Low-ring hydrophilic amino silicon oil and preparation method thereof

By preparing low-ring hydrophilic amino silicone oil, the problem of yellowing, color change and high ring content during the processing process is solved, and the industrialization of low-ring and easy-to-renovation hydrophilic amino silicone oil is realized. Production meets the market's demand for low VOC and low ring bodies, and improves product application performance.

CN119019690APending Publication Date: 2024-11-26HUBEI XINGRUI SILICON MATERIAL CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411146154.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing modified amino silicone oil is prone to yellowing, color change and poor recovery during processing, and block silicone oil cannot meet the market demand for low rings and low VOCs, especially in the European and American markets for residual silicone ring volume. Under restrictions.

Method used

Using a preparation method of low-cyclic hydrophilic amino silicone oil, special amino silane and special amino silane are added by pre-drying hydroxyl-terminated polydimethylsiloxane and reacting with catalyst and dialkoxy coupling agent under nitrogen protection. The catalyst is added and the reaction stopper is finally added, and the reaction conditions are controlled to obtain a low-cyclic hydrophilic amino silicone oil.

Benefits of technology

It realizes the industrial production of hydrophilic amino silicone oil with low ring body and easy to rework. The product has low ring body content, smooth feel, and low yellowness. It meets the market's requirements for low VOC and low ring body, simple process and environmentally friendly, and energy consumption Low, the product structure is controllable.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019690A_ABST
    Figure CN119019690A_ABST
Patent Text Reader

Abstract

The invention provides low-ring hydrophilic amino silicone oil and a preparation method thereof. The preparation method comprises the following steps: carrying out pre-drying treatment on hydroxyl-terminated polydimethylsiloxane; then adding a catalyst and a dialkoxy coupling agent into the treated raw material, heating under the protection of nitrogen, controlling the reaction temperature, and removing the temperature until a certain viscosity is reached; secondly, discharging nitrogen to vacuum, adding special amino silane, heating after adding the materials, preserving heat, stirring and reacting for several hours; and adding a reaction terminator after the reaction is finished, keeping the temperature for a certain time, and cooling to obtain the product. The hydrophilic amino silicon oil has the advantages of easily available synthesis raw materials, extremely low ring content and no solvent reaction, the response to low ring product requirements and low VOC (volatile organic compound) limitation of the current organic silicon material and the urgent demand of hydrophilic functional silicon oil is very matched, the synthesis process route is easy for industrial production, and the hydrophilic amino silicon oil product synthesized by the method is particularly smooth in hand feeling, fine and elastic, and has a good market prospect. The anti-yellowing agent is extremely low in yellowing property and can be commonly used in the fields of textile after-finishing auxiliaries, daily chemical care additives and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of silicone oil synthesis, and in particular to a low-ring hydrophilic amino silicone oil and a preparation method thereof. Background Art With the rapid development of modified silicone oil, the replacement of various modified silicone softeners has accelerated. In the past, traditional amino silicone oil had the disadvantages of yellowing, color change and poor recovery. Modified amino silicone oil came into being. Because it has a significant effect on improving the softness of fabrics, it has become a widely used fabric finishing agent in the market. As consumers pursue a more comfortable lifestyle, textiles need to be repaired due to color change during product application, and the hydrophilicity of silicone oil needs to be further improved. In addition, although block silicone oil has been popular in recent years, it has solved the technical problems of easy oil bleaching, demulsification and easy repair of traditional amino silicone oil, and there are also regulatory restrictions on the VOC and ring content in the product, especially for the export of products to the European and American markets, it is necessary to comply with the EU REACH regulations on the amount of residual siloxane rings, that is, the mass fractions of octamethylcyclotetrasiloxane (D4), decamethylcyclopentasiloxane (D5) and dodecamethylcyclohexasiloxane (D6) should be less than 0.1% respectively. Obviously, the current 60%-80% block silicone oil (volatile components are ring body and solvent components) can no longer meet the requirements for low VOC content and low ring body. Based on the technical problems existing in the above industry, the development of a solvent-free, low-ring body and easy-to-repair hydrophilic silicone softener seems to be more in line with market demand. Summary of the invention

[0002] The invention provides a functional organosilicon polymer which is hydrophilic and low-cyclic and easy to industrialize.

[0003] The general chemical structure of the low-ring hydrophilic amino silicone oil is as follows: Type ① In the formula: R0 is one selected from NN diethylaminopropyl, 3-(N,N-dimethylaminopropyl)-aminopropyl, NN dimethylaminopropyl, tetramethyl quaternary ammonium, piperazinylpropyl, N,N-dimethylpropylenediaminopropyl, 3-(N-cyclohexylamino)propyl; R1, R2, R3 are one or more selected from CH3, CH2CH3, CH3O, CH3CH2O, CH3CH2CH2O and R0, and R1, R2, R3 connected to different Si atoms are independent of each other; a, b, c are natural numbers ranging from 1 to 1000 and are independent of each other.

