Gas shield welding process suitable for 1000MPa hydroelectric steel

By adopting the 1000MPa gas-protective welding technology for hydropower in the field of hydropower, the problem of equal strength matching and welder operationality of high-strength steel welding materials is solved, the welding effect and underwater application strength are guaranteed, and the welding wire preparation method is provided. Simplified welding process.

CN119035706APending Publication Date: 2024-11-29CHINA THREE GORGES PROJECTS DEV CO LTD +1

Patent Information

Application Number
CN202411033148.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

In the field of hydropower, there are problems with strong matching, welder operability and impact toughness in the welding technology of 1000MPa grade high-strength steel plates, and domestic welding materials lack preparation methods, making it difficult to obtain suitable welding wires.

Method used

Adopt the welding process suitable for 1000MPa water and electricity steel gas welding, including inspection of base material and welding wire, preheating, heat input control, determination of base and fill cover welding process parameters, as well as post-weld heat treatment to ensure welding effect and water Application intensity.

Benefits of technology

The non-destructive detection of welds and the mechanical properties comply with technical specifications, solve the problems of strong matching, welder operability, and impact toughness such as high-strength steel welding materials, and provide welding wire preparation methods, simplifying the welding process.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a gas shield welding process suitable for 1000MPa hydroelectric steel, which comprises the following steps of: determining that adopted materials meet use requirements through inspection of base metal and welding wires, and determining preheating temperature and backing welding process parameters used by the welding process through an iron grinding test; and filling cosmetic welding process parameters and post-welding dehydrogenation treatment temperature are determined through heat input control and post-welding heat treatment, and the welding effect of the 1000 MPa grade hydroelectric steel is guaranteed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of welding 1000MPa high-strength steel plates for pressure steel pipes and bifurcated pipes in water conservancy and hydropower engineering, in particular to a gas shielded welding process suitable for 1000MPa hydropower steel. Background Art

[0002] my country's hydropower units have been developing towards large drop and ultra-high head, which puts forward higher requirements on the strength, toughness and high plasticity of hydropower steel. Whether the performance of hydropower steel meets the standards directly affects the construction period and operation safety of hydropower stations. In order to meet the needs of hydropower station layout and reduce the comprehensive cost of the project, the application research of new materials will be an important topic. With the rapid development of science and technology, the construction of large and giant hydropower stations will continue to adopt new materials, new technologies and new processes. Hydropower steel is also developing in the direction of large-scale, high-strength, green and energy-saving. Domestic 1000MPa hydropower steel plates have also begun to be developed and produced, and the corresponding domestic welding materials are also being developed and developed.

[0003] Regarding the 1000MPa steel plate and the matching domestic welding materials for hydropower, the steel has the characteristics of high strength, high plasticity, high toughness and high weldability. In the welding of high-strength steel welding materials for hydropower, there are problems of equal strength matching, welder operability and impact toughness. However, this grade of steel plate has not been widely used, and there is a blank in how to weld in hydropower applications. It is necessary to ensure both the welding effect and the application strength in the hydropower field. At the same time, the performance test of the welding wire deposited metal is carried out according to the recommended welding process parameters. There are certain requirements on the performance of the welding materials during the welding process. There is a lack of preparation methods for this welding material in the industry and it is difficult to obtain it except by importing.

[0004] Therefore, there is an urgent need for a gas shielded welding process suitable for 1000MPa hydropower steel. Summary of the invention

[0005] The present invention provides a gas shielded welding process suitable for 1000MPa hydropower steel, aiming to solve the above-mentioned problems of lack of a welding process for 1000MPa hydropower high-strength welding materials that can ensure both welding effect and underwater application strength and difficulty in obtaining welding wire.

[0006] In order to solve the above technical problems, the technical solution adopted by the present invention is: A gas shielded welding process for 1000MPa hydroelectric steel, comprising the following steps: Step 1: Parent material inspection: According to the quality requirements of 1000MPa grade hydropower steel, the parent material is tested for tensile strength, yield strength, elongation after fracture and -60℃ impact energy, where the tensile strength is ≥950MPa, the yield strength is ≥890MPa, the elongation after fracture is ≥14%, and the average impact energy at -60℃ is ≥70J; Step 2: Preparation and inspection of welding wire. Conduct welding wire deposited metal performance test according to recommended welding process parameters. The tensile strength of welding wire is ≥950MPa, the yield strength is ≥890MPa, the elongation after fracture is ≥14%, and the average impact energy at -40℃ is ≥47J. Step 3: Preheating: determine the preheating temperature according to the iron research test and preheat, the preheating temperature is ≥100℃; Step 4: Determine the heat input range, the heat input range is: 10.8-23.5kJ / cm; Step 5: Base gas shielded welding, the process parameters are current 100~130A, voltage 15~20V, welding speed 10~15cm / min; Step 6: Filling and covering gas shielded welding, the process parameters are current 105~160A, voltage 16~25V, welding speed 10~15cm / min; Step 7: Post-weld heat treatment.

