10mol%, more than 15mol%, or more than 20mol%.

[0059] The main chain portion of the copolymer A1 of the present embodiment has at least α-olefin units. The specific description of these α-olefin units is the same as the aforementioned description of the copolymer A, so it is omitted. The proportion of the α-olefin units in the main chain portion of the copolymer A1 of the present embodiment is preferably 20mol% or more. When the proportion of the α-olefin units in the main chain portion is 20mol% or more, the above-mentioned gelation and re-crosslinking can be more effectively suppressed. From the same point of view, the proportion of the α-olefin units in the main chain portion is more preferably 25mol% or more, and even more preferably 30mol% or more. The proportion of the α-olefin units in the main chain portion is not particularly limited, but it can be 60mol% or less, 55mol% or less, or 50mol% or less.

[0060] The main chain portion of the copolymer A1 of the present embodiment has at least a non-conjugated diene unit. The specific description of these non-conjugated diene units is the same as the aforementioned description of copolymer A, so it is omitted. The ratio of the non-conjugated diene units in the main chain portion of the copolymer A1 of the present embodiment is preferably more than 1.0mol%. When the ratio of the non-conjugated diene units in the main chain portion is more than 1.0mol%, sulfur vulcanization can be fully promoted. From the same point of view, the ratio of the non-conjugated diene units in the main chain portion is more preferably more than 1.5mol%, and even more preferably more than 2.0mol%. The ratio of the non-conjugated diene units in the main chain portion is not particularly limited, but from the point of view of further improving the anti-degradation characteristics, it can be less than 10mol%, less than 8mol%, or less than 5mol%.

[0061] The main chain portion of the copolymer A1 of the present embodiment has at least an aromatic vinyl unit. The specific description of these aromatic vinyl units is the same as the aforementioned description of copolymer A, so it is omitted. The ratio of the aromatic vinyl unit in the main chain portion of the copolymer A1 of the present embodiment is preferably 0.5mol% or more. When the ratio of the non-conjugated diene unit in the main chain portion is 0.5mol% or more, the degradation resistance can be further improved. From the same point of view, the ratio of the aromatic vinyl unit in the main chain portion is more preferably 0.8mol% or more, and even more preferably 1mol% or more. The ratio of the aromatic vinyl unit in the main chain portion is not particularly limited, but it can be less than 5mol%, less than 3mol%, or less than 2mol%.

[0062] The main chain portion of the copolymer A1 of the present embodiment may have other units in addition to the above-mentioned units. However, from the viewpoint of more reliably obtaining the desired effect, the proportion of other units in the main chain portion is preferably 5 mol% or less, more preferably 2 mol% or less, and even more preferably substantially 0 mol% (excluding such other units).

[0063] In a preferred example of this embodiment, in the main chain portion of copolymer A1, the proportion of ethylene units is 75 mol% or less, the proportion of α-olefin units is 20 mol% or more, the proportion of non-conjugated diene units is 1.0 mol% or more, and the proportion of aromatic vinyl units is 0.5 mol% or more.

[0064] (Branch part)

[0065] In addition, the copolymer A1 of the present embodiment has a side chain portion having a conjugated diene unit, which is bonded to the above-mentioned main chain portion. These conjugated diene units are units derived from conjugated diene compounds as monomers. Conjugated diene compounds, for example, preferably have 4 to 10 carbon atoms, and specific examples include 1,3-butadiene, isoprene, 1,3-pentadiene, 2,3-dimethylbutadiene and myrcene. One of the conjugated diene units (conjugated diene compounds) can be used alone, or a combination of two or more of these can be used. In particular, from the viewpoint of more reliably obtaining the desired effect and being easily available, the conjugated diene unit preferably includes a 1,3-butadiene unit or an isoprene unit, and more preferably includes a 1,3-butadiene unit.