[0004] The technical solution adopted by the present invention to solve the technical problem is: a low-ring hydrophilic amino silicone oil and a preparation method thereof, characterized in that the preparation process comprises the following steps: (1) Pre-drying the hydroxyl-terminated polydimethylsiloxane; The hydroxyl-terminated polydimethylsiloxane is one or more of hydroxyl silicone oil (specifically, viscosity 10-50 cts), linear silicone oil (specifically, viscosity 50-150 cts), and low-viscosity 107 glue (specifically, viscosity 150-2000 cts); The desiccant is one or more of anhydrous sodium sulfate, anhydrous calcium chloride, porous molecular sieve, color-changing silica gel, and activated alumina; The water content of the raw material after dehydration treatment is less than 100 ppm; preferably, the water content is less than 40 ppm; The drying temperature is 5-110°C; preferably, the dehydration temperature is 60°C; (2) then adding the catalyst and the dialkoxy coupling agent to the treated hydroxyl-terminated polydimethylsiloxane, and heating under nitrogen protection, controlling the reaction temperature and lowering the temperature until a certain viscosity is reached; The catalyst is one or a mixture of polydimethylsiloxane polymer prepared by tetramethylammonium hydroxide, polydimethylsiloxane polymer prepared by tetraethylammonium hydroxide, polydimethylsiloxane polymer prepared by potassium hydroxide, organic phosphazene base ligand P4-tert-butyl, sodium methoxide; The dialkoxy coupling agent is one or more of dimethyldimethoxysilane, dimethyldiethoxysilane, diethyldimethoxysilane, diethyldiethoxysilane, dimethyldipropoxysilane, diphenyldimethoxysilane, and methylphenyldimethoxysilane, but is not limited to dialkyldialkoxysilane compounds; preferably, the dialkoxy coupling agent is one or more of dimethyldimethoxysilane, dimethyldiethoxysilane, diethyldimethoxysilane, diethyldiethoxysilane, dimethyldipropoxysilane, and methylphenyldimethoxysilane; The amount of the catalyst is 0.5-2000ppm; the amount of the dialkoxy coupling agent is 0.01-20% of the mass of the hydroxyl-terminated polydimethylsiloxane; the degassing temperature is 20-80°C; the viscosity of the material after degassing is 5000-2000000 mPa.s; preferably, the amount of the catalyst is 1-500ppm; the amount of the dialkoxy coupling agent is 0.01-10% of the mass of the hydroxyl-terminated polydimethylsiloxane; the reaction temperature is 20-60°C; preferably, the viscosity of the material after degassing is controlled to be 10000-1000000 mPa.s.

[0005] (3) Next, the vacuum is released with nitrogen, and special aminosilane is added. After the addition of the materials, a certain amount of catalyst is added and the reaction is stirred and kept at a certain temperature for several hours; The special aminosilane includes one or a mixture of NN diethylaminopropyl trimethoxysilane, NN dimethylaminopropyl trimethoxysilane, 3-(N,N-dimethylaminopropyl)-aminopropyl methyl dimethoxysilane, tetramethylammonium silanol, NN diethylaminopropyl triethoxysilane, piperazine propyl triethoxysilane, tetramethyldipropylene triaminopropyl methyl dimethoxysilane, NN diethylaminopropyl methyl dimethoxysilane, N,N-dimethylpropylene diaminopropyl methyl dimethoxysilane, NN diethylaminopropyl trimethoxysilane, and 3-(N-cyclohexylamino)propyl methyl dimethoxysilane. The mass proportion of the special aminosilane is 0.1-30%; the insulation temperature is 30-150°C, and the insulation time is 0.5-15h; Preferably, the mass proportion of special aminosilane is 0.2~15%; the insulation temperature is 30~110°C, and the insulation time is 0.5~5h.

[0006] The additional catalyst is one or a mixture of polydimethylsiloxane polymers prepared by tetramethylammonium hydroxide, polydimethylsiloxane polymers prepared by tetraethylammonium hydroxide, polydimethylsiloxane polymers prepared by potassium hydroxide, organic phosphazene bases and solutions thereof, and sodium methoxide; preferably, the additional catalyst is one or a mixture of tetramethylammonium hydroxide and polydimethylsiloxane polymers prepared by tetraethylammonium hydroxide and polydimethylsiloxane polymers prepared by tetraethylammonium hydroxide, organic phosphazene bases and solutions thereof; The amount of addition is 0.5~1500ppm; preferably, the amount of addition is 0.5~500ppm; (4) After the final reaction is completed, a reaction terminator is added, and the mixture is kept warm for a certain period of time and then cooled to obtain a low-ring hydrophilic amino silicone oil product.

[0007] The amount of the terminator added in step (4) is 0.2 to 5 times the molar amount of the catalyst, and the mixture is mixed and kept warm at 20 to 120° C. for 0.05 to 2 hours and then cooled to room temperature.

[0008] The reaction terminator includes one or more of polydimethylsiloxane polymer prepared from phosphoric acid, silicic acid, formic acid, acetic acid, oleic acid, propionic acid, and pyruvic acid.

[0009] The polydimethylsiloxane polymer prepared by phosphoric acid is used as a terminator to neutralize the system alkali, which can improve compatibility, shorten the neutralization time and make the neutralization more thorough; it has similar properties to the polydimethylsiloxane polymer prepared by alkali catalyst in improving the reaction activity and catalytic efficiency.

