Rotor blade, method for manufacturing rotor blade and gas turbine engine

By applying a directional surface and an oxidation-resistant multi-layer coating at the end of the rotor blade, combined with cathode arc evaporation technology, the problem of coatings easily oxidized and worn at high temperatures in the prior art is solved, and the sealing performance and efficiency of gas turbine engines are improved .

CN119013460APending Publication Date: 2024-11-22OERLIKON SURFACE SOLUTIONS AG PFAFFIKON
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380027848.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-16
Filing Date
2023-03-14
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The end coating of rotor blades in existing gas turbine engines is prone to oxidation and failure at high temperatures, and is severely damaged in friction and wear, affecting sealing performance and efficiency.

Method used

Using a rotor blade end coating with a directional surface, the coating includes an oxidation-resistant abrasive layer applied by cathode arc evaporation technology, combining MCrAlX intermediate layer and aluminum chromium oxide top layer to form a multi-layer coating for improved adhesion and wear resistance sex.

Benefits of technology

Significantly reduces the risk of coating shear and tear, reduces friction heat and wear, extends coating life, and improves the high temperature resistance and sealing properties of rotor blades.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119013460A_ABST
    Figure CN119013460A_ABST
Patent Text Reader

Abstract

The invention relates to a rotor blade (30) in a gas turbine engine (50), characterized in that the coating (10) on the blade tip (20) of the rotor blade (30) comprises an anti-oxidation abrasive layer (11), and the rotor blade tip (20) at least partially has an orientation surface (21) having a normal vector (22), the normal vector (22) has a component (23) in the direction of rotation (R) of the rotor blade. The invention also relates to a method of manufacturing said rotor blade (30) and to a gas turbine engine (50) having said rotor blade (30).
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The invention relates to a rotor blade in a gas turbine engine having the features according to claim 1 , a method for producing a rotor blade having the features according to claim 9 , and a gas turbine engine according to claim 12 .

[0002] In a gas turbine engine, the quality of the sealing system between rotating and stationary components strongly affects the efficiency of the gas turbine engine.

[0003] Therefore, it is important to maintain minimum clearances between rotating and stationary components during nominal operation and / or transient operation.It is known to achieve this by a combination of an abradable coating on the sealing segment of the turbine shroud and an abrasive coating on the rotor blade tips.

[0004] The abradable coating is typically porous and only weakly bonded, allowing the seal to be formed by having the abrasive rotor blade tip cut a track through the abradable coating during the first run.

[0005] Rotor blade tip coatings are also used to protect the rotor blade tips from wear and oxidation. Known rotor blade tip coatings consist of abrasive particles (e.g., cubic boron nitride) embedded in a matrix (e.g., MCrAlX). "M" stands for metal, primarily cobalt, nickel, or a cobalt-nickel alloy. "Cr" stands for chromium, "Al" stands for aluminum, and "X" stands for yttrium or hafnium.

[0006] According to the prior art, such coatings are applied by complex and cost-intensive processes, such as electrolytic or electrophoretic deposition (US 935407 A). Figure 1 shows a schematic diagram of a typical cross section of such a coating.

[0007] Rotor blade tip coatings achieved in this manner can exhibit poor layer adhesion. In these coating processes, the energy input is relatively low, and there is virtually no interdiffusion at the interface between the coating and the substrate. Interdiffusion typically ensures strong chemical bonding or adhesion. Consequently, during blade rotation, due to high centrifugal forces, failure and delamination of entire layers or abrasive particles can occur.

[0008] Furthermore, neither the abrasive particles nor the matrix used in the prior art are resistant to oxidation at high temperatures and can fail due to oxidation. The abrasive particles typically used have a particle size on the order of the layer thickness and can therefore extend from the surface to the interface between the coating and the substrate. If the particles oxidize, the blade material or the corresponding interface can be susceptible to rapid oxidation attack. Furthermore, the matrix used in the prior art is susceptible to creep at high temperatures, becoming too soft to anchor the hard abrasive particles.

[0009] Therefore, there is a need for improvements in the design and manufacturing methods of rotor blades.