[0066] The branched portion of the copolymer A1 of the present embodiment may have other units in addition to the conjugated diene unit. However, from the viewpoint of more reliably obtaining the desired effect, the proportion of other units in the branched portion is preferably 5 mol% or less, more preferably 2 mol% or less, and even more preferably substantially 0 mol% (excluding such other units).

[0067] In the copolymer A1 of the present embodiment, the ratio of the branched portion is preferably 1% by mass or more. In other words, in the copolymer A1 of the present embodiment, the ratio of the main chain portion is preferably 99% by mass or less. In this case, sufficient crosslinking (vulcanization) ability can be exhibited while improving low loss properties. From the same point of view, the ratio of the branched portion in the copolymer A1 is more preferably 3% by mass or more, and even more preferably 5% by mass or more. The ratio of the branched portion in the copolymer A1 is not particularly limited, but from the point of view of maintaining good anti-deterioration properties, it is preferably 20% by mass or less, more preferably 15% by mass or less, and may also be 10% by mass or less.

[0068] The ratio of the branched moiety in the copolymer A1 can be determined from the degree of increase in the weight average molecular weight (Mw) before and after the branched moiety is introduced during the production of the copolymer A1.

[0069] In a preferred example of the present embodiment, the weight average molecular weight of the copolymer A1 is 200,000 or more and the ratio of the branched portion in the copolymer A1 is 1% by mass or more.

[0070] <Method for producing copolymer>

[0071] A method for producing a copolymer according to one embodiment of the present disclosure (hereinafter sometimes referred to as "the production method according to the present embodiment") is a method for producing the above-mentioned copolymer A, which includes a step (copolymerization step) of copolymerizing ethylene, an α-olefin compound having 6 or more carbon atoms, a non-conjugated diene compound and an aromatic vinyl compound.

[0072] According to the production method of this embodiment, a copolymer A (rubber component) having excellent degradation resistance can be produced. If necessary, the production method of this embodiment may further include a coupling process, a washing process, and other processes after the copolymerization process.

[0073] In the copolymerization step, ethylene, one or more α-olefin compounds having 6 or more carbon atoms, one or more non-conjugated diene compounds and one or more aromatic vinyl compounds are copolymerized to obtain a copolymer A having at least ethylene units, α-olefin units, non-conjugated diene units and aromatic vinyl units. In the copolymerization step, other monomers may or may not be used as monomers.

[0074] Ethylene can be introduced into the reaction system in a gas phase while adjusting the pressure.

[0075] The copolymerization process can be carried out by any method that allows the copolymerization of the individual monomers. However, from the viewpoint of promoting the copolymerization reaction, it is preferred to carry out the copolymerization process in the presence of a catalyst composition containing a metal complex represented by the following general formula (I):

[0076] [Chemical formula 1]

[0077]

[0078] In the formula, M represents a Group 4 element, Cp represents a substituted or unsubstituted cyclopentadienyl, indenyl, or fluorenyl group, and R 1 , R 2 and R 3 Each independently represents a hydrocarbon group, and X 1 and X 2 Each independently represents a halogen atom, a hydrogen atom, an amino group, or a hydrocarbon group.

[0079] The Group 4 elements represented by M in the general formula (I) include titanium (Ti), zirconium (Zr), hafnium (Hf) and (rutherfordium)(Rf). Among them, titanium (Ti) is preferred.

[0080] Cp in the general formula (I) is preferably an unsubstituted cyclopentadienyl group, an indenyl group, or a fluorenyl group, and more preferably an unsubstituted cyclopentadienyl group.

[0081] In the general formula (I), R 1 , R 2 and R 3 Examples of the hydrocarbon groups represented by include, for example, straight-chain or branched aliphatic hydrocarbon groups such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, neopentyl, hexyl and octyl; aromatic hydrocarbon groups such as phenyl, tolyl and naphthyl; and aralkyl groups such as benzyl. 1 and R 2 It is preferably a hydrocarbon group having 1 to 6 carbon atoms, more preferably a straight-chain or branched aliphatic hydrocarbon group, even more preferably a methyl group, an ethyl group, or a tert-butyl group, and further preferably a methyl group. 3 It is preferably a hydrocarbon group having 1 to 6 carbon atoms, more preferably a linear or branched aliphatic hydrocarbon group, even more preferably a methyl group, an ethyl group, or a tert-butyl group, and further preferably a tert-butyl group.

