Modified glass fiber reinforced corundum-mullite castable and preparation method thereof
By modifying glass fiber reinforced silicon sol combined with corundum-mullite castable, a three-dimensional network structure is formed, which solves the problem of insufficient strength of silicon sol combined with castable at low temperatures, significantly improves the low- and high-temperature strength, and is suitable for large-scale industrial applications. .
Patent Information
- Application Number
- CN202411129618.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-08-16
AI Technical Summary
Silicone sol-bound corundum-mullite castable is low in strength at low temperatures, limiting its large-scale application.
Modified glass fibers are treated with high-temperature calcination and silane coupling agent to enhance the surface roughness and activity of glass fibers, combined with silica sol to form a three-dimensional network structure, and improve the low-temperature and high-temperature strength of the castable.
It significantly improves the low-temperature strength of the castable material, and improves the high-temperature strength and wear resistance, solves the problem of insufficient strength of the silicon sol combined with the castable material at low temperatures, and is suitable for large-scale industrial applications.
Smart Images

Figure BDA0004997439020000071
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of amorphous refractory materials, and in particular relates to a modified glass fiber reinforced corundum-mullite castable and a preparation method thereof. Background Art
[0002] The high temperature and high pressure smelting environment inside the blast furnace brings severe challenges to the safety and longevity of the blast furnace. The lining materials of blast furnaces, hot blast furnaces and other furnaces are usually cast by integrated construction of high-aluminum castables. However, during the operation of the equipment, due to the long-term severe mechanical scouring of high-temperature slag liquid and the erosion of various dust and smoke, the organizational structure of the furnace lining is easily damaged, resulting in cracks, bulges and other deformations in the lining material, and even large-scale shedding and collapse in severe cases, posing a serious threat to people's lives and property safety.
[0003] Corundum-mullite castables have excellent properties such as high high temperature strength, good thermal shock resistance, good structural spalling resistance, good thermal shock resistance, high load softening temperature, low high temperature creep rate, and good chemical corrosion resistance. They are widely used in linings of blast furnaces, hot blast furnaces, etc. The binder of corundum-mullite castables on the market is mainly aluminate cement, etc., which has the advantages of high early strength and rheological properties, but the low high temperature strength and long construction period limit the large-scale use of aluminate cement combined with mullite-corundum castables. In recent years, with the continuous application and development of nanotechnology in the metallurgical industry, silica sol as a castable binder has become one of the research hotspots at home and abroad. For example, Xiong Jiquan et al. studied the characteristics and application of silica sol combined with corundum-silicon carbide castables. The results showed that the castables have high high-temperature strength, good resistance to slag erosion, good thermal shock stability and rapid baking performance (Bulletin of Silicates, Vol. 32, No. 8, 2013, 1688-1692); Wang Xitang et al. studied the rheological properties of silica sol combined with corundum refractory castables. The results showed that the type of Al2O3 powder affects the slurry stability. Qualitative, the castable has good fluidity, and its high temperature flexural strength is higher than that of cement-bonded corundum castable (Rare Metal Materials and Engineering, 2009, Vol. 38, Supplement 2); Xu Yong et al. summarized the performance research and application status of silica sol-bonded amorphous refractory materials. Silica sol-bonded refractory materials have many excellent properties due to the presence of nano-SiO2, such as good medium and high temperature strength, good resistance to slag erosion and good thermal shock resistance, and can be quickly dried and baked, saving time for normal production, energy saving and environmental protection (Refractory Materials, 2014, Vol. 48, No. 5, 391-396). Compared with aluminate cement, silica sol as a binder does not introduce Ca into the system. 2+, can avoid the formation of low-melting materials such as calcium feldspar, calcium aluminum feldspar, tricalcium aluminate at high temperatures, significantly enhance its high-temperature strength and corrosion resistance, and at the same time, the use of silica sol does not produce hydration products, less crystal water, the castable can be quickly constructed and baked, greatly shortening the construction period, etc. However, a major problem with silica sol-bonded castables is that their strength is very low at low temperatures. This is because the low-temperature strength of the castable is mainly provided by the condensation reaction of a small amount of siloxane alcohol groups (-Si-OH). In this reaction, it is only the reorganization of the molecular bonds between silica sol particles, thereby forming a siloxane space network structure, and the degree of spontaneous condensation reaction of -Si-OH is low, and the resulting bonding force is weak, resulting in the inability of the particles to bond tightly together. Therefore, the low-temperature strength of silica sol-bonded castables is low, which also seriously limits the large-scale promotion and application of silica sol-bonded refractory castables. Summary of the invention
[0004] The purpose of the present invention is to provide a modified glass fiber reinforced corundum-mullite castable and a preparation method thereof in view of the deficiencies in the prior art. The obtained corundum-mullite castable has higher low-temperature strength, overcomes the disadvantage of low low-temperature strength of silica sol combined with corundum-mullite, and improves its high-temperature performance, which is conducive to large-scale industrial application of silica sol combined with corundum-mullite castable.