[0010] This problem is solved by a rotor blade in a gas turbine engine, the rotor blade having a coating on a blade tip of the rotor blade, the coating including an oxidation-resistant abrasive layer, and the rotor blade tip at least partially having an orientation surface having a normal vector having a component in the direction of rotation of the rotor blade. Such a rotor blade tip includes an orientation surface positioned in a specific relationship to the direction of rotation.

[0011] An advantage of a rotor blade tip having such a directional surface is that, when cutting into abradable material, the force distribution on the rotor blade tip is nearly orthogonal to the coating of the rotor blade tip. This reduces the risk of shearing or tearing the coating, as can occur with prior art rotor blades due to transverse forces along the coating. Furthermore, the force and friction are distributed over a larger area, thereby reducing frictional heat and wear.

[0012] This advantage also applies to rotor blades with coatings produced using other methods (such as PVD). PVD coatings have stronger adhesion, oxidation resistance and wear resistance. In particular, cathodic arc evaporation technology is particularly suitable for applying rotor blade tip coatings for the following reasons: higher energy input of ions can be achieved through cathodic arc evaporation technology, which contributes to strong layer adhesion and dense coating structure; cathodic arc evaporation technology can achieve the deposition of various materials and their combinations, and can achieve precise layer structures, thereby achieving unique coating properties. By designing the coating material and adjusting the coating parameters, the coating can be adapted to different substrate materials and application requirements. Cathodic arc evaporation technology is widely used in industry due to its high coating rate and production safety.

[0013] However, the tip friction behavior of PVD- and electrolytically coated rotor blade tips differs. For electrolytically coated rotor blade tips, as shown in Figure 1, hard, extruded cubic boron nitride abrasive particles are embedded in an MCrAlX matrix on the flat rotor blade tip. These particles cut into the abradable coating through localized contact between the particle's sharp corners and facets. PVD coating, on the other hand, applies the abrasive coating along the contour of the flat rotor blade tip, resulting in complete contact between the entire coated rotor blade tip surface and the abradable coating.

[0014] Due to the greater contact area between the coated rotor blade tip and the abradable coating, PVD coatings generate much higher friction (and therefore frictional heat) during abrasive events than electrolytically coated blade tips. However, these thermal properties are a reason why PVD coatings on rotor blade tips can fail. High temperatures have been shown to significantly increase the wear of multilayer CrAlNPVD-coated flat rotor blade tips (Watson, M., Fois, N. and Marshall, MB (2015) Effects of blade surface treatments in tip-shroud abradable contacts. In Wear, vol. 338-33, 15 September 2015, pp. 268-281, ISSN 1873-2577). It has been reported that due to the poor high-temperature tribological properties of CR(Al)N PVD coatings, portions of the coating tear off and become lodged in the abradable material. These hard particles in the abradable material resist abrasion and cause the rotor blade tip to wear much faster, wearing through the coating and exposing the underlying substrate to oxidation. In this study, the rotor blade tip was also chamfered, where the oriented surface of the chamfered rotor blade tip had a normal vector with a component opposite to the direction of rotation of the blade. With this modification, the CrAlN PVD-coated chamfered rotor blade tip had much better cutting performance, but the chamfered rotor blade tip was still ground flat, and the coating on the tip and the sides near the tip was also removed, so the coating failed to protect the rotor blade tip from oxidation.

[0015] It is known that rotor blade tips with coatings that result in higher layer adhesion (e.g., PVD coatings) generally experience higher wear and rotor blade tip coating temperatures, and thus coating failure. Rotor blades with such coatings particularly benefit from the rotor blade tip according to the present invention, as frictional heat and wear are significantly reduced.

[0016] In one embodiment, the rotor blade tip has a multi-layer coating comprising an oxidation resistant abrasive layer on top of an MCrAlX layer, wherein M comprises one or more of Ni and Co, and X comprises one or more of Y and Hf.

[0017] In one embodiment, the oxidation-resistant polishing layer comprises oxide, boride, carbide, nitride or a mixture thereof.

[0018] In one embodiment, the orientation surface is convex or concave relative to the abradable coating during operation.

[0019] In one embodiment, at least a portion of the rotor blade tip is chamfered such that a directional surface of the chamfer has a normal vector having a component in the direction of rotation of the rotor blade.