[0082] In the general formula (I), X 1 and X 2 Examples of the halogen atom represented by include, for example, a fluorine atom, a chlorine atom, a bromine atom and an iodine atom.

[0083] In the general formula (I), X 1 and X 2 Examples of the amino group represented include, for example, aliphatic amino groups such as dimethylamino, diethylamino and diisopropylamino; arylamino groups such as phenylamino, 2,6-di-tert-butylphenylamino, 2,6-diisopropylphenylamino, 2,6-dineopentylphenylamino, 2-tert-butyl-6-isopropylphenylamino, 2-tert-butyl-6-neopentylphenylamino, 2-isopropyl-6-neopentylphenylamino and 2,4,6-tri-tert-butylphenylamino; and bistrialkylsilylamino groups such as bistrimethylsilylamino.

[0084] In the general formula (I), X 1 and X 2 Examples of the hydrocarbon groups represented include, for example, straight-chain or branched aliphatic hydrocarbon groups such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, neopentyl, hexyl and octyl; aromatic hydrocarbon groups such as phenyl, tolyl and naphthyl; and aralkyl groups such as benzyl.

[0085] Among them, X 1 and X 2 A chlorine atom or a dimethylamino group is preferred.

[0086] In the above copolymerization process, any method can be used, such as solution polymerization, suspension polymerization, liquid phase bulk polymerization, emulsion polymerization, gas phase polymerization, or solid phase polymerization. When a solvent is used in the polymerization reaction, any solvent can be used as long as it is inert in the polymerization reaction, and examples include toluene, cyclohexane and hexane (n-hexane).

[0087] In the copolymerization step, the polymerization reaction is preferably performed in an atmosphere of an inert gas, and the inert gas is preferably nitrogen or argon.

[0088] The polymerization temperature of the polymerization reaction is not particularly limited. The polymerization temperature is preferably in the range of, for example, -100°C to 200°C, and may be approximately room temperature.

[0089] In addition, in order to allow sufficient raw material monomers to enter the polymerization reaction system, the polymerization reaction pressure is preferably 0.1 to 10.0 MPa. The reaction time of the polymerization reaction is not particularly limited. The reaction time is preferably in the range of, for example, 1 second to 10 days, although the reaction time can be appropriately selected according to conditions such as the type of polymerization catalyst and the polymerization temperature.

[0090] In the copolymerization process, a polymerization terminator such as methanol, ethanol or isopropanol may be used to stop the polymerization reaction.

[0091] The coupling step is a step of performing a coupling reaction to modify at least a portion (for example, a terminal) of the obtained copolymer. The number average molecular weight (Mn) can be increased by performing the coupling reaction.

[0092] The coupling step is preferably carried out when the polymerization reaction reaches 100%.

[0093] The coupling agent used in the coupling reaction is not particularly limited and can be appropriately selected according to the purpose. Examples thereof may include: tin-containing compounds such as bis(maleic acid-1-octadecyl) dioctyltin (IV); isocyanate compounds such as 4,4'-diphenylmethane diisocyanate; and alkoxysilane compounds such as glycidylpropyltrimethoxysilane. These can be used alone or in combination of two or more. Among them, from the viewpoint of its high reaction efficiency and low gel formation, bis(maleic acid-1-octadecyl) dioctyltin (IV) is preferred.

[0094] The cleaning process is a process for cleaning the obtained copolymer. The cleaning process can appropriately reduce the amount of catalyst residue in the copolymer. The medium used in the cleaning process is not particularly limited and can be appropriately selected according to the purpose. Examples of the medium include methanol, ethanol and isopropanol.