[0010] The terminator is added in an amount of 0.2 to 5 times the molar amount of the catalyst; preferably, the amount is added in an amount of 0.5 to 3.5 times; The insulation temperature is 20-120°C, and the insulation time is 0.2-1h; preferably, the temperature is 30-105°C, and the time is 0.3-1h; The low-ring hydrophilic amino silicone oil prepared by the present invention not only has a low ring body content, but also is hydrophilic and easy to process and repair in printing and dyeing factories. In addition, the product feels particularly smooth and fluffy, has low yellowing, and is a multifunctional amino silicone oil that is easy to industrialize. The specific reaction equation is as follows: Formula ② In the formula, R0 is selected from NN diethylaminopropyl, 3-(N,N-dimethylaminopropyl)-aminopropyl, NN dimethylaminopropyl, tetramethyl quaternary ammonium, piperazinyl propyl, N,N-dimethyl propylene diaminopropyl, 3-(N-cyclohexylamino) propyl; R1, R2, R3 are selected from CH3, CH2CH3, CH3O, CH3CH2O, CH3CH2CH2O and one or more of R0, and R1, R2, R3 connected to different Si atoms are independent of each other; m is a natural number greater than 400; a, b, c are natural numbers of 1 to 1000, and are independent of each other. The molecular weight of the prepared low-ring hydrophilic amino silicone oil is between 500 and 100000, and the polydispersity index (PDI) is between 1.15 and 2.20.

[0011] The chemical structural formula of the hydrophilic amino silicone oil includes but is not limited to the following: , , , , , , Any one of the following; a, b, c are natural numbers ranging from 1 to 1000.

[0012] The technical solution of the present invention also provides a hydrophilic silicone softener, comprising the amino silicone oil prepared by the method described or the amino silicone oil described.

[0013] Compared with the existing related technologies, the advantages of the present invention are: 1. The synthetic process route is simple, environmentally friendly, and easy for industrial production. The existing industry technology mainly uses block silicone oil to solve the problems of softener sticking, yellowing, and rework in printing and dyeing factories. It mainly uses DMC / D4 to first synthesize terminal hydrogen silicone oil, and then synthesize epoxy silicone oil through silylation with epoxy active monomers; then it is synthesized with polyether organic amines in a solvent through 2-5 steps. Finally, the solvent can be selectively removed or used directly. The present invention directly adopts the raw material hydroxyl-terminated polydimethylsiloxane produced by the upstream monomer enterprise of silicone, which is first polymerized and then micro-amination balancing process. The process is simple. Compared with the multi-step block silicone oil produced by downstream enterprises, it is not only time-saving and energy-saving, but also low-carbon and environmentally friendly.

[0014] 2. The product synthesized by the process of the present invention has low cyclic body and high yield. At present, the mainstream way for the industry to implement the relevant low-cyclic body requirements by using this route is to first condense hydroxyl-terminated polydimethylsiloxane and then synthesize low-cyclic bodies, but the temperature used is very high (KOH catalyst, decondensation 150~190℃), and then cool to synthesize low-cyclic body products. The present invention utilizes the characteristics of dialkoxy coupling agent and hydroxyl-terminated polydimethylsiloxane that are very easy to condense and adopts a high-activity catalyst at low temperature (minimum less than 80℃) vacuum condensation polymerization equilibrium process, which greatly reduces energy consumption and procedures, and can avoid cooling after high-temperature condensation, which is convenient for continuous reaction and more conducive to industrial production; at the same time, by controlling the amount of catalyst, it is possible to avoid excessive catalyst and excessive temperature so that the polymer depolymerizes into a high-cyclic body, and the product synthesis yield is higher and the cyclic body is lower.

[0015] 3. The polymer structure design is highly controllable, and the product can adjust the feel according to the user's hydrophilic speed and low yellowing performance requirements. The hydrophilic amino silicone oil synthesized by the present invention has a wide range of selectivity. The product application performance, fabric finishing style and hydrophilicity brought by different tertiary amine and quaternary ammonium structure functional silanes and low-ring hydroxyl silica gels with different viscosities are richer. Compared with the traditional block silicone oil synthesis technology, the traditional block silicone oil synthesis process is easy to cause product structure instability due to the complexity of epoxy silicone oil intermediate raw material synthesis, various auxiliary materials and additives, and cumbersome process flow (conventionally more than four steps of reaction). The product application indicators are prone to change and uncontrollable. Therefore, block silicone oils in the industry market often have obvious batch differences and many customer complaints; in addition, the synthesis of block silicone oils also requires the addition of solvents to react, which easily causes the product to change color and reduce hydrophilicity due to solvents. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 This is the gel chromatography molecular weight distribution diagram of Example 3 of the prepared low-ring hydrophilic amino silicone oil.

[0017] Figure 2 This is a diagram showing the ring body content analysis of the prepared low-ring body hydrophilic amino silicone oil Example 2. DETAILED DESCRIPTION

[0018] The present invention is further described in detail below through examples and accompanying drawings, but the examples are not intended to limit the scope of protection of the present invention. The raw materials used in the examples can be purchased commercially or prepared by conventional methods. In addition, for ease of understanding, the hydroxyl-terminated polydimethylsiloxane of the present invention has a molecular formula of HO-Si(CH3)2O[Si(CH3)2O]nSi(CH3)2-OH; the main commercial forms such as linear bodies, hydroxyl silicone oils, and low-viscosity 107 glues have relevant basic indicators, viscosity: (25°C, mPa﹒s): ≤ 2000; volatile matter (150°C*3h, %): ≤ 1.5; hydroxyl content (hydroxyl mass percentage, %): ≤ 2.5.