[0005] In order to solve the above technical problems, the present invention adopts the following technical solutions:
[0006] Provided is a modified glass fiber reinforced silica sol combined with corundum-mullite casting material, wherein the raw materials include, by mass percentage: 38-48% of dense corundum particles, 20-30% of mullite particles, 16-20% of dense corundum powder, 2-5% of silicon micropowder, 5-10% of activated alumina powder, 1-3% of composite additives, 0.05-0.15% of water reducing agent, 0.2-0.6% of modified glass fiber, and 7.5-8.5% of silica sol; wherein:
[0007] The modified glass fiber is prepared by high-temperature calcining the glass fiber at a temperature of 350-400° C., adding the glass fiber into a solution containing a silane coupling agent, immersing the solution under stirring, and then ultrasonically treating the solution.
[0008] According to the above scheme, the high temperature burning time is 1.5 to 3 hours; the soaking time is 0.5 to 1 hour; and the ultrasonic treatment time is 1 to 3 hours.
[0009] According to the above scheme, the length of the glass fiber is 3-6 mm and the diameter is 0.05-0.1 mm.
[0010] According to the above scheme, the silane coupling agent is one of KH-570, KH-560 and KH-550.
[0011] According to the above scheme, in the solution containing silane coupling agent, the mass percentage of silane coupling agent is 10-20%.
[0012] According to the above scheme, the dense corundum particles are mixed by three types of dense corundum particles with particle sizes of 5-3mm, 3-1mm, and 1-0mm in a mass ratio of 1:(2.5-3.5):(2.5-3); wherein the Al2O3 content is ≥98%.
[0013] According to the above scheme, the mullite particles are formed by mixing three types of mullite particles with particle sizes of 5-3mm, 3-1mm and 1-0mm in a mass ratio of 1:(2.5-3.5):(2.5-3); wherein the Al2O3 content is ≥60%.
[0014] According to the above scheme, the SiO2 in the silicon micropowder is ≥96% and the particle size is ≤5μm.
[0015] According to the above scheme, the Al2O3 content in the activated alumina powder is ≥98% and the particle size is ≤1.5μm.
[0016] According to the above scheme, the composite additive is a mixture of magnesium oxide and boron carbide; preferably, the mass ratio of magnesium oxide to boron carbide is 1:(1.5-3).
[0017] According to the above scheme, the particle size of the composite additive is ≤0.088mm.
[0018] According to the above scheme, the water reducer is one or more of sodium hexametaphosphate, sodium pyrophosphate, and sodium tripolyphosphate; preferably, the particle size of the water reducer is ≤0.074 mm.
[0019] According to the above scheme, the mass fraction of SiO2 in the silica sol is 20-35%, and the particle size of the particles is 5-30nm.
[0020] Provided is a method for preparing a modified glass fiber reinforced silica sol combined with corundum-mullite castable, comprising the following steps:
[0021] The weighed dense corundum particles, mullite particles, dense corundum powder, silica powder, activated alumina powder, composite additives, water reducer and modified glass fiber are mechanically stirred and mixed into dry uniform aggregate, and then silica sol is added, and after fully mixing and stirring, pouring construction can be carried out.
