Iron-based high-temperature alloy and preparation method thereof
By reasonably selecting chemical components and process flows in iron-based high-temperature alloys, the problem of insufficient performance of iron-based high-temperature alloys is solved, and the improvement of high-temperature long-lasting performance and cost control are achieved to meet the high-temperature application needs of aircraft engines.
Patent Information
- Application Number
- CN202411006096.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing iron-based high-temperature alloys are insufficient in aircraft engine applications and are difficult to meet the ever-increasing high-temperature load-bearing and cost control requirements.
By reasonably selecting and controlling the chemical components (C, Cr, Ni, Mo, Ti, B, V, Al, Co, etc.) in iron-based high-temperature alloys, combined with vacuum induction, electroslag remelting, forging and heat treatment processes, prepare Iron-based high-temperature alloy with excellent high-temperature durability is produced.
The room temperature tensile strength of the alloy is achieved to reach 1120~1190MPa, and the high-temperature long-lasting life of 80~120 hours at 650℃ is maintained, meeting the high-temperature performance needs of aircraft engines and reducing costs.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of alloy material preparation, and in particular relates to an iron-based high-temperature alloy and a preparation method thereof. Background Art
[0002] According to the type of matrix elements, high-temperature alloys are divided into three categories: iron-based, nickel-based, and cobalt-based high-temperature alloys. Iron-based high-temperature alloys are developed by adding alloying elements to the iron-nickel-chromium matrix. Depending on the added elements, controlling the element content and taking appropriate processing technology, alloys with special properties such as high strength, high toughness, high durability, wear resistance, corrosion resistance, low temperature resistance, high temperature resistance, and non-magneticity can be obtained to adapt to different application scenarios. They have been widely used in combustion chambers, turbine disks, casings, fasteners and other parts.
[0003] With the continuous updating and iteration of aircraft engines, the performance level requirements for high-temperature alloys are getting higher and higher. Although nickel-based alloys have a wider range of applications and cobalt-based alloys have stronger temperature resistance, iron-based alloys have low costs and my country has abundant iron resources. Increasing the proportion of iron-based alloys used in aircraft engines can achieve the goal of reducing costs and reducing the import of alloy materials.
[0004] Therefore, it is necessary to develop iron-based high-temperature alloys with better comprehensive performance. Summary of the invention
[0005] The object of the present invention is to provide an iron-based high-temperature alloy and a preparation method thereof. The provided iron-based high-temperature alloy has an average room temperature tensile strength of 1120-1190 MPa and an average high-temperature endurance life of 80-120 h at 650°C and 448 MPa.
[0006] In order to achieve the above-mentioned object of the invention, the technical solution adopted by the present invention is: An iron-based high-temperature alloy, whose chemical composition by weight percentage is: C: 0.02-0.06%, Cr: 13.5-16%, Ni: 24-27%, Mo: 1.0-1.5%, Ti: 1.9-2.35%, B: 0.003-0.01%, V: 0.1-0.5%, Al: 0.1-0.35%, Mg: 0.001-0.1%, Co: 0.01-0.1%, and the balance is Fe.
[0007] The specification of the iron-based high-temperature alloy of the present invention is φ165-200mm.
[0008] The preparation method of the iron-based high-temperature alloy of the present invention comprises vacuum induction, electroslag remelting, forging and heat treatment processes.
[0009] Furthermore, the forging process of the present invention is as follows: placing the electroslag ingot in a heating furnace and heating it to 1060°C-1120°C, and keeping it warm for 1.5-3h; then hot forging, with the start forging temperature ≥930°C, the final forging temperature ≥850°C, the deformation in the intermediate fire being controlled at 25%-45%, and the deformation in the final fire being controlled at 30%-45%.
[0010] Furthermore, the heating furnace in the forging process of the present invention is a chamber-type electric heating furnace.
[0011] Furthermore, the heat treatment process of the present invention is: the forged rod is subjected to solid solution and aging treatment, the solid solution system is 950-1000°C, heat preservation for 1-2 hours, and air cooling; the aging system is 700-720°C, heat preservation for 12-16 hours, and air cooling.
[0012] Furthermore, the heat treatment process described in the present invention is to load the furnace to the set temperature, and the timing starts when the temperature rises to the set temperature after loading the furnace.
