Constant-temperature microcapsule PCM cool-feeling fabric and preparation method thereof
By using phase-change microcapsules and nylon fabric printing technology with bishell structure in cool-sensing fabrics, the durability and breathability of existing cool-sensing fabrics are solved, and more efficient temperature adjustment and stability are achieved. It is suitable for Extremely cold and high temperature environment.
Patent Information
- Application Number
- CN202411109938.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-29
AI Technical Summary
The existing cool fabrics have poor durability, and the large amount of phase-change microcapsules will reduce breathability, making it difficult to provide effective temperature adjustment in extremely cold and high temperature environments.
A constant temperature microcapsule PCM cool-sensing fabric was designed, and phase-changing microcapsules with bi-shell structure were used. The shell thickness and porosity were adjusted through chemical etching and magnetron sputtering technology, and combined with the printing technology of nylon fabrics, it achieved More efficient temperature regulation and stability.
It improves the long-term stability and mechanical strength of microcapsules, enhances the temperature adjustment effect, maintains the breathability of the fabric, and provides a more comprehensive temperature adjustment function without increasing the amount of phase-change microcapsules.
Smart Images

Figure CN119041224A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of PCM fabrics, and in particular to a constant temperature microcapsule PCM cool fabric and a preparation method thereof. Background Art
[0002] The phase change materials contained in thermoregulating textiles are a type of intelligent material that responds to temperature changes by absorbing or releasing heat. They can effectively improve the body temperature of the human body in high or cold environments, making it convenient for people to live and work outdoors. In the application of phase change materials in the textile field, there are mainly a series of problems such as leakage of phase change materials and poor wearing performance. As for the leakage problem of phase change materials, the most common practice is to use microcapsule technology to encapsulate phase change materials, and the preparation process is relatively mature. For the comfort of clothing fabrics, the microcapsule spinning method can effectively improve the feel and wearing performance of the fabric, but the number of microcapsules in the fiber is small, and the thermoregulating effect is limited. In special environments such as extreme cold and high temperature, functionality is often ranked before comfort.
[0003] Most cooling fabrics have poor durability of cooling effect, and the cooling effect may weaken over time and with the use of the fabric; while cooling fabrics with a large amount of phase change microcapsules added will reduce their air permeability. In order to solve the above problems, the present invention decides to design a constant temperature microcapsule PCM cooling fabric and its preparation method. Summary of the invention
[0004] In order to solve the above problems, the present invention provides a constant temperature microcapsule PCM cool fabric and a preparation method thereof.
[0005] A constant temperature microcapsule PCM cool fabric, which comprises 100% nylon fabric by mass percentage, wherein the nylon fabric is provided with a print that accounts for 40 to 70% of the area of the nylon fabric, wherein phase change microcapsules are added to the print, and the average distribution density of the phase change microcapsules is 15 to 50 g / m 2 .
[0006] Furthermore, the phase change microcapsule comprises an outer shell, an intermediate shell and a core material from the outside to the inside, wherein the thickness of the outer shell is 5 to 10 μm, the thickness of the intermediate shell is 30 to 40 μm, and the particle size of the core material is 70 to 100 μm.
[0007] Note: A shell that is too thin may not be able to provide sufficient mechanical strength and chemical stability, especially under high temperature or high pressure environments. On the other hand, a shell that is too thick will increase thermal resistance and reduce heat exchange efficiency. If the diameter of the microcapsules is too small, they may migrate in the storage medium due to Brownian motion, thus affecting the stability of the system; on the contrary, larger microcapsules may have a lower thermal response speed and a lower specific surface area.
[0008] Furthermore, the preparation method of the phase change microcapsule is:
[0009] Paraffin, Tween 80 and caprylic acid glyceride are heated to 50-60° C. in a mass ratio of 1:0.1-0.2:40 and mixed evenly to obtain a dispersed phase, and a water-soluble polymer is selected as a coagulation bath; the dispersed phase is formed into a core material in the form of micro-droplets with a particle size of 70-100 μm by a microfluidic device and the core material is dripped into the coagulation bath, so that the micro-droplet core material is coagulated at 4-8° C. and wrapped with an intermediate shell of a water-soluble polymer with a thickness of 30-40 μm to obtain a substrate;
[0010] Chemically etching the surface of the intermediate shell of the substrate using a 4-6 M NaOH solution at 20-25° C. for 40-60 min to obtain a substrate after surface etching;
[0011] Then, magnetron sputtering is used to deposit the shell on the surface of the substrate after surface etching. The vacuum degree before magnetron sputtering is 1.5-4.5×10 -4 Pa, the argon flow rate is 35-40 sccm, the gas pressure in the vacuum chamber is maintained at 0.4-0.8 Pa, the magnetron sputtering temperature is room temperature, the magnetron sputtering power is 180-220 W, and phase change microcapsules are obtained.