[0019] The polydimethylsiloxane polymer prepared from tetramethylammonium hydroxide, tetraethylammonium hydroxide and polydimethylsiloxane polymer prepared from it, potassium hydroxide and polydimethylsiloxane polymer prepared from it, organic phosphazene base ligand P4-tert-butyl and its solution, sodium methoxide or a mixture thereof.

[0020] For example, the polydimethylsiloxane polymer prepared by tetramethylammonium hydroxide is prepared by using tetramethylammonium hydroxide (or its hydrate) and raw material hydroxyl-terminated polydimethylsiloxane at 80-95°C, nitrogen gas (flow rate controlled at 2-3L / min) is passed through the bottom for 3-4 hours to obtain a colorless, transparent, viscous liquid (polymer liquid yield is about 89-95%), wherein the mass concentration of tetramethylammonium hydroxide is 0.1-3.0%. Similarly, the method for preparing the catalyst by replacing tetramethylammonium hydroxide (or its hydrate) with tetraethylammonium hydroxide (or its hydrate) is the same as above.

[0021] The polydimethylsiloxane polymer prepared by potassium hydroxide is prepared by using KOH and the raw material hydroxyl-terminated polydimethylsiloxane to keep warm for 4-5 hours at 120-150°C with nitrogen passing through the bottom (the flow rate is controlled at 1-2L / min) to obtain a colorless, transparent, viscous liquid (the yield of the high molecular polymer liquid is about 85-95%). A colorless, transparent, viscous liquid (viscosity (25°C, 100-6000cps, KOH mass concentration 0.1-3.0%) is obtained.

[0022] The polydimethylsiloxane polymer prepared from phosphoric acid is prepared by using phosphoric acid and raw material hydroxyl-terminated polydimethylsiloxane to keep warm for 3-4 hours at 90-110°C with nitrogen flowing through the bottom (flow rate controlled at 2-3L / min) to obtain a colorless, transparent, viscous liquid (the yield of the high molecular polymer liquid is about 89-95%), wherein the mass concentration of phosphoric acid is 5.0-7.0%.

[0023] The conventional physical and chemical properties and application-related properties of the products at each stage in each embodiment are measured and calculated as follows: (1) Viscosity measurement: Rotary digital viscometer SNB-4T (0.1-2000000 mPa.s); (2) Yellowing test: using digital whiteness meter WSB-2; (3) Friction coefficient, softness and fluffiness measurement: measured using YG821L fabric style meter; (4) Hydrophilicity determination: using the sedimentation method GB / T 22799 (test method for hydrophilicity of towel products); (5) Moisture determination: Coulometric Karl Fischer moisture meter (HOGON); (6) Determination of low-ring D4 / D5 / D6: Use the methods specified in EPA 3550C:2007 and EPA 8270E:2018.

[0024] Example 1 Add 700 parts of hydroxy silicone oil (Hubei Xingtuo New Materials Technology Co., Ltd., viscosity 38cts, hydroxyl content 4.5%) to a clean and dry 1000ml three-necked reaction flask, add 20 parts of 4A molecular sieve under stirring, and filter at 35℃ for half an hour under stirring adsorption (the water content of the filtrate is 30.5ppm). Transfer the filtrate to 680 parts of a 1000ml four-necked reaction flask, evacuate the nitrogen, add 2 parts of dimethyldimethoxysilane, 0.68 parts of phosphazene base ligand P4-tert-butyl (hexane solvent, mass solubility 0.5%), heat to 65℃, control the negative pressure to -0.99MPa, and evacuate the nitrogen to obtain 670 parts of hydroxy silica gel A (viscosity measured 325000 mPa.s). Continue to add 34 parts of NN diethylaminopropyl trimethoxysilane to raw material A, add 0.40 parts of phosphazene base ligand P4-tert-butyl (hexane solvent, mass solubility 0.5%) under nitrogen protection, and keep warm at 50℃ for 3h under nitrogen protection. Then drop 0.4 parts of silicic acid (concentration 0.5%, ethanol solvent), keep warm at 50℃ for 0.5h, cool to room temperature and discharge to obtain a colorless, transparent, viscous liquid. The product yield is 97.10%. The specific structural formula of hydrophilic amino silicone oil is Among them, (a+b+c)=90~100.

[0025] The low-ring hydrophilic amino silicone oil sample prepared in Example 1 was measured by PL-GPC50 gel permeation chromatography, with polysiloxane as the standard sample and toluene as the mobile phase. The weight average molecular weight of the prepared silicone oil sample was 6530, the number average molecular weight was 5661, and the polydispersity index PDI was 1.95; the viscosity of the low-ring hydrophilic amino silicone oil product at 25°C was 120 mPa.s by a rotational viscometer. The main ring body content of the sample was determined to be D4: 126 mg / kg, D5: 398 mg / kg, and D6: 524 mg / kg.