[0022] The present invention provides a modified glass fiber reinforced silica sol combined with corundum-mullite castable. The modified glass fiber is combined with silicon micropowder, activated alumina powder, composite additives and water reducing agent, which effectively improves the low-temperature strength of the silica sol combined with corundum-mullite castable, and at the same time improves the high-temperature strength and wear resistance; specifically, it is embodied as follows:
[0023] The modified glass fiber is modified by sintering the glass fiber and grafting the silane coupling agent to make its surface rougher and contain a large amount of -OH; on the one hand, the modified glass fiber is added to the silica sol combined castable, and its rough surface increases the interface friction, improves the bonding performance of the fiber and the powder, and forms a force-bearing skeleton, strengthening the connection between the refractory powder and the silica sol. When the castable is subjected to external stress, the modified fiber can effectively share part of the load and prevent the crack from further expanding, and the fracture path of the material is lengthened, so that the low-temperature strength is improved; on the other hand, the silane coupling agent is modified, physically adsorbed on the surface of the glass fiber and chemically grafted with the glass fiber. The surface of the modified glass fiber has a large amount of active -OH, which undergoes a dehydration condensation reaction with Si-OH in the silica sol (Si-OH+HO-R-=-Si-OR-+H2O), further accelerating the formation of a three-dimensional network structure of the silica sol, so that the low-temperature strength of the castable is significantly improved.
[0024] At the same time, the modified glass fiber is more tightly bonded to the powder due to its rough surface, which reduces the porosity of the castable on the one hand. When calcined at high temperature, the sintering degree between the castable particles is higher, and its high temperature performance is better. On the other hand, the main component of glass fiber is SiO2. The close combination of modified glass fiber and powder is also more conducive to the formation of needle-shaped or prismatic mullite phases by SiO2 of glass fiber and Al2O3 in raw materials at high temperature. Mullite intersperses and interlaces with each other, thereby significantly improving the high temperature strength and wear resistance of the castable. In addition, the liquid phase formed by the very little Na in the modified glass fiber prompts the particles to fill the gaps, which is conducive to promoting the sintering between particles, improving the stacking degree of the castable, and significantly improving the high temperature strength and wear resistance of the castable.
[0025] The beneficial effects of the present invention are as follows:
[0026] 1. The present invention provides a modified glass fiber reinforced silica sol combined with corundum-mullite castable. The modified glass fiber has a rough surface and contains a large amount of -OH. The addition of silica sol combined with corundum-mullite castable can be used as a load-bearing skeleton to enhance the bonding effect with powder and silica sol, showing obvious physical enhancement, and can also react with silica sol to form a three-dimensional network structure to show chemical enhancement. The physical and chemical dual enhancement significantly improves the low-temperature strength of the castable; at the same time, the modified glass fiber has good bonding with the powder, reduces the porosity, and is conducive to the generation of mullite phase, thereby improving the high-temperature strength and wear resistance of the castable; the present invention effectively improves the low-temperature strength, high-temperature strength, porosity and wear resistance of the silica sol combined corundum-mullite castable by combining a very small amount of modified glass fiber with silicon powder, activated alumina powder, composite additives and water reducer, and has low price, basically no impurities are introduced, and has important application potential.
[0027] 2. The preparation process of the mullite-corundum castable of the present invention is simple and effective, has low equipment requirements, and can be used for large-scale industrial production. DETAILED DESCRIPTION
[0028] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0029] The specific indicators of the raw materials in the embodiments of the present invention are as follows:
[0030] The dense corundum particles are prepared by mixing three types of dense corundum particles with particle sizes of 5-3 mm, 3-1 mm and 1-0 mm in a mass ratio of 1:(2.5-3.5):(2.5-3); wherein the Al2O3 content is ≥98%.
[0031] The mullite particles are formed by mixing three types of mullite particles with particle sizes of 5-3mm, 3-1mm and 1-0mm in a mass ratio of 1:(2.5-3.5):(2.5-3); wherein the Al2O3 content is ≥60%.