[0095] <Method for producing a copolymer (copolymer A1) in a preferred aspect>

[0096] Next, a method for producing a copolymer A1 which is basically included in the scope of the above-mentioned "production method of the present embodiment" will be described. The production method includes: a step A of copolymerizing ethylene, an α-olefin compound having 6 or more carbon atoms, a non-conjugated diene compound, and an aromatic vinyl compound to obtain a prepolymer corresponding to the main chain portion; and

[0097] A step B is to graft-polymerize the prepolymer obtained in the step A with a conjugated diene compound to introduce a branched portion.

[0098] According to this production method, the copolymer A1 (rubber component) having excellent anti-degradation characteristics and low loss properties can be produced.

[0099] In step A, ethylene, one or more α-olefins having 6 or more carbon atoms, one or more non-conjugated diene compounds, and one or more aromatic vinyl compounds are copolymerized to obtain a prepolymer corresponding to the main chain portion of a copolymer having at least ethylene units, α-olefin units, non-conjugated diene units, and aromatic vinyl units. In step A, other monomers may or may not be used.

[0100] Since the operation in step A (main chain forming step) is basically the same as the copolymerization step in the "production method of this embodiment", the description thereof is omitted. The prepolymer obtained in step A is basically the same as copolymer A.

[0101] Next, in step B, the prepolymer obtained in step A is graft polymerized with one or more conjugated diene compounds to introduce a branched portion having a conjugated diene unit. In this way, copolymer A1 (graft polymer) is obtained. In step B, other monomers may or may not be used.

[0102] Step B (branch portion formation step) can be performed by any method that allows graft polymerization of the prepolymer and the conjugated diene compound. However, from the viewpoint of promoting graft polymerization, step B is preferably performed by anionic polymerization.

[0103] In anionic polymerization, lithium compounds are preferably used as polymerization initiators. Examples of lithium compounds include ethyl lithium, n-propyl lithium, isopropyl lithium, n-butyl lithium, sec-butyl lithium, tert-octyl lithium, n-decyl lithium, phenyl lithium, 2-naphthyl lithium, 2-butylphenyl lithium, 4-phenylbutyl lithium, cyclohexyl lithium, cyclopentyl lithium, and the reaction product of diisopropenylbenzene and butyl lithium.

[0104] In addition, amide lithium compounds can also be used as polymerization initiators in anionic polymerization. Examples of amide lithium compounds include hexamethylene imide lithium, pyrrolidine lithium, piperidine lithium, heptamethylene imide lithium, dodecamethylene imide lithium, dimethyl amide lithium, diethyl amide lithium, dipropyl amide lithium, dibutyl amide lithium, dihexyl amide lithium, diheptyl amide lithium, dioctyl amide lithium, di-2-ethylhexyl amide lithium, didecyl amide lithium, N-methylpiperazine lithium, ethylpropyl amide lithium, ethylbutyl amide lithium, methylbutyl amide lithium, ethylbenzyl amide lithium and methylphenethyl amide lithium.

[0105] Using less initiator results in longer branched portions, while using more initiator results in shorter branched portions. Therefore, the amount of polymerization initiator used can be appropriately adjusted according to the desired length of the branched portion.

[0106] In step B, any method such as solution polymerization, suspension polymerization, liquid phase bulk polymerization, emulsion polymerization, gas phase polymerization, or solid phase polymerization can be used. When a solvent is used in the polymerization reaction, any solvent can be used as long as it is inert in the polymerization reaction, and examples include toluene, cyclohexane, and hexane (n-hexane).

[0107] In step B, the polymerization reaction is preferably carried out in an atmosphere of an inert gas, preferably nitrogen or argon.

[0108] The polymerization temperature of the polymerization reaction is not particularly limited. The polymerization temperature is preferably in the range of, for example, -100°C to 200°C, and may be approximately room temperature.