[0007] Preferably, the heat input determination in Step 4 includes the following steps: conducting welding joint tests under different heat inputs through a determined base welding process and preheating temperature, and performing nondestructive testing and performance testing after welding, wherein the joint strength of the heat input used is ≥950MPa, the bending performance is qualified, and the -40°C weld and heat-affected zone impact average is ≥47J.

[0008] Preferably, the protective gas used in Step 5 and Step 6 is 85% Ar+15% CO2.

[0009] Preferably, the welding power source used in Step 5 and Step 6 is a pulse arc welding machine, and the current type is reverse direct current.

[0010] Preferably, the interlayer temperature in Step 5 and Step 6 is 150±25°C.

[0011] Preferably, the post-weld heat treatment in Step 7 is a dehydrogenation process, and the process parameters are a temperature of 150-250° C. and a time of 2 hours.

[0012] Preferably, the welding wire preparation method in Step 2 further comprises the following steps: Step 201: After the molten iron is processed in the converter process, it enters the refining furnace for refining, and then produces square billets through the continuous casting process; Step 202: The billet is then rolled into the required round welding wire through a rolling process; Step 203: Heat treat the welding wire to improve the performance of the welding wire; Step 204: The welding wire after heat treatment is acidified to remove the oxide layer and other impurities on the surface; Step 205: The welding wire after acid treatment is rough-drawn and fine-drawn to reduce the diameter; Step 206: copper plating is performed on the welding wire after drawing to improve the conductivity and welding performance of the welding wire; Step 207: After copper plating, the welding wire is degreased on the surface to ensure cleanliness during welding.

[0013] More preferably, the heat treatment in Step 203 includes a primary heat treatment and a secondary heat treatment; The parameters of the primary heat treatment are temperature 850~900℃, time 10~20min; The parameters of the secondary heat treatment are temperature 750~820℃ and time 10~30min.

[0014] Beneficial effects of the present invention: 1. The present invention has developed a matching gas shielded welding process based on the characteristics of the steel plate. The non-destructive testing and mechanical properties of the welds meet the requirements of technical specifications. This technology overcomes the difficulties of strong matching of hydropower high-strength steel welding materials, welder operability, and impact toughness; 2. The present invention provides a corresponding welding wire preparation method according to the parameter requirements of the welding wire, which facilitates welding to obtain the welding wire and facilitates actual welding while ensuring welding. DETAILED DESCRIPTION

[0015] As follows, the embodiments are further described.

[0016] As a preferred embodiment 1: A gas shielded welding process for 1000MPa hydroelectric steel, comprising the following steps: 1. Inspection of parent materials: According to the quality requirements of 1000MPa grade hydropower steel, the tensile strength, yield strength, elongation after fracture and -60℃ impact energy tests shall be carried out. The tensile strength shall be ≥950MPa, the yield strength shall be ≥890MPa, the elongation after fracture shall be ≥14%, and the average impact energy at -60℃ shall be ≥70J.

[0017] 2. Preparation and inspection of welding wire, The preparation of welding wire needs to start with high-quality molten iron. After the molten iron is processed in the converter process, it enters the refining furnace for refining, and then the billet is produced through the continuous casting process. The billet is then rolled into the required coil through the rolling process. The performance of the welding wire is improved by heat treatment. The first heat treatment is usually carried out at 850-900℃ for 10-20 minutes, and the second heat treatment is carried out at 750-820℃ for 10-30 minutes. The heat-treated material is acidified to remove the oxide layer and other impurities on the surface. After that, it is rough-drawn and fine-drawn to reduce the diameter to meet the specifications of high-strength steel welding wire. In order to improve the conductivity and welding performance of the welding wire, copper plating is carried out on the high-strength steel welding wire after drawing. High-strength steel welding wire also needs to be degreased during the production process to ensure cleanliness during welding. The welding wire deposited metal performance test is carried out according to the recommended welding process parameters, where the tensile strength is ≥950MPa, the yield strength is ≥890MPa, the elongation after fracture is ≥14%, and the average impact energy at -40℃ is ≥47J.