[0012] Description: The double-shell structure can provide an additional physical and chemical barrier to protect the phase change material from environmental factors such as temperature, humidity and chemical erosion, thereby improving the long-term stability and durability of the microcapsules; the single-shell phase change microcapsules can effectively store and release heat, while the chemical etching and deposition shell can further regulate heat conduction and heat diffusion, optimize the thermal properties of the microcapsules, and achieve more efficient temperature regulation. By precisely controlling the chemical etching and deposition process, the porosity and thickness of the outer layer can be adjusted, thereby controlling the release rate of the phase change material, achieving on-demand release, and improving the intelligent response effect of the microcapsules; the obtained double-shell structure can enhance the mechanical strength of the microcapsules, making them less likely to break during processing and use, thereby improving their applicability and reliability in various applications.
[0013] Furthermore, the water-soluble polymer is one of melamine urea-formaldehyde resin or polyacrylamide, and the shell is composed of a mixture of water-based polyurethane and CX-880 cross-linking agent in a mass ratio of 1:0.2-0.3.
[0014] Description: Melamine urea-formaldehyde resin can provide a stable chemical environment, reduce the leakage of the core material, protect the core material from the influence of external chemical factors, extend the service life of the phase change microcapsules, and improve the overall performance of the phase change microcapsules; polyacrylamide can effectively block moisture and other substances that may affect the performance of the phase change material, ensuring the long-term stability of the phase change material; the hydrophilic group of the water-based polyurethane can improve the air permeability of the phase change microcapsules, and the addition of the cross-linking agent can improve the mechanical properties of the water-based polyurethane and maintain the stability of the shell.
[0015] A method for preparing a constant temperature microcapsule PCM cool fabric as described in any one of the above, comprising the following steps:
[0016] S1. Weaving:
[0017] Nylon FDY is used for weft knitting with a weaving density of 36 to 40 needles per inch to obtain a woven fabric;
[0018] S2, Pre-order type:
[0019] The woven fabric is placed in a setting machine, and pre-set at 190-200° C. and 19-21 m / min for 1.5-2.5 min, and 245-255 g / L of nylon anti-yellowing powder is added to a water tank of the setting machine during the pre-setting process, and the water volume of the water tank is 80 L, to obtain a pre-set fabric;
[0020] S3, dyeing and finishing:
[0021] The pre-shaped fabric is subjected to acid dyeing and finishing at 95-100° C. for 50-60 minutes to obtain a dyed and finished fabric, and 3-5 g / L of a nylon anti-yellowing agent is added to the dyed and finished fabric after acid dyeing and finishing, and the fabric is subjected to heat preservation treatment at a temperature of 50-80° C. for 18-22 minutes to obtain an anti-yellowing fabric;
[0022] S4, drying:
[0023] The anti-yellowing fabric is dried at a temperature of 155 to 165° C., a speed of 27 to 29 m / min, and a time of 1 to 2 min to obtain a dried fabric;
[0024] S5, rotary screen PCM printing:
[0025] The dried fabric is subjected to rotary screen PCM printing by means of electromagnetic magnetic rod pressure, wherein the rotary screen mesh of the rotary screen PCM printing is 105 mesh, the magnetic rod is an N35 magnet, the magnetic rod model is No. 12, and the rotary screen printing speed is 29-31 m / min to obtain a printed fabric;
[0026] The dye liquor used for the rotary screen PCM printing comprises, by mass percentage, 44-46% of phase change microcapsules, 34-36% of CX-880 crosslinking agent, 0.05-0.15% of LD-4126 softener, 2-3% of PTF thickener, 0.1-0.3% of XR-500 curing agent, 0.1-0.3% of SRN-618 hydrophilic agent and the balance of water;
[0027] S6, Thermal Stability Baking:
[0028] Baking the printed fabric at 95-105° C. for 2-3 minutes to obtain a baked fabric;
[0029] S7, re-shaping:
[0030] The baked fabric is placed in a setting machine and set again at 145-155° C. and 15-20 m / min for 1.5-2.5 min to obtain a PCM cool fabric.