[0026] Example 2 Add 700 parts of hydroxy silicone oil (Hubei Xingtuo New Materials Technology Co., Ltd., viscosity 26cts, hydroxyl content 8.9%) to a clean and dry 1000ml three-necked reaction flask, add 20 parts of 4A molecular sieves under stirring, and filter at 35℃ for half an hour under stirring adsorption (the water content of the filtrate is 40ppm). Transfer the filtrate to 685 parts of a 1000ml four-necked reaction flask, evacuate the nitrogen, add 2 parts of dimethyldiethoxysilane, 0.69 parts of phosphazene base ligand P4-tert-butyl (hexane solvent, mass solubility 0.5%), heat to 65℃, control the negative pressure to -0.99MPa, and evacuate the nitrogen to obtain 668 parts of hydroxy silica gel A (viscosity measured 306000 mPa.s). Continue to add 35 parts of tetramethyldipropylenetriaminopropylmethyldimethoxysilane to raw material A, add 0.40 parts of phosphazene base ligand P4-tert-butyl (hexane solvent, mass solubility 0.5%) under nitrogen protection, and keep warm at 50℃ for 3h under nitrogen protection. Then drop 0.4 parts of silicic acid (concentration 0.5%, ethanol solvent), keep warm at 50℃ for 0.5h, cool to room temperature and discharge, and obtain a light yellow transparent viscous liquid. The product yield is 97.56%. The specific structural formula of hydrophilic amino silicone oil is Among them, (a+b+c)=140~155.

[0027] The low-ring hydrophilic amino silicone oil sample prepared in Example 2 was measured by PL-GPC50 gel permeation chromatograph, with polysiloxane as the standard sample and toluene as the mobile phase. The weight average molecular weight of the prepared silicone oil sample was 10030, the number average molecular weight was 9652, and the polydispersity index PDI was 1.65; the viscosity of the low-ring hydrophilic amino silicone oil product at 25°C was 260 mPa.s using a rotational viscometer. The main ring body content of the sample was determined to be D4: 156 mg / kg, D5: 268 mg / kg, and D6: 300 mg / kg.

[0028] Example 3 Add 700 parts of hydroxy silicone oil (Hubei Xingtuo New Materials Technology Co., Ltd., viscosity 26cts, hydroxyl content 8.9%) to a clean and dry 1000ml three-necked reaction flask, add 35 parts of 4A molecular sieves under stirring, and filter at 45℃ for half an hour under stirring adsorption (the water content of the filtrate is 35ppm). Transfer the filtrate to 685 parts of a 1000ml four-necked reaction flask, evacuate the nitrogen, add 2 parts of dimethyldimethoxysilane, 0.65 parts of phosphazene base ligand P4-tert-butyl (hexane solvent, mass solubility 0.5%), heat to 65℃, control the negative pressure to -0.99MPa, and evacuate the nitrogen to obtain 668 parts of hydroxy silica gel A (viscosity measured 556000 mPa.s). Continue to add 18 parts of tetramethylammonium silanol and 17 parts of NN diethylaminopropyl trimethoxysilane to the raw material A, add 0.40 parts of phosphazene base ligand P4-tert-butyl (hexane solvent, mass solubility 0.5%) under nitrogen protection, and keep warm at 50℃ for 3h under nitrogen protection. Then drop 0.4 parts of silicic acid (concentration 0.5%, ethanol solvent), keep warm at 50℃ for 0.5h, cool to room temperature and discharge, and obtain a light yellow transparent viscous liquid. The product yield is 96.56%. The specific structural formula of hydrophilic amino silicone oil is Among them, (a+b+c)=110~125.

[0029] The low-ring hydrophilic amino silicone oil sample prepared in Example 3 was measured by PL-GPC50 gel permeation chromatography, with polysiloxane as the standard sample and toluene as the mobile phase. The weight average molecular weight of the prepared silicone oil sample was 7855, the number average molecular weight was 4443, and the polydispersity index PDI was 1.76; the viscosity of the low-ring hydrophilic amino silicone oil product at 25°C was 56 mPa.s using a rotational viscometer. The main ring body content of the sample was determined to be D4: 119 mg / kg, D5: 256 mg / kg, and D6: 521 mg / kg.

[0030] Example 4 Add 700 parts of hydroxy silicone oil (Hubei Xingrui Silicon Material Co., Ltd., linear body 70cts, hydroxyl content 1.5%) to a clean and dry 1000ml three-necked reaction bottle, add 35 parts of 4A molecular sieve under stirring, and filter at 45℃ for half an hour under stirring adsorption (the water content of the filtrate is 25ppm). Transfer the filtrate to 685 parts of a 1000ml four-necked reaction flask, after nitrogen is evacuated, add 2 parts of dimethyldimethoxysilane, 0.65 parts of phosphazene base ligand P4-tert-butyl (hexane solvent, mass solubility 0.5%), heat to 65℃, control the negative pressure to -0.99MPa, and release the vacuum with nitrogen to obtain 670 parts of hydroxy silica gel A (viscosity measured 556000 mPa.s). Continue to add 16 parts of tetramethyldipropylenetriaminopropylmethyldimethoxysilane and 19 parts of NN dimethylaminopropyltrimethoxysilane to the raw material A, stir and add 0.40 parts of phosphazene base ligand P4-tert-butyl (hexane solvent, mass solubility 0.5%) under nitrogen protection, and keep warm at 50℃ for 3h under nitrogen protection. Then drop 0.4 parts of silicic acid (concentration 0.5%, ethanol solvent), keep warm at 50℃ for 0.5h, cool to room temperature and discharge, and obtain a light yellow transparent viscous liquid. The product yield is 96.60%. The specific structural formula of hydrophilic amino silicone oil is Among them, (a+b+c)=195~215.