[0020] In one embodiment, at least a portion of the rotor blade tip is chamfered with an angle of between 1 and 30 degrees, and in another embodiment, the flat surface of this chamfer comprises an edge radius between 5 and 200 μm.

[0021] In one embodiment, at least a portion of the rotor blade tip is curved such that the curved directional surface has at least one normal vector having a component in the direction of rotation of the rotor blade.

[0022] This problem is also solved by a method having the features of claim 9 .

[0023] Some embodiments will be explained in more detail with the aid of the following figures.

[0024] FIG1 shows a prior art coated rotor blade tip;

[0025] Figure 2 An embodiment of a rotor blade tip coating is shown;

[0026] Figure 3 shows the rotor blade as viewed from the front and rear, and an enlarged view of the rotor blade tip;

[0027] Figure 4 An embodiment of a rotor blade tip geometry with interacting forces is shown;

[0028] Figure 5-8 An embodiment of a rotor blade tip geometry is shown;

[0029] Figure 9 An embodiment of a rotor blade after intrusion friction testing is shown;

[0030] Figure 10 shows blade wear of an embodiment of a rotor blade and a prior art rotor blade in an intrusion friction test;

[0031] Figure 11 shows the temperature of an embodiment of a rotor blade and a prior art rotor blade during an intrusion friction test;

[0032] Figure 12 An embodiment of a method of manufacturing a rotor blade tip coating is shown;

[0033] Figure 13 An X-ray diffraction pattern of an embodiment of a rotor blade tip coating is shown.

[0034] Figure 1 shows a schematic diagram of a coated rotor blade tip according to the prior art. The coating is applied to a blade substrate 14 and typically comprises abrasive particles 13 (e.g., cubic boron nitride) embedded in an MCrAlX matrix 12. Such coatings are applied by electrolytic or electrophoretic deposition. It can be seen that any abrasive processes occur primarily on the surfaces and edges of the abrasive particles 13 protruding from the MCrAlX matrix 12.

[0035] Figure 2 A schematic representation of an embodiment of a rotor blade tip coating 10 is shown, which is applied to a blade substrate 14 and includes an MCrAlX layer 12 as an intermediate layer and an oxidation-resistant grinding layer 11. The blade substrate 14 may be a superalloy, such as a single-crystal superalloy, such as CMSX4. The MCrAlX layer 11 serves both as a binder between the blade substrate 14 and the oxidation-resistant grinding layer 11 and as an oxidation-resistant layer.

[0036] The oxidation-resistant abrasive layer 11 can be an aluminum-chromium oxide ceramic, which is oxidation-resistant at high temperatures because it has already been oxidized, and is also highly abrasive because it is very hard, with a hardness exceeding 2000 HV according to the Vickers hardness test. Similarly, many other oxides, borides, carbides, nitrides, and other ceramics work for the same reason: they are oxidation-resistant and abrasive. Without the MCrAlX intermediate layer 12, the lower blade base 14 would be at risk of oxidation if the layer were oxidized. Compared to the previous image, which shows a prior art coating, it can be clearly seen that the area where abrasion could occur is much larger, as it occurs over the entire surface of the oxidation-resistant abrasive layer 11.

[0037] Figure 3 Schematic representations of a front view and a side view of a rotor blade 30 are shown, along with an enlarged view of the rotor blade tip 20 , representing one embodiment of a rotor blade tip geometry.

[0038] The counterclockwise rotation direction R of the rotor blade is indicated by an arrow. For simplicity, the geometry of the rotor blade 30 is simplified by assuming that the vertical profiles of the front and side views are flat.

[0039] For example, an IN718 blade can be selected as the rotor blade 30, having a 1 mm wide rotor blade tip 20. A flat rotor blade tip geometry is disclosed in the prior art, but one embodiment of a rotor blade tip geometry is represented by a chamfered rotor blade tip. This chamfered rotor blade tip geometry results in a directional rotor blade tip surface 21 having a normal vector 22 with a component 23 in the direction of rotation R of the rotor blade. The normal vector 22 defines a directional surface at the rotor blade tip 20 that can interact with the abradable coating 16, as will be described below.