[0031] Furthermore, after obtaining the baking fabric in step S6, the baking fabric is subjected to a strengthening treatment, and the strengthening treatment method is as follows:
[0032] The printed side of the baking fabric is used as the base, and the base is divided into several 0.003-0.005m 2 The square area of 0.003~0.005m 2 The anti-dyeing baffles are spaced and distributed in each square area one by one, and the square areas corresponding to the printing area are all distributed with the anti-dyeing baffles,
[0033] After the distribution is completed, the phase change microcapsules are sprayed on the blank part of the baking fabric, the distance between the nozzle and the baking fabric is 40-60cm, the spray pressure is 0.2-0.5MPa, and the spray amount is 1.5-1.8 times the average distribution density of the phase change microcapsules added in the printing;
[0034] After the spraying is completed, the anti-dyeing baffle is removed, and the baked fabric is baked at 95-105°C for 2-3 minutes to complete the strengthening treatment.
[0035] Description: The phase change microcapsules on both sides of the fabric can respond to changes in the external environment and internal body temperature respectively, providing a more comprehensive temperature regulation function. By rationally designing the phase change microcapsules for staggered distribution on the non-printed side of the fabric, the amount of phase change microcapsules can be saved while improving the cooling performance without destroying the breathability. The evenly spaced distribution helps prevent the phase change microcapsules from aggregating in the fabric and forming thermal bridges, which may cause local overheating or reduce the overall thermal management performance.
[0036] Furthermore, in step S2, the nylon anti-yellowing powder is Revonox 608 anti-yellowing powder; and in step S3, the nylon anti-yellowing agent is LD-RPY anti-yellowing agent.
[0037] Description: The above anti-yellowing agent can effectively improve the yellowing resistance of cool fabrics.
[0038] Compared with the existing PCM cool fabric, the beneficial effects of the present invention are:
[0039] (1) The constant temperature microcapsule PCM cool fabric of the present invention improves the coolness value of the fabric by combining phase change microcapsules and CX-880 crosslinking agent, and attaches phase change microcapsules to the printed part of the fabric surface so that the phase change microcapsules absorb or release energy during the solid-liquid conversion process, thereby achieving the effect of temperature regulation.
[0040] (2) The constant temperature microcapsule PCM cooling fabric of the present invention is designed with double-shell phase change microcapsules. The double-shell structure can provide additional physical and chemical barriers to protect the phase change material from environmental factors such as temperature, humidity and chemical erosion, thereby improving the long-term stability and durability of the microcapsules; the single-shell phase change microcapsules can effectively store and release heat, and the chemical etching and deposition shell can further regulate heat conduction and heat diffusion, optimize the thermal properties of the microcapsules, and achieve more efficient temperature regulation. By precisely controlling the chemical etching and deposition process, the porosity and thickness of the outer layer can be adjusted, thereby controlling the release rate of the phase change material, achieving on-demand release, and improving the intelligent response effect of the microcapsules; the obtained double-shell structure can enhance the mechanical strength of the microcapsules, making them less likely to break during processing and use, thereby improving their applicability and reliability in various applications.
[0041] (3) The constant temperature microcapsule PCM cooling fabric of the present invention also sprays phase change microcapsules on the non-printed surface, so that the phase change microcapsules on both sides of the fabric can respond to changes in the external environment and internal body temperature respectively, providing a more comprehensive temperature regulation function. By rationally designing the phase change microcapsules on the non-printed surface of the fabric for staggered distribution, the amount of phase change microcapsules can be saved while improving the cooling performance without damaging the air permeability. The uniform staggered distribution helps prevent the phase change microcapsules from aggregating in the fabric and forming thermal bridges, which may cause local overheating or reduce the overall thermal management performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] Figure 1 This is a flow chart of the preparation of the PCM cool fabric of the present invention;
[0043] Figure 2 It is a placement diagram of the anti-dyeing baffle sheet strengthened by the present invention. DETAILED DESCRIPTION
[0044] In order to further illustrate the method and effect of the present invention, the technical solution of the present invention will be clearly and completely described in combination with experiments.