[0031] The low-ring hydrophilic amino silicone oil sample prepared in Example 4 was measured by PL-GPC50 gel permeation chromatography, with polysiloxane as the standard sample and toluene as the mobile phase. The weight average molecular weight of the prepared silicone oil sample was 15030, the number average molecular weight was 13258, and the polydispersity index PDI was 1.85; the viscosity of the low-ring hydrophilic amino silicone oil product at 25°C was 560 mPa.s using a rotational viscometer. The main ring body content of the sample was determined to be D4: 260 mg / kg, D5: 320 mg / kg, and D6: 630 mg / kg.

[0032] Example 5 Add 700 parts of hydroxy silicone oil (Hubei Xingrui Silicon Material Co., Ltd., linear body 70cts, hydroxyl content 1.5%) to a clean and dry 1000ml three-necked reaction flask, add 36 parts of 4A molecular sieve under stirring, and filter at 45℃ for half an hour under stirring adsorption (the water content of the filtrate is 28ppm). Transfer the filtrate to 686 parts of a 1000ml four-necked reaction flask, after nitrogen is evacuated, add 2 parts of dimethyldimethoxysilane, 0.65 parts of polydimethylsiloxane prepared by tetramethylammonium hydroxide (tetramethylammonium hydroxide mass solubility 0.50%), heat to 65℃, control the negative pressure to -0.99MPa, and release the vacuum with nitrogen to obtain 670 parts of hydroxy silica gel A (viscosity measured 556000 mPa.s). Continue to add 35 parts of piperazinylpropyltriethoxysilane to raw material A, add 0.40 parts of polydimethylsiloxane prepared from tetramethylammonium hydroxide (tetramethylammonium hydroxide mass solubility 0.50%) under nitrogen protection, and keep warm at 50℃ for 3h under nitrogen protection. Then drop 0.4 parts of silicic acid (concentration 0.5%, ethanol solvent), keep warm at 50℃ for 0.5h, cool to room temperature and discharge, and obtain a light yellow transparent viscous liquid. The product yield is 95.30%. The specific structural formula of hydrophilic amino silicone oil is , where (a+b+c)=170~210.

[0033] The low-ring hydrophilic amino silicone oil sample prepared in Example 5 was measured by PL-GPC50 gel permeation chromatography, with polysiloxane as the standard sample and toluene as the mobile phase. The weight average molecular weight of the prepared silicone oil sample was 12030, the number average molecular weight was 9288, and the polydispersity index PDI was 1.82; the viscosity of the low-ring hydrophilic amino silicone oil product at 25°C was 380 mPa.s using a rotational viscometer. The main ring body content of the sample was determined to be D4: 460 mg / kg, D5: 356 mg / kg, and D6: 830 mg / kg.

[0034] Example 6 Add 700 parts of hydroxy silicone oil (Hubei Xingrui Silicon Material Co., Ltd., linear body 70cts, hydroxyl content 1.5%) to a clean and dry 1000ml three-necked reaction bottle, add 36 parts of 4A molecular sieve under stirring, and filter at 45℃ for half an hour under stirring adsorption (the water content of the filtrate is 26ppm). Transfer the filtrate to 689 parts of a 1000ml four-necked reaction flask, after nitrogen is evacuated, add 2 parts of dimethyldimethoxysilane, 0.65 parts of polydimethylsiloxane polymer prepared by tetraethylammonium hydroxide (tetraethylammonium hydroxide mass solubility 0.50%), heat to 65℃, control the negative pressure to -0.99MPa, and release the vacuum with nitrogen to obtain 675 parts of hydroxy silica gel A (viscosity measured 556000 mPa.s). Continue to add 35 parts of 3-(N-cyclohexylamino)propylmethyldimethoxysilane to raw material A, add 0.40 parts of polydimethylsiloxane polymer prepared by tetraethylammonium hydroxide (tetraethylammonium hydroxide mass solubility 0.50%) under nitrogen protection, and keep it at 50℃ for 3h under nitrogen protection. Then drop 0.4 parts of silicic acid (concentration 0.5%, ethanol solvent), keep it at 50℃ for 0.5h, cool to room temperature and discharge, and obtain a light yellow transparent viscous liquid. The product yield is 95.30%. The specific structural formula of hydrophilic amino silicone oil is

[0035] Among them, (a+b+c)=190~250.

[0036] The low-ring hydrophilic amino silicone oil sample prepared in Example 6 was measured by PL-GPC50 gel permeation chromatography, with polysiloxane as the standard sample and toluene as the mobile phase. The weight average molecular weight of the prepared silicone oil sample was 18800, the number average molecular weight was 19328, and the polydispersity index PDI was 1.87; the viscosity of the low-ring hydrophilic amino silicone oil product at 25°C was 780 mPa.s by a rotational viscometer. The main ring body content of the sample was determined to be D4: 560 mg / kg, D5: 573 mg / kg, and D6: 790 mg / kg.