[0109] In addition, in order to allow sufficient raw material monomers to enter the polymerization reaction system, the polymerization reaction pressure is preferably 0.1 to 10.0 MPa. The reaction time of the polymerization reaction is not particularly limited. The reaction time is preferably in the range of, for example, 1 second to 10 days, although the reaction time can be appropriately selected according to conditions such as the type of polymerization catalyst and the polymerization temperature.

[0110] In step B, a polymerization terminator such as methanol, ethanol or isopropanol may be used to stop the polymerization reaction.

[0111] After step B, a coupling step, a washing step, and other steps may be performed, if necessary. Detailed description of these steps is omitted because they are the same as those previously described in "Production method of the present embodiment".

[0112] <Rubber Composition>

[0113] The rubber composition of the present disclosure includes the above-mentioned copolymer A. Because the rubber composition of the present disclosure includes the above-mentioned copolymer A, its anti-degradation characteristics are excellent. In particular, when copolymer A1 is used as copolymer A, the rubber composition not only has excellent anti-degradation characteristics, but also shows excellent low loss. In addition to copolymer A, the rubber composition of the present disclosure may include other rubber components, fillers, crosslinking agents and other components.

[0114] Examples of other rubber components include natural rubber (NR), polyisoprene rubber (IR), polybutadiene rubber (BR), acrylonitrile-butadiene rubber (NBR), chloroprene rubber, ethylene-propylene rubber (EPM), ethylene-propylene-diene rubber (EPDM), polysulfide rubber, silicone rubber, fluororubber and polyurethane rubber. These can be used alone or in combination of two or more.

[0115] Examples of fillers include carbon black, silica, aluminum hydroxide, clay, aluminum oxide, talc, mica, kaolin, glass balls, glass beads, calcium carbonate, magnesium carbonate, magnesium hydroxide, magnesium oxide, titanium oxide, potassium titanate and barium sulfate. These can be used alone or in combination of two or more. Among them, carbon black is preferably used as a filler. The content (compounding amount) of the filler in the rubber composition is not particularly limited and can be appropriately selected according to its purpose. However, the content is preferably 10 to 100 parts by mass per 100 parts by mass of the rubber component. When the content of the filler is 10 parts by mass or more, improved reinforcement is achieved by including the filler; when the content is 100 parts by mass or less, good workability is maintained. From the same point of view, the content of the filler is more preferably 20 parts by mass or more, even more preferably 30 parts by mass or more, and preferably 80 parts by mass or less, even more preferably 60 parts by mass or less, per 100 parts by mass of the rubber component.

[0116] Examples of crosslinking agents include sulfur-based crosslinking agents, organic peroxide-based crosslinking agents, inorganic crosslinking agents, polyamine crosslinking agents, resin crosslinking agents, sulfur compound-based crosslinking agents, and oxime-nitrosamine-based crosslinking agents. Among them, sulfur-based crosslinking agents (vulcanizing agents) are more preferably used in tire rubber compositions. The content (compounding amount) of the crosslinking agent in the rubber composition is not particularly limited and can be appropriately selected according to the purpose, but the content is preferably 0.1 to 20 parts by mass per 100 parts by mass of the rubber component.

[0117] When the above-mentioned vulcanizing agent is used, a vulcanization accelerator may be further used. Examples of the vulcanization accelerator include guanidine-based, aldehyde-amine-based, aldehyde-ammonia-based, thiazole-based, sulfenamide-based, thiourea-based, thiuram-based, dithiocarbamate-based, and xanthate-based compounds. The vulcanization accelerator may be used alone or in combination of two or more thereof.

[0118] In addition, as required, the rubber composition of the present disclosure may include a softener, a vulcanization aid, a colorant, a flame retardant, a lubricant, a foaming agent, a plasticizer, a processing aid, an antioxidant, an anti-aging agent, a scorch protection agent, an ultraviolet protection agent, an antistatic agent, an anti-coloring agent, and other well-known compounding agents according to the purpose of use.

[0119] In addition to the tires described below, the rubber composition of the present disclosure can also be used for other applications such as vibration-damping rubber, vibration-isolating rubber, belts such as conveyor belts, rubber tracks, and various hoses.