[0045] Example 1: A constant temperature microcapsule PCM cool fabric, comprising 100% nylon fabric by mass percentage, the nylon fabric is provided with a print that accounts for 55% of the nylon fabric area, the print is added with phase change microcapsules, and the average distribution density of the phase change microcapsules is 32g / m 2 The phase-change microcapsule includes an outer shell, an intermediate shell and a core material from the outside to the inside, wherein the thickness of the outer shell is 8 μm, the thickness of the intermediate shell is 35 μm, and the particle size of the core material is 80 to 90 μm;
[0046] The preparation method of the phase change microcapsule is as follows:
[0047] Paraffin, Tween 80 and caprylic acid glyceride are heated to 55° C. in a mass ratio of 1:0.15:40 and mixed evenly to obtain a dispersed phase, and a water-soluble polymer is selected as a coagulation bath; a microfluidic device is used to form a core material in the form of micro-droplets with a particle size of 80 to 90 μm from the dispersed phase and the core material is dripped into the coagulation bath, so that the micro-droplet core material is solidified at 6° C. and wrapped with an intermediate shell of a water-soluble polymer with a thickness of 35 μm to obtain a substrate; wherein the micro-droplets can be spherical or in other shapes;
[0048] Chemically etching the surface of the intermediate shell of the substrate using a 5M NaOH solution at 23° C. for 50 min to obtain a substrate after surface etching;
[0049] Then, magnetron sputtering is used to deposit the shell on the surface of the substrate after surface etching. The vacuum degree before magnetron sputtering is 3×10 - 4 Pa, the argon flow rate was 38 sccm, the pressure of the vacuum chamber was maintained at 0.6 Pa, the magnetron sputtering temperature was 25 °C, and the magnetron sputtering power was 200 W to obtain phase change microcapsules;
[0050] The water-soluble polymer is melamine urea-formaldehyde resin, and the shell is composed of water-based polyurethane and CX-880 cross-linking agent mixed in a mass ratio of 1:0.25.
[0051] Example 2: A method for preparing a constant temperature microcapsule PCM cool fabric, such as Figure 1 As shown, the following steps are included:
[0052] S1. Weaving:
[0053] Nylon FDY is used for weft knitting with a weaving density of 38 needles / inch to obtain a woven fabric;
[0054] S2, Pre-order type:
[0055] The woven fabric is placed in a setting machine, and is pre-set for 2 minutes at 195° C. and 20 m / min, and during the pre-setting process, 250 g / L of nylon anti-yellowing powder is added to a water tank of the setting machine, and the water volume of the water tank is 80 L, to obtain a pre-set fabric; the nylon anti-yellowing powder is Revonox 608 anti-yellowing powder;
[0056] S3, dyeing and finishing:
[0057] The pre-shaped fabric is acid-dyed and finished at 98° C. with an acid dye fixing agent LTG-8053 for 55 minutes to obtain a dyed and finished fabric, and 4 g / L of a nylon anti-yellowing agent is added to the dyed and finished fabric after acid dyeing and finishing, and the fabric is heat-treated at a temperature of 65° C. for 20 minutes to obtain an anti-yellowing fabric; the nylon anti-yellowing agent is LD-RPY anti-yellowing agent;
[0058] S4, drying:
[0059] The anti-yellowing fabric is dried at a temperature of 160° C., a speed of 28 m / min, and a time of 1.5 min to obtain a dried fabric;
[0060] S5, rotary screen PCM printing:
[0061] The dried fabric is subjected to rotary screen PCM printing by means of electromagnetic magnetic rod pressure, wherein the rotary screen mesh of the rotary screen PCM printing is 105 meshes, the magnetic rod is an N35 magnet, the model of the magnetic rod is No. 12, and the rotary screen printing speed is 30 m / min to obtain a printed fabric;
[0062] The dye liquor used for the rotary screen PCM printing comprises, by mass percentage, 45% of phase change microcapsules, 35% of CX-880 crosslinking agent, 0.01% of LD-4126 softener, 2.5% of PTF thickener, 0.2% of XR-500 curing agent, 0.2% of SRN-618 hydrophilic agent and the balance of water;
[0063] S6, Thermal Stability Baking:
[0064] The printed fabric is baked at 100° C. for 2.5 minutes to obtain a baked fabric; the thermal stability baking process is to heat the material under certain temperature and time conditions, which can improve the thermal stability of the printed fabric;
[0065] S7, re-shaping:
[0066] The baked fabric was placed in a setting machine and set again at 150° C. and 18 m / min for 1 min to obtain a PCM cool fabric.