[0018] 3. Crack resistance and base welding process, Through the Tieyan test, different preheating temperatures are set to carry out the crack resistance test of the base welding. Under certain preheating temperature and welding process conditions, the cross-sectional crack rate of the Tieyan specimen is 0, and the base welding process and the required preheating temperature can be determined.

[0019] 4. Heat input control, Through the determined base welding process and preheating temperature, welding joint tests are carried out under different heat inputs, and non-destructive testing and performance tests are carried out after welding. The joint strength of the heat input used is ≥950MPa, the bending performance is qualified, and the impact average of the -40℃ weld and heat-affected zone is ≥47J. The heat input that meets the index requirements is within the heat input range used in the project.

[0020] 5. Post-weld heat treatment: Experiments with different heat treatment conditions show that 1000MPa grade hydropower steel should not be subjected to post-weld stress relief heat treatment after welding, which will cause the impact toughness of the weld and fusion line to drop seriously. However, high-strength steel above 1000MPa has a greater tendency to harden. In order to avoid hydrogen-induced delayed cracking, dehydrogenation treatment is required after welding to ensure that the joint meets the use requirements.

[0021] 6. Determine the welding process. Determine whether the base material and welding wire used meet the use requirements through inspection. Determine the preheating temperature and base welding process parameters used in the welding process through iron research test. Determine the filling and capping welding process parameters and post-weld dehydrogenation treatment temperature through heat input control and post-weld heat treatment.

[0022] As a preferred embodiment 2: The method of the present invention was used to test and study the domestic 80mm thick 1000MPa grade hydropower steel and Φ1.2mm ER120S-G welding wire. The welding method used in the test was MAG welding, the shielding gas was 85%Ar+15%CO2, and the welding power source was a pulse arc welding machine. The specific implementation is as follows: 1. Inspection of parent materials: The steel plate was tested three times as required. The results showed that the tensile strength was 1006MPa, the yield strength was 964MPa, the elongation after fracture was 18.5%, and the impact energy at -60℃ was 146J, 157J and 175J respectively, which met the requirements.

[0023] 2. Preparation and inspection of welding materials. The prepared welding wire was subjected to five cladding metal performance tests as required. The results showed that the tensile strength was 959 MPa, the yield strength was 892 MPa, the elongation after fracture was 16%, and the impact energy at -40°C was 72 J, 72 J, 68 J, 74 J and 72 J respectively, which met the requirements.

[0024] 3. Crack resistance and base welding process. Through the iron grinding test, three preheating temperatures of 75℃, 100℃ and 125℃ were set. The process parameters used for base welding were current 100~130A, voltage 15~20V, welding speed 10~15cm / min. Metallographic inspection was carried out on the cross sections of the iron grinding test at three preheating temperatures. The crack rate of the cross section of the iron grinding preheated to 75℃ was 50.8%, and the others were 0. Therefore, it was determined that the preheating temperature was ≥100℃, and the process used was for base welding.

[0025] 4. Heat input control. Prepare welding joints under different welding heat input conditions, cool to room temperature after welding, conduct non-destructive testing on the test plate 48 hours later, dissect the processing performance specimens after passing the test, and conduct performance testing. According to the test results, the heat input range is finally determined to be 10.8-23.5kJ / cm. Under this heat input, the joint strength is 965MPa, the bending performance is qualified, the impact energy of the weld at -40℃ is 70J, 71J, and 56J respectively, and the impact energy of the heat affected zone at -40℃ is 89J, 81J, and 95J respectively, which meet the index requirements.

[0026] 5. In terms of post-weld heat treatment, the welded joints were subjected to post-weld heat treatment under different conditions to avoid delayed cracks. In order to ensure the impact toughness, the welded joints after post-weld heat treatment were subjected to impact tests. Compared with the welded state, the impact absorption energy increased after post-weld dehydrogenation treatment, which could meet the index requirement of >47J. However, after stress relief heat treatment, the impact absorption energy decreased significantly, and decreased significantly with the increase of heat treatment temperature. According to the test results, the final dehydrogenation process was determined to be 150~250℃×2h.

[0027] 6. Based on the above test results, the welding process is finally determined as follows: Preheating temperature: ≥100℃ Interlayer temperature: 150±25℃ Welding machine: Pulse arc welding machine Post-heating: 150℃×2h Welding material: ER120S-G φ1.2mm Protective gas: 85%Ar+15%CO2 .