[0013] The inventive principle of the technical solution of the present invention is: (1) Effects of various alloy elements ① In order to stabilize austenite, a certain amount of Ni is usually used for alloying to transform the ferrite matrix into a stable austenite matrix. The Ni content of the present invention is controlled at 24-27%.
[0014] ② Adding 13.5-16% Cr, the Cr in the austenite matrix of the high-temperature alloy causes lattice distortion, produces stress field strengthening, improves the strength of the austenite solid solution, and plays a role in solid solution strengthening. At the same time, Cr also reduces the solid solution stacking fault energy, which significantly improves the high-temperature endurance strength.
[0015] ③ Adding 1.0-1.5% Mo can significantly increase the Ni solid solution lattice constant and significantly increase the yield strength. In addition, the addition of Mo forms a large amount of M6C carbides in the alloy. These carbides are fine and dispersed, which can also play a strengthening role. At the same time, the addition of Mo can also refine the grains.
[0016] ④ Add 1.9-2.35% Ti. When Ti element is added to the alloy, about 10% enters the γ solid solution, which plays a certain solid solution strengthening role; about 90% enters the γ' phase to form Ni(Al,Ti), which plays a precipitation strengthening role, thereby increasing the room temperature and high temperature strength of the alloy.
[0017] ⑤ Add 0.1-0.35% Al. A certain amount of Al can form γ′ precipitation phase with Ni, which plays a precipitation strengthening role and improves the strength of the alloy.
[0018] ⑥ Add 0.003-0.01% B. B can form borides at the grain boundaries, hindering grain boundary sliding and improving grain boundary strength. However, too high a content will accelerate crack propagation and reduce plasticity and toughness. Therefore, the B content is controlled at 0.1-0.5%.
[0019] ⑦ Add 0.1-0.5% V. The addition of V to high-temperature alloys affects the lattice distortion and plays a significant role in solid solution strengthening. V in the alloy can increase the tensile strength and yield strength, refine the grains, improve hot working plasticity, and is beneficial to the improvement of notch sensitivity.
[0020] ⑧ Adding 0.01-0.1% Co can improve the strength, cause solid solution strengthening, reduce the stacking fault energy, reduce the creep rate and increase the creep resistance.
[0021] ⑨ Add 0.01-0.1% Mg to eliminate the brittleness caused by the segregation of harmful elements along the grain boundaries.
[0022] (2) Preparation method In terms of preparation technology, the deformation control range of the intermediate passes is large, which makes the forging process flexible and controllable. The large deformation in the final fire ensures the refinement of the grain structure. At the same time, combined with the solid solution aging process, the process flow is simple and the process controllability is good. It is suitable for the production lines of major smelters and forging plants and can achieve large-scale batch production.
[0023] The beneficial effects of the technical solution of the present invention are: The present invention achieves excellent high-temperature endurance performance while ensuring mechanical stability by controlling the types and contents of elements added to the alloy and improving the preparation method. The room temperature tensile strength of the alloy steel can reach 1120-1190 MPa, and the average endurance life at 650°C and 448 MPa reaches 80-120 hours. DETAILED DESCRIPTION
[0024] The present invention will be further described in detail below in conjunction with specific embodiments. Example 1
[0025] The iron-based high-temperature alloy of this embodiment has a specification of φ190 mm and a composition as shown in Table 1; its preparation method includes vacuum induction, electroslag remelting, forging, and heat treatment steps, which are specifically as follows: (1) Vacuum induction: The components are prepared according to the mass percentage of each component in Table 1, and then melted in a vacuum induction furnace and cast into an ingot; (2) Electroslag remelting: After the vacuum induction casting ingot is polished, electroslag remelting is performed to melt it into φ360mm electroslag ingot; (3) Forging: After the electroslag is loaded into the chamber electric heating furnace, the temperature is raised to 1060℃ and kept at this temperature for 3h; then hot forging is performed, the start forging temperature is ≥930℃, the first fire forging is to 260mm square, the deformation is 34%, the second fire forging is to 210mm square, the deformation is 35%, the third fire forging is to round the steel to φ190mm, the deformation is 36%, and the final forging temperature is ≥850℃; finally, it is placed in the semi-finished product area for air cooling.