[0120] <Tires>

[0121] The tire of the present disclosure includes the above-mentioned rubber composition. In other words, the tire of the present disclosure is characterized in that it includes the above-mentioned rubber composition. Because the tire of the present disclosure includes the above-mentioned copolymer A, its anti-degradation characteristics are excellent. In particular, when copolymer A1 is used as copolymer A, the tire not only has excellent anti-degradation characteristics, but also exhibits excellent low loss.

[0122] The application site of the rubber composition of the present disclosure in the tire is not particularly limited and can be appropriately selected according to the purpose. Examples include treads, base treads, sidewalls, sidewall reinforcing rubbers, and bead fillers, but the sidewalls are particularly preferred.

[0123] The method for manufacturing the above tire may be a conventional method. For example, a desired tire such as a pneumatic tire may be manufactured by sequentially stacking components commonly used in tire production such as a carcass layer, a belt layer, a tread layer, etc. made of an unvulcanized rubber composition and / or cords on a tire forming drum; removing the drum to obtain a green tire; and heating and vulcanizing the green tire according to a conventional method.

[0124] Example

[0125] Hereinafter, the present disclosure will be described in more detail with reference to Examples, but the present disclosure is not limited to these Examples.

[0126] (Synthesis of Copolymer A)

[0127] The following catalyst (metal complex) was used for the synthesis of copolymer A.

[0128] [Chemical formula 2]

[0129]

[0130] 600g of toluene, 62g of 1-octene as an α-olefin compound having more than 6 carbon atoms, 13g of 5-ethylidene-2-norbornene as a non-conjugated diene compound, and 5g of 4-methylstyrene as an aromatic vinyl compound were loaded into a fully dried 2000mL pressure-resistant stainless steel reactor. Then, 6mL of modified aluminoxane (Al=5.6% by mass in hexane solution) was added, and ethylene as a non-conjugated olefin compound was introduced for 5 minutes at 0.1MPa and room temperature. 3μmol of the above catalyst (as 10mL of toluene solution) was added to the reactor, and copolymerization was carried out at 50°C for 80 minutes, while ethylene was pressed into ethylene at 0.2MPa.

[0131] After the copolymerization, 10 mL of an isopropanol solution was added to the reactor to stop the reaction, and the copolymer was separated using a large amount of methanol and vacuum dried at 50° C. to obtain a copolymer A. The yield of the obtained copolymer A was 35 g.

[0132] Using monodisperse polystyrene as a reference, gel permeation chromatography [GPC: HLC-8121GPC / HT manufactured by Tosoh Corporation, columns: 2 GMH manufactured by Tosoh Corporation] was used. HR -H(S)HT, detector: differential refractometer (RI)] to obtain the number average molecular weight (Mn), weight average molecular weight (Mw) and molecular weight distribution (Mw / Mn) of the obtained copolymer A in terms of polystyrene. Note that the measurement temperature is 40° C. The Mn of the obtained copolymer A is 220,000, the Mw is 480,000, and the molecular weight distribution is 2.2.

[0133] pass 1 The ratio of each monomer unit in the obtained copolymer A was determined from the integrated ratio of each peak in the H-NMR spectrum (100° C., d-tetrachloroethane standard: 6 ppm). As a result, it was found that in the copolymer A, the ratio of the ethylene unit was 60.5 mol% (27.5 mass%), the ratio of the 1-octene unit was 34.2 mol% (62.2 mass%), the ratio of the 5-ethylidene-2-norbornene unit was 4.1 mol% (8.0 mass%), and the ratio of the 4-methylstyrene unit was 1.2 mol% (2.3 mass%).

[0134] (Synthesis of Copolymer A1 (Graft Polymer))

[0135] The main chain part (prepolymer) was obtained by the same procedure as the synthesis of copolymer A. The main chain part (prepolymer) was substantially the same as the above-mentioned copolymer A.