[0032] The silicon micropowder contains SiO2≥96% and a particle size≤5μm.
[0033] The Al2O3 content of the activated alumina powder is ≥98%, and the particle size is ≤1.5 μm.
[0034] The composite additive is a mixture of magnesium oxide and boron carbide, with a mass ratio of 1:2 and a particle size of ≤0.088 mm.
[0035] The water reducing agent is sodium hexametaphosphate, and the particle size of the water reducing agent is ≤0.074 mm.
[0036] The mass fraction of SiO2 in the silica sol is 20-35%, and the particle size is 5-30nm.
[0037] The modified glass fiber is prepared by calcining the glass fiber at a temperature of 350-400° C., adding the glass fiber to a solution containing a silane coupling agent, mixing the mixture evenly, and then ultrasonically treating the mixture; wherein:
[0038] The glass fiber has a length of 3-6 mm and a diameter of 0.05-0.1 mm;
[0039] The silane coupling agent is one of KH-570, KH-560 and KH-550;
[0040] In the solution containing the silane coupling agent, the mass percentage of the silane coupling agent is 10-20%.
[0041] The casting material in the embodiment is prepared by the following method:
[0042] The weighed dense corundum particles, mullite particles, dense corundum powder, silica powder, activated alumina powder, composite additives, water reducer and modified glass fiber are mechanically stirred and mixed into dry uniform aggregate, and then silica sol is added externally. After fully mixing and stirring, pouring construction can be carried out.
[0043] Example 1
[0044] Provided is a modified glass fiber reinforced corundum-mullite castable, wherein the components and their mass percentages are as follows:
[0045] Dense corundum particles 40%, mullite particles 25%, dense corundum powder 19%, silica powder 4%, activated alumina powder 10%, composite additives 1.53%, sodium hexametaphosphate 0.07%, modified glass fiber 0.4%, and added silica sol 7.8%.
[0046] The modified glass fiber production method is as follows: the glass fiber is placed in a muffle furnace and calcined at 400°C for 2 hours, and then the calcined glass fiber is soaked in 15% KH-570 by mass for about 30 minutes, the solution is continuously stirred to make it evenly mixed, and ultrasonically treated at room temperature for 2 hours, the filtrate is removed, and the glass fiber is washed with ethanol for 3 times, and then placed in an oven at 110°C for drying before use.
[0047] According to the above formula, the castable is packaged into two components (powder and silica sol) and transported to the construction site. The powder and silica sol are mixed and stirred evenly according to proportion to obtain the corundum-mullite castable, which can be used for blast furnace and hot blast furnace lining casting construction.
[0048] The performance test results of the corundum-mullite castable obtained in this example are shown in Table 1.
[0049] Comparative Example 1
[0050] According to the preparation method of Example 1, the modified glass fiber is not added to prepare the corundum-mullite castable, and the components and their mass percentages are: dense corundum particles 40%, mullite particles 25%, dense corundum powder 19.4%, silicon powder 4%, activated alumina powder 10%, composite additives 1.53%, sodium hexametaphosphate 0.07%, and added silica sol 7.8%.
[0051] The performance test results of the corundum-mullite castable obtained in this comparative example are shown in Table 1.
[0052] Example 2
[0053] The modified glass fiber reinforced corundum-mullite castable, each component and its mass percentage are: the modified glass fiber reinforced corundum-mullite castable, each component and its mass percentage are: 38% dense corundum particles, 28% mullite particles, 19% dense corundum powder, 4% silicon powder, 9% active alumina powder, 1.73% composite additives, 0.07% sodium hexametaphosphate, 0.2% modified glass fiber, and 8% silica sol. The modified glass fiber is prepared by placing the glass fiber in a muffle furnace and calcining it at 400°C for 2h, then soaking the calcined glass fiber in KH-570 with a mass fraction of 15% for about 30 minutes, stirring the solution continuously to make it evenly mixed, ultrasonically treating it at room temperature for 2h, removing the filtrate, washing it with ethanol 3 times, and drying it in an oven at 110°C for use.