[0040] Figure 4 Shown is a schematic representation of an embodiment of a rotor blade 30 having a rotor blade tip 20 that cuts into the abradable coating 16 of the turbine shroud 15. The orientation surface defined by the normal vector 22 is inclined towards the abradable coating 16 in the direction of rotation R of the rotor blade.

[0041] For example, during thermal expansion or if the turbine is deflected from center by vibration, rotor blades 30 can move into turbine casing 15. Physically, the same situation occurs if turbine casing 15 moves into rotor blades 30. Therefore, the intrusion test involves testing the interaction between rotor blade tip 20 and anti-wear coating 16 by moving the turbine casing into the rotor blade at an intrusion velocity v. However, the same physical processes occur as in an actual operating turbine.

[0042] When the rotor blade tip 20 of the rotor blade 30 moves into the abradable coating 16 of the turbine shroud 15 or vice versa, the rotor blade tip is subjected to a force Fv from the intrusive motion into the abradable material and a force Fv from the rotational motion into the abradable coating 16. r , which leads to Figure 5 The total force F shown 总 .

[0043] Total force F 总 The direction depends on the intrusion force F v and the rotational force F r fraction (fraction).

[0044] The rotor blade tip 20 at least partially has a directional surface 21 with a normal vector 22 having a component 23 in the direction of rotation R of the rotor blade, which has the advantage that in this case the total force vector F 总 is aligned with the normal vector 22 to some extent, for example, they point in nearly opposite directions or have components pointing in opposite directions. Depending on the shape of the oriented surface with the normal vector 22, the orientation of the surface with respect to the vector F总 The weights of the offsetting vector components can be selected. In the embodiment shown, the orientation surface is a plane (i.e., a chamfered plane) that can be described by a normal vector 22. As will be shown below, in other embodiments, the orientation surface 21 has at least local curvature, so that the normal vector 22 locally describes the orientation. In any case, the orientation surface will have a certain component 23 in the direction of rotation R of the rotor blade.

[0045] This results in a distribution of forces normal to the coating 10 at the rotor blade tip, rather than forces transverse to the coating or to the sides of the rotor blade tip 20 .

[0046] In this case, the risk of shearing or tearing of the coating is significantly reduced. Furthermore, the friction is distributed over a larger area, thereby reducing local frictional heat and temperature-related wear processes on the coated blade tip. Together, this could be a possible explanation for the improved performance. The chamfered rotor blade tip geometry shown is to be regarded as merely one example of a rotor blade tip geometry and is not restrictive.

[0047] Figure 5-8 Other embodiments of rotor blade tip geometries are shown. Figure 5 and Figure 6 In FIG, a chamfered rotor blade 30 is shown with a normal vector 22 having a component 23 in the direction of rotation R of the rotor blade. Figure 7 and Figure 8 In FIG, a curved rotor blade is shown, where one normal vector 22 is illustrated among many possible normal vectors, said normal vector 22 having a component 23 in the direction of rotation R of the rotor blade. A corresponding abradable coating 16 on the turbine casing 15 is also shown.

[0048] This shows that the orientation surface 21 can be concave relative to the abradable coating 16 (e.g. Figure 7 ) or convex (e.g. Figure 5 、 Figure 6 or Figure 8 ).

[0049] Figure 9 An exemplary cross-sectional analysis of an embodiment of a rotor blade 30 is shown. In this example, the rotor blade tip 20 is coated with a multilayer coating consisting of an MCrAlY intermediate layer and an aluminum chromium oxide top layer. The rotor blade tip 20 has been chamfered at a 10° angle. The figure shows the blade tip 20 after an intrusion friction test. As indicated by the dashed line, the sample is sectioned in the middle. The arrow indicates the counterclockwise direction of rotation R of the blade. It can be seen that the coating remains intact after the friction test and covers all surfaces of the rotor blade tip.