[0026] (4) Heat treatment: The forged bars are subjected to solution treatment and aging treatment. ① Solution treatment: The heating furnace is heated to 950℃, and then the forged bars are placed in. After the furnace temperature stabilizes at 950℃, the bars are kept at this temperature for 2 hours and then taken out of the furnace for air cooling. ② Aging: The heating furnace is heated to 700℃, and then the forged bars are placed in. After the furnace temperature stabilizes at 700℃, the bars are kept at this temperature for 16 hours and then taken out of the furnace for air cooling.
[0027] Samples were taken at 1 / 2 radius of the iron-based high-temperature alloy rod prepared in this embodiment. After testing, the room temperature tensile strength was 1190 MPa, and the high-temperature endurance life at 650° C. and 448 MPa was 84 h. Example 2
[0028] The iron-based high-temperature alloy of this embodiment has a specification of φ165 mm and a composition as shown in Table 1; its preparation method includes vacuum induction, electroslag remelting, forging, and heat treatment steps, which are specifically as follows: (1) Vacuum induction: The components are prepared according to the mass percentage of each component in Table 1, and then melted in a vacuum induction furnace and cast into an ingot; (2) Electroslag remelting: After the vacuum induction casting ingot is polished, electroslag remelting is performed to melt it into φ360mm electroslag ingot; (3) Forging: After the electroslag is loaded into the chamber electric heating furnace, the temperature is raised to 1120℃ and kept warm for 1.5h; then hot forging is performed, the start forging temperature is ≥980℃, the first fire forging is to 260mm, the deformation is 34%, the second fire forging is to 210mm, the deformation is 35%, the third fire forging is to 180mm, the deformation is 26%, the fourth fire is to round the steel to φ165mm, the deformation is 34%, and the final forging temperature is ≥890℃; finally, it is placed in the semi-finished product area for air cooling.
[0029] (4) Heat treatment: The forged bars are subjected to solution treatment and aging treatment; ① Solution treatment: The heating furnace is heated to 980℃, and then the forged bars are placed in. After the furnace temperature stabilizes at 980℃, the bars are kept at this temperature for 1.5 hours and then air-cooled; ② Aging: The heating furnace is heated to 700℃, and then the forged bars are placed in. After the furnace temperature stabilizes at 700℃, the bars are kept at this temperature for 16 hours and then air-cooled.
[0030] Samples were taken at 1 / 2 radius of the iron-based high-temperature alloy rod prepared in this embodiment. After testing, the room temperature tensile strength was 1128 MPa, and the high-temperature endurance life at 650°C and 448 MPa was 121 h. Example 3
[0031] The iron-based high-temperature alloy in this embodiment has a specification of φ200 mm and a composition as shown in Table 1; its preparation method includes vacuum induction, electroslag remelting, forging, and heat treatment steps, which are specifically as follows: (1) Vacuum induction: The components are prepared according to the mass percentage of each component in Table 1, and then melted in a vacuum induction furnace and cast into an ingot; (2) Electroslag remelting: After the vacuum induction cast ingot is polished, electroslag remelting is performed to melt it into a φ360mm electroslag ingot; (3) Forging: After the electroslag is loaded into the chamber electric heating furnace, the temperature is raised to 1100℃ and kept at this temperature for 2h; then hot forging is performed, the start forging temperature is ≥950℃, the first fire forging is to 270mm, the deformation is 28%, the second fire forging is to 220mm, the deformation is 34%, the third fire rounding is φ200mm, the deformation is 35%, and the final forging temperature is ≥880℃; finally, it is placed in the semi-finished product area for air cooling.
[0032] (4) Heat treatment: The forged bars are subjected to solution treatment and aging treatment; ① Solution treatment: The heating furnace is heated to 1000℃, and then the forged bars are placed in. After the furnace temperature stabilizes at 1000℃, the bars are kept at this temperature for 1 hour and then taken out of the furnace for air cooling; ② Aging: The heating furnace is heated to 720℃, and then the forged bars are placed in. After the furnace temperature stabilizes at 720℃, the bars are kept at this temperature for 12 hours and then taken out of the furnace for air cooling.