[0054] The performance test results of the mullite castable prepared in this embodiment are shown in Table 1.
[0055] Comparative Example 2
[0056] According to the preparation method of Example 2, a corundum-mullite castable is prepared without adding modified glass fiber, and the components and their mass percentages are: dense corundum particles 38%, mullite particles 28%, dense corundum powder 19.2%, silicon micropowder 4%, activated alumina powder 9%, composite additives 1.73%, sodium hexametaphosphate 0.07%, and added silica sol 8%.
[0057] The performance test results of the corundum-mullite castable obtained in this comparative example are shown in Table 1.
[0058] Example 3
[0059] The modified glass fiber reinforced corundum-mullite castable has the following components and their mass percentages: 45% dense corundum particles, 25% mullite particles, 16% dense corundum powder, 3% silicon powder, 8% active alumina powder, 2.3% composite additives, 0.1% sodium hexametaphosphate, 0.6% modified glass fiber, and 8.1% silica sol. The modified glass fiber is prepared by calcining the glass fiber at 400°C in a muffle furnace, and then soaking the calcined glass fiber in 15% KH560 by mass for about 30 minutes, stirring the solution constantly to make it uniformly mixed, ultrasonically treating it at room temperature for 2 hours, removing the filtrate, washing it with ethanol for 3 times, and drying it in an oven at 110°C for use.
[0060] The performance test results of the mullite castable prepared in this embodiment are shown in Table 1.
[0061] Comparative Example 3
[0062] According to the preparation method of Example 3, the glass fiber is added directly to the corundum-mullite castable without modification. The components and their mass percentages are: 45% dense corundum particles, 25% mullite particles, 16% dense corundum powder, 3% silica powder, 8% activated alumina powder, 2.3% composite additives, 0.1% sodium hexametaphosphate, 0.6% glass fiber, and 8.1% added silica sol.
[0063] The performance test results of the corundum-mullite castable obtained in this comparative example are shown in Table 1.
[0064] Comparative Example 4
[0065] The modified glass fiber reinforced corundum-mullite castable has the following components and their mass percentages: 45% dense corundum particles, 25% mullite particles, 15.8% dense corundum powder, 3% silicon powder, 8% active alumina powder, 2.3% composite additives, 0.1% sodium hexametaphosphate, 0.8% modified glass fiber, and 8.1% silica sol. The modified glass fiber is prepared by placing the glass fiber in a muffle furnace and calcining it at 400°C for 2h, then soaking the calcined glass fiber in KH-560 with a mass fraction of 15% for about 30 minutes, stirring the solution continuously to make it uniformly mixed, ultrasonically treating it at room temperature for 2h, removing the filtrate, washing it with ethanol 3 times, and drying it in an oven at 110°C for use.
[0066] The performance test results of the corundum-mullite castable obtained in this comparative example are shown in Table 1.
[0067] Comparative Example 5
[0068] The modified glass fiber reinforced corundum-mullite castable has the following components and their mass percentages: 45% dense corundum particles, 25% mullite particles, 16.5% dense corundum powder, 3% silicon powder, 8% active alumina powder, 2.3% composite additives, 0.1% sodium hexametaphosphate, 0.1% modified glass fiber, and 8.1% silica sol. The modified glass fiber is prepared by placing the glass fiber in a muffle furnace and calcining it at 400°C for 2h, then soaking the calcined glass fiber in KH-560 with a mass fraction of 15% for about 30 minutes, stirring the solution continuously to make it evenly mixed, ultrasonically treating it at room temperature for 2h, removing the filtrate, washing it with ethanol 3 times, and drying it in an oven at 110°C for use.
[0069] The performance test results of the corundum-mullite castable obtained in this comparative example are shown in Table 1.