[0037] Example 7 In the process of this embodiment, the catalyst is a polydimethylsiloxane polymer prepared by KOH, that is, the polydimethylsiloxane polymer prepared by 0.68 parts of KOH in the first time and the polydimethylsiloxane polymer prepared by 0.40 parts of KOH in the second time; the mass concentration of the catalyst is 0.50%, and the other steps and processes are consistent with Example 1. This comparative experiment obtains a light yellow transparent viscous liquid, the product yield is 96.78%, the weight average molecular weight of the product is 20528, the number average molecular weight is 19213, and the polydispersity index PDI is 1.98; the viscosity of the product at 25°C is 960 mPa.s. The main ring body content of the sample was determined to be D4: 566mg / kg, D5: 685mg / kg, D6: 952mg / kg.

[0038] Comparative Example 1 Except that tetramethylammonium silanol is not used, the other steps of the comparative example process are consistent with those of Example 3. The comparative example experiment obtained a light yellow transparent viscous liquid with a product yield of 96.78%, a weight average molecular weight of 16360, a number average molecular weight of 14552, and a polydispersity index PDI of 1.60; the viscosity of the product at 25°C is 620 mPa.s. The main ring body content of the sample was measured as D4: 150 mg / kg, D5: 360 mg / kg, and D6: 608 mg / kg.

[0039] Comparative Example 2 Except for using acetic acid to replace silicic acid, the other steps of the comparative example process are consistent with Example 4. The comparative example experiment obtained a light yellow transparent viscous liquid with a product yield of 96.98%. The weight average molecular weight of the sample was 14620, the number average molecular weight was 12658, and the polydispersity index PDI was 1.83; the viscosity of the product at 25°C was 486 mPa.s. The main ring body content of the sample was measured as D4: 560 mg / kg, D5: 890 mg / kg, and D6: 1020 mg / kg.

[0040] Product Examples and Comparative Examples Different tertiary amine aminosilanes were selected and process conditions were changed through experiments, and relevant performance index comparison and application tests were carried out with conventional block silicone oil products on the market. The specific experimental results are shown in the following table:

[0041] Note: The sample fabrics in the table were tested according to the sedimentation method GB / T 22799; the blank fabric samples were measured: hydrophilic time 50s; whiteness 101.6; dynamic friction coefficient μdynamic 1.986, static friction coefficient μstatic 2.358; fabric activity rate 12.28%, bending stiffness 108.94 cN.cm; fluffiness 92 cm3 / g. Explanation of the meaning of the index data: the lower the friction coefficient, the more obvious the slippage of the fabric sample; the higher the activity rate, the smaller the bending stiffness, which means the softer the fabric feels; the larger the fluffiness value, the better the fluffiness of the fabric sample.

[0042] It can be seen from the examples and comparative examples in the table that the change of the catalyst in Example 7 relative to Example 1 mainly affects the equilibrium polymerization degree, the catalytic activity of the organic phosphazene base is stronger than that of the tetramethyl alkali glue, the utilization rate of the balanced end-capping of the amino coupling agent is higher, the product viscosity is low, the molecular distribution is more uniform, the yellowing is significantly lower, the softness and hydrophilicity are better, the looseness is close, and the application evaluation is almost the same as that of Demei T803; the synthesis experiment of Comparative Example 1 has no tetramethylammonium silanol ionic group introduced, and the hydrophilicity is significantly reduced compared with Example 3, and there is also a significant difference in fluffiness and hydrophilicity; Comparative Example 2 is compared with Example 4, and the acids with different compatibilities are relatively not completely neutralized in the system. After the reaction, the catalyst acid balance does not completely crack the polymer, which will cause the product ring body to increase. In addition, in terms of hydrophilicity, the product is slightly reduced, and there is no significant change in other aspects. The product can be comparable to the market Runhe 9901. In addition, compared with Example 1, after increasing the number of tertiary amine amino groups, Example 2 has a significantly faster hydrophilicity, and the smoothness, fluffiness and softness are greatly improved, but the yellowing property is reduced. Therefore, while adjusting the hydrophilicity and hand feel, the selectivity balance is considered according to customer needs and application needs. In addition, compared with the traditional market Demei, Kefeng, and Runhe block silicone oil products, the ring body content of the present invention is significantly lower, which can meet the EU REACH regulatory standards (the content of D4, D5, and D6 is required to be less than 1000ppm).

[0043] Compared with the current related technology (solvent synthesis method), the low-ring hydrophilic amino silicone oil product of the present invention has the advantages of easy availability of synthetic raw materials, simple process and low industrialization cost. In addition, the technical route has high yield, solvent-free reaction, low product ring body content, and the synthetic process route is easy to industrialize, which is very consistent with the current requirements for low-ring products of organic silicon materials, low VOC restrictions and urgent demand for hydrophilic functional silicone oils. The hydrophilic amino silicone oil product synthesized by this method has a particularly smooth, delicate and elastic feel, and has extremely low yellowing, and can often be used in the fields of textile finishing auxiliaries and daily chemical care additives.

[0044] The above-described embodiment is only a relatively preferred example of the present invention and does not limit the present invention in any form. There are other structures without exceeding the technical solutions described in the claims.