[0050] Figure 10 The blade wear as a percentage of the total penetration depth is shown for three blade tip geometries, two of which are prior art and one of which is a claimed embodiment. The two prior art blade tip geometries are a flat blade tip geometry and a chamfered blade tip geometry that lacks a directional surface whose normal vector has a component in the direction of rotation of the rotor blade. All rotor blade tips are coated with a multilayer consisting of an MCrAlY intermediate layer and an aluminum chromium oxide top layer. It can be clearly seen that the blade tip of the claimed embodiment exhibits significantly lower wear (<1%) compared to the prior art blade tip (~25%).

[0051] Figure 11 The temperatures measured at the blade tip during the intrusion friction test are shown. The two prior art blade tips experienced temperature increases of approximately 480°C and 160°C, respectively, while the blade tip of the embodiment did not experience any temperature increase at all.

[0052] An embodiment of the method for producing a rotor blade tip coating 10 can be realized in particular by means of a PVD process using deposition from the gas phase. Figure 12 This is explained exemplarily in more detail.

[0053] The use of reactive cathodic arc evaporation is particularly preferred. By using reactive cathodic arc evaporation, the adhesion of the rotor blade tip coating 10 can be significantly improved, since a higher ion energy input contributes to improved layer adhesion. The coating can also be adapted to different blade substrate materials 14 and application requirements. Different PVD coating materials can be used, either as a single layer or in a multilayer combination, in order to provide the desired properties in terms of high-temperature oxidation resistance, hardness and ductility. These materials may include oxides, borides, carbides and nitrides. The coating is deposited on a rotor blade tip 20 made of a superalloy, such as CMSX4 as substrate 14, said coating having the following structure: an MCrAlY intermediate layer 12 followed by an aluminum chromium oxide layer as an oxidation-resistant grinding layer 11.

[0054] The MCrAlX layer 12 is deposited from a MCrAlX material source or target by plasma enhanced cathodic arc evaporation. Depending on the desired oxidation resistance, the MCrAlX layer 12 may have a thickness of 0.1-100 μm. In this example, the layer thickness is selected to be 10 μm.

[0055] The oxidation-resistant grinding layer 11 is deposited on the MCrAlX bonding and oxidation-resistant layer 12. The aluminum chromium oxide layer is deposited from a metallic AlCr target by reactive cathodic arc evaporation in an oxygen environment. The oxide layer 11 can be 0.5 to 50 μm thick. In this example, the layer thickness was chosen to be 10 μm.

[0056] The coating system is deposited on the rotor blade 30 using an arc deposition method. In order to apply the coating system to the rotor blade 30 using the coating method according to the claim, the rotor blade 30 is placed in a vacuum coating chamber 60. The rotor blade 30 is rotatably placed on a turntable 61 in the center of the vacuum chamber. The coating system can be deposited on the rotor blade 30 by using a different number of targets acting as cathodes, for example two, four or even more targets. The order and number of targets can be anything you want. In this specific example ( Figure 3 ) comprises four targets 63, 64, 65, 66, all of which are arranged so as to function as cathodes. Targets 63, 64, 65, 66 are mounted on the walls of a vacuum coating chamber 60. To produce the coating system described in this particular embodiment, cathodes 63 and 64 are targets comprising MCrAlY as a main component, and cathodes 65 and 66 are targets comprising aluminum chromium (AlCr) as a main component. The positions of the targets are to be regarded as an example only and are not limiting. To generate an oxygen-containing (O2) layer, a non-zero amount of O2 is fed into the vacuum chamber 60 via a gas inlet. In this example, the O2 pressure is set to 1.0 10 -2 Millibars. Figure 3 As shown, an argon (Ar) gas inlet is also installed to allow the use of argon as the working gas. For the production coating system, the coating temperature is selected to be in the range of 200-600°C. A magnet, not shown in this figure, is positioned behind the target, and the magnetic field can be adjusted to achieve variations in coating properties. A shutter 62 can be installed in front of the targets 63, 64, 65, 66 to allow the coating of different layers, but this is not required.

[0057] Figure 13 An X-ray diffraction pattern of an exemplary oxidation-resistant polishing layer 11, which is aluminum chromium oxide, is shown.

[0058] Although the embodiments have been described in the context of a plasma deposition process, chemical vapor deposition may be used in at least some steps.