[0070] Table 1. Performance test results of Examples 1-3 and Comparative Examples 1-5
[0071]
[0072] It can be seen from the data of Example 1 and Comparative Example 1, Example 2 and Comparative Example 2 in Table 1 that the flexural and compressive strengths of the corundum-mullite castable with modified glass fiber added in the present invention at low, medium and high temperatures are significantly higher than those of the corundum-mullite castable without modified glass fiber added, especially after drying at 110°C, the flexural and compressive strengths of the castable without modified glass fiber added are only about 5MPa and 22MPa, while the flexural and compressive strengths of the castable with modified glass fiber added are significantly enhanced, especially after curing at 110°C, the flexural and compressive strengths reach 9MPa and 30MPa or more, respectively. This is mainly because modified glass fiber is added. After the glass fiber is modified, its surface becomes rougher, the interface friction force increases, the bonding performance between the fiber and the powder is improved, and a stress skeleton is formed, which strengthens the connection between the refractory powder and the silica sol. When the castable is subjected to external stress, the modified fiber can effectively share part of the load and prevent the crack from further expanding, and the fracture path of the material is lengthened, so that the strength is improved. On the other hand, the modified glass fiber surface has a large number of active -OH groups after modification by silane coupling agent, which react with -Si-OH in silica sol by dehydration condensation, further accelerating the formation of a three-dimensional network structure of silica sol, and significantly improving the low-temperature strength of the castable. In addition, since the surface of the modified glass fiber is rough, the bonding force between the modified glass fiber and the castable particles is increased, so the porosity is significantly reduced compared with the castable without modified glass fiber. At the same time, after the corundum-mullite castable with modified glass fiber is heat-treated, because the main component of the modified glass fiber is SiO2, it is easy to generate needle-shaped or prismatic mullite phases with Al2O3 in the raw material at high temperature, and the mullite intersperses and interweaves with each other, which improves the high-temperature strength of the castable, and the line change rate after firing shows that the castable shrinks less and the volume is more stable. In addition, the liquid phase formed by the very small amount of Na in the modified glass fiber prompts the particles to fill the gaps, which is beneficial to promote the sintering between the particles, improve the stacking degree of the castable, and significantly improve the high-temperature strength of the castable.
[0073] Compared with Example 3-5, it can be seen that the flexural and compressive strengths of the corundum-mullite castable with the modified glass fiber at low, medium and high temperatures are significantly higher than those of the corundum-mullite castable with the unmodified glass fiber. This is mainly because the unmodified glass fiber has only a partial physical reinforcement effect. Although it can share part of the load of the castable, there is a bundle agent on the fiber surface, the surface is relatively smooth, and the bonding force with the powder in the castable is slightly poor. The addition of modified glass fiber can not only effectively share part of the load of the castable, but also has a rough surface and a large amount of active -OH, which undergoes a dehydration condensation reaction with the -Si-OH in the silica sol, further accelerating the formation of a three-dimensional network structure of the silica sol. Therefore, the strength is significantly higher than that of the corundum-mullite castable with the unmodified glass fiber. Comparing Example 3 with Comparative Examples 4 and 5, it can be seen that adding too much modified glass fiber will cause the fibers to be partially entangled and agglomerated in the castable, affecting the bonding between the fibers and the powder and the sol, resulting in a decrease in strength. Adding too little modified glass will not fully exert the reinforcing effect of the modified glass fiber, and the reinforcing effect is average. Therefore, adding an appropriate amount of modified glass fiber to the corundum-mullite castable has a significant positive effect on improving the strength of the corundum-mullite castable.
[0074] In summary, the present invention adds modified glass fiber to the corundum-mullite castable, and the low-temperature strength of the corundum-mullite castable is significantly improved compared to the castable without the modified glass fiber, and its high-temperature performance is improved at the same time, and the problem of low strength of the silica sol-bonded corundum-mullite castable at low temperature is effectively solved, which is conducive to the further promotion and application of the silica sol-bonded corundum-mullite castable. At the same time, the modified glass fiber added to the mullite-corundum castable itself is less, low in price, and basically no impurities are introduced, and it can directly react with the raw material at high temperature, and the castable has stable low-temperature and high-temperature performance. In addition, the preparation process of the mullite-corundum castable of the present invention is simple and effective, the equipment requirements are low, and large-scale industrial production can be carried out, with good economic benefits and broad development prospects.