[0067] Example 3: This example is different from Example 1 in that the nylon fabric is provided with a print that occupies 40% of the nylon fabric area, and the average distribution density of the phase change microcapsules is 15 g / m 2 .
[0068] Example 4: This example is different from Example 1 in that the nylon fabric is provided with a print that occupies 70% of the nylon fabric area, and the average distribution density of the phase change microcapsules is 50 g / m 2 .
[0069] Example 5: This example is different from Example 1 in that the phase change microcapsule includes an outer shell, an intermediate shell and a core material from the outside to the inside, wherein the thickness of the outer shell is 5 μm, the thickness of the intermediate shell is 40 μm, and the particle size of the core material is 70 to 80 μm.
[0070] Example 6: This example is different from Example 1 in that the phase change microcapsule includes an outer shell, an intermediate shell and a core material from the outside to the inside, wherein the thickness of the outer shell is 10 μm, the thickness of the intermediate shell is 30 μm, and the particle size of the core material is 90 to 100 μm.
[0071] Example 7: This example is different from Example 1 in that paraffin, Tween 80 and caprylic / decanoic acid glyceride are heated to 50°C in a mass ratio of 1:0.1:40 and mixed evenly to obtain a dispersed phase with a solidification temperature of 4°C.
[0072] Example 8: This example is different from Example 1 in that paraffin, Tween 80 and caprylic / decanoic acid glyceride are heated to 60°C in a mass ratio of 1:0.2:40 and mixed evenly to obtain a dispersed phase with a solidification temperature of 8°C.
[0073] Example 9: This example is different from Example 1 in that the intermediate shell surface of the substrate is chemically etched using a 4M NaOH solution at 20° C. for 40 min.
[0074] Example 10: This example is different from Example 1 in that the intermediate shell surface of the substrate is chemically etched using a 6M NaOH solution at 25° C. for 60 min.
[0075] Example 11: This example is different from Example 1 in that the vacuum degree before magnetron sputtering is 1.5×10 -4 Pa, the argon flow rate is 35sccm, the gas pressure in the vacuum chamber is maintained at 0.4Pa, and the magnetron sputtering power is 180W.
[0076] Example 12: This example is different from Example 1 in that the vacuum degree before magnetron sputtering is 4.5×10 -4Pa, the argon flow rate is 40sccm, the gas pressure in the vacuum chamber is maintained at 0.8Pa, and the magnetron sputtering power is 220W.
[0077] Example 13: This example is different from Example 1 in that the water-soluble polymer is polyacrylamide, and the shell is composed of a mixture of water-based polyurethane and CX-880 cross-linking agent in a mass ratio of 1:0.2.
[0078] Example 14: This example is different from Example 1 in that the water-soluble polymer is melamine urea-formaldehyde resin, and the shell is composed of a mixture of water-based polyurethane and CX-880 cross-linking agent in a mass ratio of 1:0.3.
[0079] Example 15: This example differs from Example 2 in that the weaving density is 36 needles / inch.
[0080] Example 16: This example differs from Example 2 in that the weaving density is 40 needles / inch.
[0081] Example 17: This example is different from Example 2 in that the pre-setting is performed at 190°C and 19 m / min for 1.5 min, and 245 g / L of nylon anti-yellowing powder is added to the water tank of the setting machine during the pre-setting process.
[0082] Example 18: This example differs from Example 2 in that the pre-setting is performed at 200°C and 21 m / min for 2.5 min, and 255 g / L of nylon anti-yellowing powder is added to the water tank of the setting machine during the pre-setting process.
[0083] Example 19: This example differs from Example 2 in that the pre-shaped fabric is subjected to acid dyeing and finishing with an acid leveling agent at 95°C for 50 minutes.
[0084] Example 20: This example is different from Example 2 in that the pre-shaped fabric is acid-dyed and finished at 100°C with an acid-releasing agent AS-35 for 60 minutes.
[0085] Example 21: This example is different from Example 2 in that 3 g / L of nylon anti-yellowing agent is added to the dyed and finished fabric after acid dyeing and the fabric is heat-treated at 50°C for 18 minutes.
[0086] Example 22: This example differs from Example 2 in that 5 g / L of nylon anti-yellowing agent is added to the dyed and finished fabric after acid dyeing and the fabric is heat-treated at 80° C. for 22 minutes.
[0087] Example 23: This example differs from Example 2 in that the drying temperature is 155°C, the speed is 27 m / min, and the time is 1 min.