[0033] Samples were taken at 1 / 2 radius of the iron-based high-temperature alloy rod prepared in this embodiment. After testing, the room temperature tensile strength was 1123 MPa, and the high-temperature endurance life at 650° C. and 448 MPa was 115 h. Example 4
[0034] The iron-based high-temperature alloy of this embodiment has a specification of φ180 mm and a composition as shown in Table 1; its preparation method includes vacuum induction, electroslag remelting, forging, and heat treatment steps, which are specifically as follows: (1) Vacuum induction: The components are prepared according to the mass percentage of each component in Table 1, and then melted in a vacuum induction furnace and cast into an ingot; (2) Electroslag remelting: After the vacuum induction cast ingot is polished, electroslag remelting is performed to melt it into a φ360mm electroslag ingot; (3) Forging: After the electroslag is loaded into the chamber electric heating furnace, the temperature is raised to 1100℃ and kept at this temperature for 2h; then hot forging is performed, the start forging temperature is ≥950℃, the first fire forging is to 260mm, the deformation is 34%, the second fire forging is to 200mm, the deformation is 40%, the third fire forging is to φ180mm, the deformation is 36%, and the final forging temperature is ≥880℃; finally, it is placed in the semi-finished product area for air cooling.
[0035] (4) Heat treatment: The forged bars are subjected to solution treatment and aging treatment; ① Solution treatment: The heating furnace is heated to 970°C, and then the forged bars are placed in. After the furnace temperature stabilizes at 970°C, the bars are kept at this temperature for 1.5 hours, and then taken out of the furnace for air cooling; ② Aging: The heating furnace is heated to 710°C, and then the forged bars are placed in. After the furnace temperature stabilizes at 710°C, the bars are kept at this temperature for 14 hours, and then taken out of the furnace for air cooling.
[0036] Samples were taken at 1 / 2 radius of the iron-based high-temperature alloy rod prepared in this embodiment. After testing, the room temperature tensile strength was 1134 MPa, and the high-temperature endurance life at 650°C and 448 MPa was 98 h. Example 5
[0037] The iron-based high-temperature alloy in this embodiment has a specification of φ185 mm and a composition as shown in Table 1; its preparation method includes vacuum induction, electroslag remelting, forging, and heat treatment steps, which are as follows: (1) Vacuum induction: The components are prepared according to the mass percentage of each component in Table 1, and then melted in a vacuum induction furnace and cast into an ingot; (2) Electroslag remelting: After the vacuum induction cast ingot is polished, electroslag remelting is performed to melt it into a φ360mm electroslag ingot; (3) Forging: After the electroslag is loaded into the chamber electric heating furnace, the temperature is raised to 1110℃ and kept at this temperature for 2h; then hot forging is performed, with the start forging temperature ≥950℃. The first fire forging is performed to 260mm with a deformation of 34%, the second fire forging is performed to 200mm with a deformation of 40%, the third fire forging is performed to a roundness of φ185mm with a deformation of 33%, and the final forging temperature is ≥880℃; finally, it is placed in the semi-finished product area for air cooling.
[0038] (4) Heat treatment: The forged bars are subjected to solution treatment and aging treatment; ① Solution treatment: The heating furnace is heated to 970℃, and then the forged bars are placed in. After the furnace temperature stabilizes at 970℃, the bars are kept at this temperature for 1.5 hours and then taken out of the furnace for air cooling; ② Aging: The heating furnace is heated to 700℃, and then the forged bars are placed in. After the furnace temperature stabilizes at 700℃, the bars are kept at this temperature for 15 hours and then taken out of the furnace for air cooling.