[0136] Next, 22.5 g of the main chain part (prepolymer) obtained above and 250 g of cyclohexane were added to a fully dried 1000 mL glass reactor and dissolved for 24 hours. Then, 3.9 mL of tetramethylethylenediamine (1 M in cyclohexane solution) and 3.9 mL of sec-butyllithium (1 M in hexane solution) were added and aged at 50 ° C for 40 minutes. Then, 2.5 g of 1,3-butadiene (25 mass % in cyclohexane solution) as a conjugated diene compound was added, and a grafting reaction was performed at 50 ° C for 30 minutes.

[0137] After the reaction, 5 mL of a degassed isopropanol solution was added to a glass reactor to stop the reaction, and the product was separated using a large amount of methanol and vacuum dried at 50° C. to obtain a copolymer A1 (graft polymer) having an introduced branched portion containing a 1,3-butadiene unit. The yield of the obtained copolymer was 25 g.

[0138] Using monodisperse polystyrene as a reference, gel permeation chromatography [GPC: HLC-8121GPC / HT manufactured by Tosoh Corporation, columns: 2 GMH manufactured by Tosoh Corporation] was used. HR -H(S)HT, detector: differential refractometer (RI)] to obtain the number average molecular weight (Mn), weight average molecular weight (Mw) and molecular weight distribution (Mw / Mn) of the obtained copolymer A1 (grafted polymer) in terms of polystyrene. The Mn of the obtained copolymer A1 (grafted polymer) was 240,000, the Mw was 490,000, and the molecular weight distribution was 2.0. The proportion of the branched portion in the copolymer A1 (grafted polymer) was 10% by mass.

[0139] pass 1 The ratio of each monomer unit in the obtained copolymer A1 (graft polymer) was determined by the integrated ratio of each peak in the H-NMR spectrum (100° C., d-tetrachloroethane standard: 6 ppm). As a result, it was found that in the copolymer A1 (graft polymer), the ratio of ethylene units was 53.7 mol% (24.8 mass%), the ratio of 1-octene units was 30.4 mol% (56.0 mass%), the ratio of 5-ethylidene-2-norbornene units was 3.6 mol% (7.2 mass%), the ratio of 4-methylstyrene units was 1.1 mol% (2.1 mass%), and the ratio of 1,3-butadiene units was 11.2 mol% (10.0 mass%).

[0140] (Preparation of rubber composition)

[0141] According to the formulation listed in Table 1, a rubber composition was prepared by performing a primary kneading (non-masterbatch kneading, NR) and then a secondary kneading (masterbatch kneading, P). The rubber composition was vulcanized at 160° C. to obtain a vulcanized rubber composition. The obtained vulcanized rubber composition was evaluated as follows.

[0142] <Degradation resistance characteristics>

[0143] Ring test pieces were made from each vulcanized rubber composition, and tensile tests were carried out at 23°C according to JIS K 6251 to measure elongation at break Eb1 (%) and 100% tensile modulus M1001 (MPa). The vulcanized rubber composition was then placed in a 100°C oven for 2 days, and elongation at break Eb2 (%) and 100% tensile modulus M1002 (MPa) were measured in the same manner. The rate of change of Eb before and after thermal degradation was calculated as Eb2 / Eb1×100, and the rate of change of M100 before and after thermal degradation was calculated as M1002 / M1001×100. The results are listed in Table 1. Values ​​close to 100 indicate better anti-degradation properties (higher anti-degradation properties).

[0144] <Low loss>

[0145] The tan δ of each vulcanized rubber composition sample was measured in a torsion mode at a frequency of 15 Hz and a deformation change temperature of 1% using a dynamic mechanical analyzer (manufactured by TA Instruments). The tan δ value at 50°C of each sample was indexed, and the value of Comparative Example 1 was set to 100. The results are listed in Table 1. The smaller the index value, the better the low loss property and the less the hysteresis loss.