[0088] Example 24: This example differs from Example 2 in that the drying temperature is 165°C, the speed is 29 m / min, and the time is 2 min.
[0089] Example 25: This example differs from Example 2 in that the dye solution used for the rotary screen PCM printing comprises, by mass percentage, 44% phase change microcapsules, 36% CX-880 crosslinker, 0.05% LD-4126 softener, 2% PTF thickener, 0.1% XR-500 curing agent, 0.1% SRN-618 hydrophilic agent and the remainder water.
[0090] Example 26: This example differs from Example 2 in that the dye solution used for the rotary screen PCM printing comprises, by mass percentage, 46% of phase change microcapsules, 34% of CX-880 crosslinking agent, 0.15% of LD-4126 softener, 3% of PTF thickener, 0.3% of XR-500 curing agent, 0.3% of SRN-618 hydrophilic agent and the remainder of water.
[0091] Example 27: This example differs from Example 2 in that the printed fabric is baked at 95°C for 2 minutes to obtain a baked fabric.
[0092] Example 28: This example differs from Example 2 in that the printed fabric is baked at 105°C for 3 minutes to obtain a baked fabric.
[0093] Example 29: This example is different from Example 2 in that the molding is performed again at 145°C and 15 m / min for 1.5 min.
[0094] Example 30: This example is different from Example 2 in that the molding is performed again at 155°C and 20 m / min for 2.5 min.
[0095] Embodiment 31: This embodiment is different from Embodiment 2 in that after obtaining the baked fabric in step S6, it is subjected to a strengthening treatment, and the strengthening treatment method is as follows:
[0096] like Figure 2 As shown in the figure, the printed side of the baking fabric is used as the base, and the base is divided into several 0.004m 2 square area, 0.004m 2 The anti-dyeing baffles are spaced and distributed in each square area one by one, and the square areas corresponding to the printing area are all distributed with the anti-dyeing baffles,
[0097] Phase change microcapsules were sprayed on the blank part of the baking fabric, the distance between the nozzle and the baking fabric was 50 cm, the spraying pressure was 0.4 MPa, and the spraying amount was 1.6 times the average distribution density of the phase change microcapsules added in the printing;
[0098] After the spraying is completed, the anti-dyeing baffle is removed, and the baked fabric is baked at 100°C for 2.5 minutes to complete the strengthening treatment.
[0099] Example 32: This example differs from Example 31 in that the distance between the nozzle and the baking fabric is 40 cm, the spraying pressure is 0.2 MPa, and the spraying amount is 1.5 times the average distribution density of the phase change microcapsules added in the printing.
[0100] Example 33: This example differs from Example 31 in that the distance between the nozzle and the baking fabric is 60 cm, the spraying pressure is 0.5 MPa, and the spraying amount is 1.8 times the average distribution density of the phase change microcapsules added in the printing.
[0101] Example 34: This example differs from Example 31 in that the anti-staining baffle is removed and the baked fabric is baked at 95°C for 2 minutes.
[0102] Example 35: This example differs from Example 31 in that the anti-staining baffle is removed and the baked fabric is baked at 105°C for 3 minutes.
[0103] Example 36: This example is different from Example 31 in that the base is divided into several 0.003 m 2 square area, 0.003m 2 The anti-dyeing baffles are spaced apart and distributed in each square area one by one.
[0104] Example 37: This example is different from Example 31 in that the base is divided into several 0.005 m 2 square area, 0.005m 2 The anti-dyeing baffles are spaced apart and distributed in each square area one by one.
[0105] Experimental Example: The description of this experimental example is based on the scheme described in Example 2, and is intended to illustrate the practical application effect of the present invention.
[0106] Experimental design: In order to illustrate the cooling effect of the cooling fabric prepared by the present invention, the cooling fabric prepared in each embodiment was tested five times according to the national standard GB / T 35263-2017 "Testing and evaluation of instantaneous cooling performance of textiles", and the average value was taken as the cooling value of the cooling fabric / J / (cm 2 ·s), the higher the coldness value, the stronger the cooling effect of the cooling fabric;
[0107] Then, the friction test was carried out 50 times to detect the cool feeling value of the cool feeling fabric after the friction test. The loss rate of the cool feeling fabric was calculated by (the cool feeling value of the initial test - the cool feeling value after the friction test) / the cool feeling value of the initial test. The smaller the loss rate, the stronger the durability of the cool feeling fabric.