[0039] Samples were taken at 1 / 2 radius of the iron-based high-temperature alloy rod prepared in this embodiment. After testing, the room temperature tensile strength was 1145 MPa, and the high-temperature endurance life at 650° C. and 448 MPa was 96 h. Example 6
[0040] The iron-based high-temperature alloy of this embodiment has a specification of φ170 mm and a composition as shown in Table 1; its preparation method includes vacuum induction, electroslag remelting, forging, and heat treatment steps, which are specifically as follows: (1) Vacuum induction: The components are prepared according to the mass percentage of each component in Table 1, and then melted in a vacuum induction furnace and cast into an ingot; (2) Electroslag remelting: After the vacuum induction casting ingot is polished, electroslag remelting is performed to melt it into φ360mm electroslag ingot; (3) Forging: After the electroslag is loaded into the chamber electric heating furnace, the temperature is raised to 1090℃ and kept warm for 2.5h; then hot forging is performed, the start forging temperature is ≥940℃, the first fire forging is to 260mm, the deformation is 28%, the second fire forging is to 220mm, the deformation is 34%, the third fire forging is to 185mm, the deformation is 29%, the fourth fire is to round the steel to φ170mm, the deformation is 34%, and the final forging temperature is ≥860℃; finally, it is placed in the semi-finished product area for air cooling.
[0041] (4) Heat treatment: The forged bars are subjected to solution treatment and aging treatment; ① Solution treatment: The heating furnace is heated to 970°C, and then the forged bars are placed in. After the furnace temperature stabilizes at 970°C, the bars are kept at this temperature for 1.5 hours, and then taken out of the furnace for air cooling; ② Aging: The heating furnace is heated to 720°C, and then the forged bars are placed in. After the furnace temperature stabilizes at 720°C, the bars are kept at this temperature for 13 hours, and then taken out of the furnace for air cooling.
[0042] Samples were taken at 1 / 2 radius of the iron-based high-temperature alloy rod prepared in this embodiment. After testing, the room temperature tensile strength was 1138 MPa, and the high-temperature endurance life at 650°C and 448 MPa was 104 h.
[0043] Table 1 Composition and content of iron-based high-temperature alloys in various examples (%) .
Claims
1. An iron-based high-temperature alloy, It is characterized in that The element composition and weight proportions of the iron-based high-temperature alloy are: C: 0.02-0.06%, Cr: 13.5-16%, Ni: 24-27%, Mo: 1.0-1.5%, Ti: 1.9-2.35%, B: 0.003-0.01%, V: 0.1-0.5%, Al: 0.1-0.35%, Mg: 0.001-0.1%, Co: 0.01-0.1%, and the balance is Fe.
2. An iron-based high-temperature alloy according to claim 1, It is characterized in that The specification of the iron-based high-temperature alloy is φ165-200mm.
3. The iron-based high-temperature alloy according to claim 1, It is characterized in that The room temperature tensile strength of the iron-based high-temperature alloy is 1120-1190 MPa, and the average endurance life at 650° C. and 448 MPa reaches 80-120 hours.
4. A method for preparing an iron-based high-temperature alloy according to any one of claims 1 to 3, It is characterized in that It includes vacuum induction, electroslag remelting, forging and heat treatment processes.
5. The method for preparing the iron-based high-temperature alloy according to claim 4, It is characterized in that The forging process comprises heating the electroslag ingot to 1060° C. to 1120° C. and keeping the temperature for 1.5 to 3 hours; and then hot forging, wherein the starting forging temperature is ≥ 930° C. and the final forging temperature is ≥ 850° C.
6. The method for preparing the iron-based high-temperature alloy according to claim 4 or 5, It is characterized in that In the forging process, the deformation amount in the intermediate fire is controlled at 25% to 45%, and the deformation amount in the final fire is controlled at 30% to 45%.
7. The method for preparing the iron-based high-temperature alloy according to claim 4, It is characterized in that The heat treatment process is to perform solid solution and aging treatment on the forged bars.
8. The method for preparing the iron-based high-temperature alloy according to claim 7, It is characterized in that The solid solution system is 950-1000° C., keeping warm for 1-2 hours, and air cooling.
9. The method for preparing the iron-based high-temperature alloy according to claim 7, It is characterized in that The aging system is 700-720° C., heat preservation for 12-16 hours, and air cooling.
Citation Information
Patent Citations
GH2674 alloy
CN101418420A
Heat treatment method for super-alloy electromagnetic stirring roller used in high-temperature environment
CN103409601A
Aging treatment method for improving high-temperature endurance performance of GH2132 bolt
CN107201431A
Large-size high-toughness GH2132 bar for aerospace and preparation method thereof
CN110408846A
GH2132 alloy and preparation method thereof
CN113684353A