[0075] It should be understood that those skilled in the art can make improvements or changes based on the above description, and all these improvements and changes should fall within the scope of protection of the appended claims of the present invention.
Claims
1. A modified glass fiber reinforced silica sol combined with corundum-mullite castable, It is characterized in that The raw materials include, by mass percentage: 38-48% of dense corundum particles, 20-30% of mullite particles, 16-20% of dense corundum powder, 2-5% of silicon powder, 5-10% of activated alumina powder, 1-3% of composite additives, 0.05-0.15% of water reducing agent, 0.2-0.6% of modified glass fiber, and 7.5-8.5% of silica sol; wherein: The modified glass fiber is prepared by high-temperature calcining the glass fiber at a temperature of 350-400° C., adding the glass fiber into a solution containing a silane coupling agent, immersing the solution under stirring, and then ultrasonically treating the solution.
2. The silica sol combined corundum-mullite castable according to claim 1, It is characterized in that The high temperature burning time is 1.5 to 3 hours; the soaking time is 0.5 to 1 hour; and the ultrasonic treatment time is 1 to 3 hours.
3. The silica sol combined corundum-mullite castable according to claim 1, It is characterized in that The length of the glass fiber is 3-6 mm and the diameter is 0.05-0.1 mm.
4. The silica sol combined corundum-mullite castable according to claim 1, It is characterized in that The silane coupling agent is one of KH-570, KH-560 and KH-550.
5. The silica sol combined corundum-mullite castable according to claim 1, It is characterized in that In the solution containing the silane coupling agent, the mass percentage of the silane coupling agent is 10-20%.
6. The silica sol combined corundum-mullite castable according to claim 1, It is characterized in that The dense corundum particles are prepared by mixing three types of dense corundum particles with particle sizes of 5 to 3 mm, 3 to 1 mm, and 1 to 0 mm in a mass ratio of 1: (2.5-3.5): (2.5-3); wherein Al 2 O 3 The content is ≥98%; the mullite particles are made of three types of mullite particles with particle sizes of 5-3mm, 3-1mm, and 1-0mm, mixed in a mass ratio of 1: (2.5-3.5): (2.5-3); wherein Al 2 O 3 content ≥60%。 7. The silica sol combined corundum-mullite castable according to claim 1, It is characterized in that The SiO in the silicon powder 2 ≥96%, particle size ≤5μm; Al in the activated alumina powder 2 O 3 content ≥ 98%, particle size ≤ 1.5 μm; SiO 2 The mass fraction is 20-35% and the particle size is 5-30nm.
8. The silica sol combined corundum-mullite castable according to claim 1, It is characterized in that The composite additive is a mixture of magnesium oxide and boron carbide.
9. The silica sol combined corundum-mullite castable according to claim 1, It is characterized in that The water reducing agent is one or more of sodium hexametaphosphate, sodium pyrophosphate and sodium tripolyphosphate.
10. A method for preparing the silica sol combined corundum-mullite castable as claimed in claim 1, It is characterized in that The following steps are involved: The weighed dense corundum particles, mullite particles, dense corundum powder, silica powder, activated alumina powder, composite additives, water reducer and modified glass fiber are mechanically stirred and mixed into dry uniform aggregate, and then silica sol is added, and after fully mixing and stirring, pouring construction can be carried out.
Citation Information
Patent Citations
Preparation and method of silicon dioxide aerogel composite material
CN102557577A
Method for preparing ceramic membrane from bauxite and silicon dioxide
CN114573326A
Preparation method of high-temperature wear-resistant castable containing fused alumina zirconia
CN115448703A
Rare earth oxide modified corundum-mullite castable as well as use method and application thereof
CN115893994A
Production of ceramic composite material
JP1990258679A
Cited By
Preparation method of porous nano calcium silicate thermal insulation material
CN119219388A