[0108] 1. Explore the preparation method of phase change microcapsules and the influence of their content in printing on the cooling value and loss rate of cool fabrics.
[0109] Table 1 Effect of Examples 1, 3 to 13 and Comparative Example 1 on the Cold Sensation Value and Loss Rate of Cool Feeling Fabrics
[0110]
[0111] The difference between the comparative example 1 and the example 1 is that the surface of the intermediate shell is not chemically etched;
[0112] From the results in Table 1, it can be seen that the control example 1 lacks chemical etching, and the cold feeling value of the cool feeling fabrics of Examples 1, 3 to 14 is significantly reduced, and the loss rate is correspondingly increased, so chemical etching has a certain effect on the phase change microcapsules;
[0113] By comparing Examples 1 and 3 to 14, it can be seen that too small or too large an amount of phase change microcapsules added, too small or too large a size of the phase change microcapsules, too small or too large a preparation parameter of the dispersed phase, too small or too large a parameter of chemical etching, too small or too large an adoption number of vacuum sputtering deposition, and too small or too large a proportion of waterborne polyurethane in the outer shell will all reduce the cold feeling value of the cool fabric and increase the loss rate accordingly. Among them, improving some parameters can enhance the cold feeling value, but the loss rate does not reach the level of Example 1. Therefore, in comprehensive comparison, the parameter effect of Example 1 is relatively better.
[0114] 2. Explore the influence of the preparation method of cool fabrics on the cooling value and loss rate of cool fabrics.
[0115] Table 2 Effect of Examples 2, 15-30 and Comparative Example 2 on the Cold Sensation Value and Loss Rate of Cool Fabrics
[0116]
[0117]
[0118] The difference between Control Example 2 and Example 2 is that the dye liquor for printing does not include CX-880 crosslinking agent;
[0119] From the results in Table 2, it can be seen that the control example 2 lacks the CX-880 crosslinking agent required for the printing dye solution. Compared with the examples 2 and 15 to 30, the cold feeling values of the cool feeling fabrics are significantly reduced, and the loss rate is correspondingly increased. Therefore, the CX-880 crosslinking agent is a key component for improving the performance of the cool feeling fabrics.
[0120] By comparing Examples 2 and 15 to 30, it can be seen that weaving density that is too small or too large, pre-setting parameters that are too small or too large, acid dyeing and finishing parameters that are too small or too large, nylon anti-yellowing agent addition parameters that are too small or too large, drying parameters that are too small or too large, the proportion of phase change microcapsules in the printing dye solution that is too small or too large, baking parameters that are too small or too large, and re-setting parameters that are too small or too large will all reduce the cold feeling value of the cool fabric and increase the loss rate accordingly. Among them, the increase of some parameters can enhance the cold feeling value, but the loss rate does not reach the level of Example 1. Therefore, in comprehensive comparison, the parameter effect of Example 2 is relatively better.
[0121] 3. Explore the effect of strengthening treatment of cool fabrics on the cooling value and loss rate of cool fabrics.
[0122] Table 3 Effect of Examples 31 to 35 on the cold feeling value and loss rate of cool fabrics
[0123]
[0124] The difference between Control Example 3 and Example 31 is that the spraying amount is twice that of the phase change microcapsules added in the printing;
[0125] From the results in Table 3, it can be seen that the strengthening treatment significantly improves the cold feeling value of the cool feeling fabric and reduces the loss rate accordingly compared with Examples 1 to 30. Therefore, the strengthening treatment plays a certain role in improving the performance of the cool feeling fabric. Compared with Examples 31 to 35, the spraying amount of the phase change microcapsules in Control Example 3 is larger, but the increase in the cold feeling value is smaller than that in Example 31, and the loss rate is the same as that in Example 31. Therefore, from the perspective of economy, Control Example 3 is not good and is not suitable for mass production.
[0126] By comparing Examples 31 to 37, it can be seen that too small injection parameters of the phase change microcapsules and too small or too large parameters of the secondary baking will reduce the effect of improving the cooling value of the cool fabric and reduce the degree of reduction in the loss rate. The square area in Example 36 is smaller and denser, so the distribution density of the phase change microcapsules is greater, and the cooling effect is higher than that in Example 31. The distribution density of the phase change microcapsules in Example 37 becomes smaller, and the cooling effect decreases accordingly compared with Example 31. Therefore, as the distribution density of the phase change microcapsules increases, the overall cooling effect gradually increases, but the increase is small. Therefore, from an economic point of view, the parameter effect of Example 31 is relatively better.