Claims

1. A gas shielded welding process suitable for 1000MPa hydropower steel, characterized in that: The following steps are involved: Step 1: Parent material inspection: According to the quality requirements of 1000MPa grade hydropower steel, the parent material is tested for tensile strength, yield strength, elongation after fracture and -60℃ impact energy, where the tensile strength is ≥950MPa, the yield strength is ≥890MPa, the elongation after fracture is ≥14%, and the average impact energy at -60℃ is ≥70J; Step 2: Preparation and inspection of welding wire. Conduct welding wire deposited metal performance test according to recommended welding process parameters. The tensile strength of welding wire is ≥950MPa, the yield strength is ≥890MPa, the elongation after fracture is ≥14%, and the average impact energy at -40℃ is ≥47J. Step 3: Preheating: determine the preheating temperature according to the iron research test and preheat, the preheating temperature is ≥100℃; Step 4: Determine the heat input range, the heat input range is: 10.8-23.5kJ / cm; Step 5: Base gas shielded welding, the process parameters are current 100~130A, voltage 15~20V, welding speed 10~15cm / min; Step 6: Filling and covering gas shielded welding, the process parameters are current 105~160A, voltage 16~25V, welding speed 10~15cm / min; Step 7: Post-weld heat treatment.

2. The gas shielded arc welding process for 1000MPa hydroelectric steel according to claim 1 is characterized in that: The heat input determination in Step 4 includes the following steps: conducting welding joint tests under different heat inputs through the determined base welding process and preheating temperature, and performing nondestructive testing and performance testing after welding, wherein the joint strength of the heat input used is ≥950MPa, the bending performance is qualified, and the impact mean of the -40°C weld and heat-affected zone is ≥47J.

3. The gas shielded arc welding process for 1000MPa hydroelectric steel according to claim 1 is characterized in that: The protective gas used in Step 5 and Step 6 is 85% Ar + 15% CO2.

4. The gas shielded arc welding process for 1000MPa hydroelectric steel according to claim 1 is characterized in that: The welding power source used in Step 5 and Step 6 is a pulse arc welding machine, and the current type is direct current reverse connection.

5. The gas shielded arc welding process for 1000MPa hydroelectric steel according to claim 1 is characterized in that: The interlayer temperature in Step 5 and Step 6 is 150±25°C.

6. The gas shielded arc welding process for 1000MPa hydroelectric steel according to claim 1 is characterized in that: The post-weld heat treatment in Step 7 is a dehydrogenation process, and the process parameters are a temperature of 150-250° C. and a time of 2 hours.

7. The gas shielded arc welding process for 1000MPa hydroelectric steel according to claim 1 is characterized in that: The welding wire preparation method in Step 2 further comprises the following steps: Step 201: After the molten iron is processed in the converter process, it enters the refining furnace for refining, and then produces square billets through the continuous casting process; Step 202: The billet is then rolled into the required round welding wire through a rolling process; Step 203: Heat treat the welding wire to improve the performance of the welding wire; Step 204: The welding wire after heat treatment is acidified to remove the oxide layer and other impurities on the surface; Step 205: The welding wire after acid treatment is rough-drawn and fine-drawn to reduce the diameter; Step 206: copper plating is performed on the welding wire after drawing to improve the conductivity and welding performance of the welding wire; Step 207: After copper plating, the welding wire is degreased on the surface to ensure cleanliness during welding.

8. The gas shielded arc welding process for 1000MPa hydroelectric steel according to claim 7 is characterized in that: The heat treatment in Step 203 includes primary heat treatment and secondary heat treatment; The parameters of the primary heat treatment are temperature 850~900℃, time 10~20min; The parameters of the secondary heat treatment are temperature 750~820℃ and time 10~30min.

Citation Information

Patent Citations

  • Welding method for high-strength seamless steel tube

    CN103990895A

  • Welding method of high-strength steel of 900 MPa level

    CN105014208A

  • Welding wire for silicon steel laser filler wire welding, preparation method of welding wire, and welding method

    CN108971797A

  • Gas shield welding method for 1000 MPa steel plate with thickness larger than or equal to 40 mm

    CN110076430A

  • Welding wire used for FCB method high heat input submerged arc welding and preparation thereof, welding flux and preparation of welding flux, welding material and application of welding material

    CN113695784A

Cited By

  • Welding wire special for 1000MPa-grade hydroelectric low-alloy high-strength steel and matched welding method of welding wire

    CN121928254A

  • Gas shielded welding method for 1000MPa rare earth hydroelectric steel plate

    CN122231413A