[0146] [Table 1]

[0147]

[0148] *1SBR: Manufactured by Asahi Kasei Corporation, “Tufdene 2000”

[0149] *2EPDM: manufactured by JSR Corporation, “JSR EP35”

[0150] *3 Carbon black: Manufactured by Tokai Carbon Co., Ltd., “Seast F”

[0151] *4 Stearic acid: manufactured by NOF Corporation, "Kiri-jirushi Stearic Acid"

[0152] *5 Zinc oxide: Two types of zinc oxide manufactured by Hakusui Tech Co., Ltd.

[0153] *6 Vulcanization accelerator A: manufactured by Sanshin Chemical Industry Co., Ltd., "Sanceler DM-TG"

[0154] *7 Vulcanization accelerator B: manufactured by Sanshin Chemical Industry Co., Ltd., "Sanceler NS-G"

[0155] *8 Sulfur: manufactured by Hosoi Chemical Industry Co., Ltd., "HK200-5"

[0156] From the results in Table 1, it can be understood that the examples using the copolymers of the present disclosure have higher degradation resistance characteristics, and the change rates of the elongation at break Eb and the 100% tensile modulus M100 before and after thermal degradation are smaller than those of the comparative examples using conventional rubber. In particular, it was found that the examples using the copolymer A1 (grafted polymer) not only exhibited high degradation resistance characteristics, but also exhibited excellent low loss properties.

[0157] Industrial Applicability

[0158] According to the present disclosure, a rubber component having excellent anti-degradation characteristics and a method for producing the same are provided.

[0159] Furthermore, according to the present disclosure, using such a rubber component, a rubber composition and a tire having excellent anti-degradation characteristics can be provided.

Claims

1. A copolymer comprising an ethylene unit, an α-olefin unit having 6 or more carbon atoms, a non-conjugated diene unit and an aromatic vinyl unit.

2. The copolymer according to claim 1, wherein the proportion of the ethylene unit is 75 mol% or less, the proportion of the α-olefin unit is 20 mol% or more, the proportion of the non-conjugated diene unit is 1.0 mol% or more, and the proportion of the aromatic vinyl unit is 0.5 mol% or more.

3. The copolymer according to claim 1, comprising: A main chain portion having an ethylene unit, an α-olefin unit having 6 or more carbon atoms, a non-conjugated diene unit and an aromatic vinyl unit, and A branch chain portion having a conjugated diene unit is bonded to the main chain portion.

4. The copolymer according to claim 3, wherein in the main chain portion, the proportion of the ethylene unit is 75 mol% or less, the proportion of the α-olefin unit is 20 mol% or more, the proportion of the non-conjugated diene unit is 1.0 mol% or more, and the proportion of the aromatic vinyl unit is 0.5 mol% or more. 5 . The copolymer according to claim 3 , wherein the weight average molecular weight of the copolymer is 200,000 or more, and the ratio of the branched portion in the copolymer is 1% by mass or more. The copolymer according to claim 1 or 3, which has a weight average molecular weight of 200,000 or more.

7. The copolymer according to claim 1 or 3, wherein the aromatic vinyl unit comprises a 4-methylstyrene unit.

8. The copolymer according to claim 1 or 3, which has a molecular weight distribution of 4.0 or less. 9 . A rubber composition comprising the copolymer according to claim 1 or 3 . 10 . A tire comprising the rubber composition according to claim 9 .

11. A method for producing a copolymer according to claim 1 or 2, comprising the following steps: Ethylene, an α-olefin compound having 6 or more carbon atoms, a non-conjugated diene compound and an aromatic vinyl compound are copolymerized.

12. A method for producing a copolymer according to claim 3 or 4, comprising: A step A of copolymerizing ethylene, an α-olefin compound having 6 or more carbon atoms, a non-conjugated diene compound, and an aromatic vinyl compound to obtain a prepolymer corresponding to the main chain portion; and A step B is to graft-polymerize the prepolymer obtained in the step A with a conjugated diene compound to introduce the branched portion.