Claims

1. A method for preparing a low-ring hydrophilic amino silicone oil, characterized in that: The preparation process comprises the following steps: (1) First, dry the hydroxyl-terminated polydimethylsiloxane until the water content is less than 100 ppm; (2) then adding the catalyst and the dialkoxy coupling agent to the hydroxyl-terminated polydimethylsiloxane in step (1), heating under nitrogen protection, controlling the reaction temperature and lowering the temperature until a certain viscosity is reached; (3) Next, the vacuum is released with nitrogen, and special aminosilane is added. After the addition of the materials, a certain amount of catalyst is added and the reaction is stirred and kept at a certain temperature; (4) After the final reaction is completed, a reaction terminator is added, and the mixture is kept warm for a certain period of time and then cooled to obtain a low-ring hydrophilic amino silicone oil product.

2. The method for preparing a low-ring hydrophilic amino silicone oil according to claim 1, characterized in that: The hydroxyl-terminated polydimethylsiloxane described in step (1) is one or more of hydroxyl silicone oil, linear silicone oil, and low-viscosity 107 glue; the desiccant used in the drying treatment includes one or more of anhydrous sodium sulfate, anhydrous calcium chloride, a porous molecular sieve, color-changing silica gel, and activated alumina, and the drying treatment temperature is 5~110°C.

3. The method for preparing low-ring hydrophilic amino silicone oil according to claim 1, characterized in that: The catalyst in step (2) is one or a mixture of polydimethylsiloxane polymer prepared by tetramethylammonium hydroxide, polydimethylsiloxane polymer prepared by tetraethylammonium hydroxide, polydimethylsiloxane polymer prepared by potassium hydroxide, phosphazene base ligand P4-tert-butyl, sodium methoxide, and the amount of the catalyst is 0.5~2000ppm.

4. The method for preparing low-ring hydrophilic amino silicone oil according to claim 1, characterized in that: The dialkoxy coupling agent described in step (2) is one or more of dimethyldimethoxysilane, dimethyldiethoxysilane, diethyldimethoxysilane, diethyldiethoxysilane, dimethyldipropoxysilane, diphenyldimethoxysilane, and methylphenyldimethoxysilane; the amount of the dialkoxy coupling agent is 0.01-20% of the mass of the hydroxyl-terminated polydimethylsiloxane; and the reaction temperature is 20-80°C.

5. The method for preparing low-ring hydrophilic amino silicone oil according to claim 1, characterized in that: The special aminosilane described in step (3) includes one or a mixture of NN diethylaminopropyl trimethoxysilane, NN dimethylaminopropyl trimethoxysilane, 3-(N,N-dimethylaminopropyl)-aminopropyl methyl dimethoxysilane, tetramethylammonium silanol, NN diethylaminopropyl triethoxysilane, piperazine propyl triethoxysilane, tetramethyldipropylene triaminopropyl methyl dimethoxysilane, NN diethylaminopropyl methyl dimethoxysilane, N,N-dimethylpropylene diaminopropyl methyl dimethoxysilane, NN diethylaminopropyl trimethoxysilane, and 3-(N-cyclohexylamino)propyl methyl dimethoxysilane; the mass proportion of the special aminosilane is 0.1~30%.

6. The method for preparing low-ring hydrophilic amino silicone oil according to claim 1, characterized in that: The catalyst in step (3) is one or a mixture of polydimethylsiloxane polymer prepared by tetramethylammonium hydroxide, polydimethylsiloxane polymer prepared by tetraethylammonium hydroxide, polydimethylsiloxane polymer prepared by potassium hydroxide, organic phosphazene base, sodium methoxide, and the amount of the catalyst is 0.5-1500ppm; the insulation temperature is 30-150°C, and the insulation time is 0.5-15h.

7. The method for preparing low-ring hydrophilic amino silicone oil according to claim 1, characterized in that: The terminator described in step (4) includes one or more of polydimethylsiloxane polymer prepared from phosphoric acid, silicic acid, formic acid, acetic acid, oleic acid, propionic acid, and pyruvic acid; the amount of the terminator added is 0.2 to 5 times the mass of the catalyst, and the mixture is mixed and kept warm at 20 to 120° C. for 0.05 to 2 hours and then cooled to room temperature.

8. The low-ring hydrophilic amino silicone oil prepared according to the method according to any one of claims 1 to 7, characterized in that: The general chemical structure of the block silicone oil is as follows: , wherein: R0 is one selected from NN diethylaminopropyl, 3-(N,N-dimethylaminopropyl)-aminopropyl, NN dimethylaminopropyl, tetramethyl quaternary ammonium, piperazinylpropyl, N,N-dimethylpropylenediaminopropyl, 3-(N-cyclohexylamino)propyl; R1, R2, R3 are one or more selected from CH3, CH2CH3, CH3O, CH3CH2O, CH3CH2CH2O and R0, and R1, R2, R3 connected to different Si atoms are independent of each other; a, b, c are natural numbers from 1 to 1000 and are independent of each other.

9. The low-ring hydrophilic amino silicone oil according to claim 8, characterized in that: The chemical structural formula of the hydrophilic amino silicone oil includes but is not limited to the following: , , , , , , Any one of the following; a, b, c are natural numbers ranging from 1 to 1000.

10. A hydrophilic silicone softener, characterized in that: The invention relates to an amino silicone oil prepared by the method according to any one of claims 1 to 7 or an amino silicone oil according to claim 8 or 9.

Citation Information

Cited By

  • Preparation method of low-ring-body high-hydroxyl siloxane polymer

    CN121226734A