[0059] List of Reference Numbers

[0060] 10 Rotor blade tip coating

[0061] 11 Anti-oxidation polishing layer

[0062] 12 MCrAlX layer

[0063] 13 Abrasive particles

[0064] 14 blade base

[0065] 15 Turbine housing

[0066] 16 Abradable coating

[0067] 20 Rotor blade tip

[0068] 21 Directed rotor blade tip surface

[0069] 22 Normal vector to the oriented rotor blade tip surface

[0070] 23 Component of the normal vector in the direction of rotation of the rotor blade

[0071] 30 rotor blades

[0072] 50 gas turbines

[0073] 60 Vacuum Chamber

[0074] 61 Turntable

[0075] 62 baffle

[0076] 63 Coated Target

[0077] 64 Coated Target

[0078] 65 Coated Target

[0079] 66 Coated Target

[0080] Al Aluminum

[0081] Argon

[0082] Cobalt

[0083] Cr chromium

[0084] F v Invasiveness

[0085] F r Rotational force

[0086] F 总 Total force

[0087] Hf Hafnium

[0088] M Metal

[0089] N Nitrogen

[0090] O2 oxygen

[0091] R Rotor blade rotation direction

[0092] v Intrusion speed

[0093] X consists of yttrium or hafnium or both

[0094] Yttrium

Claims

1. A rotor blade (30) in a gas turbine engine (50), It is characterized in that The coating (10) on the blade tip (20) of the rotor blade (30) comprises an oxidation-resistant abrasive layer (11), and the rotor blade tip (20) at least partially has a directional surface (21), the directional surface (21) having a normal vector (22), the normal vector (22) having a component (23) in the direction of rotation (R) of the rotor blade.

2. The rotor blade (30) according to claim 1, wherein: The rotor blade tip (20) comprises a multi-layer coating (10), wherein the multi-layer coating (10) further comprises an oxidation resistant abrasive layer (11) located on the MCrAlX layer, wherein M comprises one or more of Ni and Co, and X comprises one or more of Y and Hf.

3. The rotor blade (30) according to at least one of the preceding claims, wherein: The anti-oxidation grinding layer (11) comprises oxide, boride, carbide, nitride or a mixture thereof.

4. The rotor blade (30) according to at least one of the preceding claims, wherein: At least partially, the orientation surface (21) is convex or concave relative to the abradable coating (16) of the turbine casing (15) during operation.

5. The rotor blade (30) according to at least one of the preceding claims, wherein: The rotor blade tip (20) at least partially has an orientation surface (21) comprising a chamfered plane with a normal vector (22) having a component (23) in the direction of rotation (R) of the rotor blade.

6. The rotor blade (30) according to claim 5, wherein: The orientation surface (21) comprises a chamfered plane having a chamfer angle between 1 and 30 degrees, in particular between 5 and 15 degrees.

7. The rotor blade (30) according to claim 5 or 6, wherein: The chamfered flat surface comprises an edge radius between 5 and 200 μm.

8. The rotor blade (30) according to at least one of the preceding claims, wherein: At least a portion of the rotor blade tip (20) has a curved orientation surface (21), the curved orientation surface (21) having at least one normal vector (22), the at least one normal vector (22) having a component (23) in the direction of rotation (R) of the rotor blade.

9. A method for manufacturing a rotor blade (30), wherein: A coating (10) is deposited on a blade tip (20) of the rotor blade (30) by plasma vapor deposition and / or chemical vapor deposition, the coating (10) comprising an oxidation-resistant abrasive layer (11), and the rotor blade tip (20) at least partially has a directional surface (21), the directional surface (21) having a normal vector (22), the normal vector (22) having a component (23) in the direction of rotation (R) of the rotor blade.

10. The method of manufacturing a rotor blade (30) according to claim 9, wherein: The plasma vapor deposition method is cathodic arc evaporation.

11. The method for manufacturing a rotor blade (30) according to claim 9 or 10, wherein: The coating (10) is a multi-layer coating, comprising an oxidation resistant grinding layer (11) located on a MCrAlX layer, wherein M comprises one or more of Ni and Co, and X comprises one or more of Y and Hf.

12. Gas turbine engine (50) having a rotor blade (30) according to at least one of claims 1 to 7.