Claims
1. A constant temperature microcapsule PCM cool fabric, characterized in that: The invention comprises 100% nylon fabric by mass percentage, wherein the nylon fabric is provided with a printing which accounts for 40 to 70% of the area of the nylon fabric, and the printing is added with phase change microcapsules, and the average distribution density of the phase change microcapsules is 15 to 50 g / m 2 .
2. A constant temperature microcapsule PCM cool fabric as claimed in claim 1, characterized in that: The phase-change microcapsule comprises an outer shell, an intermediate shell and a core material from the outside to the inside, wherein the outer shell has a thickness of 5 to 10 μm, the intermediate shell has a thickness of 30 to 40 μm, and the core material has a particle size of 70 to 100 μm.
3. A constant temperature microcapsule PCM cool fabric as claimed in claim 2, characterized in that: The preparation method of the phase change microcapsule is as follows: Paraffin, Tween 80 and caprylic acid glyceride are heated to 50-60° C. in a mass ratio of 1:0.1-0.2:40 and mixed evenly to obtain a dispersed phase, and a water-soluble polymer is selected as a coagulation bath; the dispersed phase is formed into a core material in the form of micro-droplets with a particle size of 70-100 μm by a microfluidic device and the core material is dripped into the coagulation bath, so that the micro-droplet core material is coagulated at 4-8° C. and wrapped with an intermediate shell of a water-soluble polymer with a thickness of 30-40 μm to obtain a substrate; Chemically etching the surface of the intermediate shell of the substrate using a 4-6M NaOH solution at 20-25° C. for 40-60 minutes to obtain a substrate after surface etching; Then, magnetron sputtering is used to deposit the shell on the surface of the substrate after surface etching. The vacuum degree before magnetron sputtering is 1.5-4.5×10 -4 Pa, the argon flow rate is 35-40 sccm, the gas pressure in the vacuum chamber is maintained at 0.4-0.8 Pa, the magnetron sputtering temperature is room temperature, the magnetron sputtering power is 180-220 W, and phase change microcapsules are obtained.
4. A constant temperature microcapsule PCM cool fabric as claimed in claim 3, characterized in that: The water-soluble polymer is one of melamine urea-formaldehyde resin and polyacrylamide, and the shell is composed of a mixture of water-based polyurethane and CX-880 cross-linking agent in a mass ratio of 1:0.2-0.
3.
5. The method for preparing a constant temperature microcapsule PCM cool fabric according to any one of claims 1 to 4, characterized in that: The following steps are involved: S1. Weaving: Nylon FDY is used for weft knitting with a weaving density of 36 to 40 needles per inch to obtain a woven fabric; S2, Pre-order type: The woven fabric is placed in a setting machine, and pre-set at 190-200° C. and 19-21 m / min for 1.5-2.5 min, and 245-255 g / L of nylon anti-yellowing powder is added to a water tank of the setting machine during the pre-setting process, and the water volume of the water tank is 80 L, to obtain a pre-set fabric; S3, dyeing and finishing: The pre-shaped fabric is subjected to acid dyeing and finishing at 95-100° C. for 50-60 minutes to obtain a dyed and finished fabric, and 3-5 g / L of a nylon anti-yellowing agent is added to the dyed and finished fabric after acid dyeing and finishing, and the fabric is subjected to heat preservation treatment at a temperature of 50-80° C. for 18-22 minutes to obtain an anti-yellowing fabric; S4, drying: The anti-yellowing fabric is dried at a temperature of 155 to 165° C., a speed of 27 to 29 m / min, and a time of 1 to 2 min to obtain a dried fabric; S5, rotary screen PCM printing: The dried fabric is subjected to rotary screen PCM printing by means of electromagnetic magnetic rod pressure, wherein the rotary screen mesh of the rotary screen PCM printing is 105 mesh, the magnetic rod is an N35 magnet, the magnetic rod model is No. 12, and the rotary screen printing speed is 29-31 m / min to obtain a printed fabric; The dye liquor used for the rotary screen PCM printing comprises, by mass percentage, 44-46% of phase change microcapsules, 34-36% of CX-880 crosslinking agent, 0.05-0.15% of LD-4126 softener, 2-3% of PTF thickener, 0.1-0.3% of XR-500 curing agent, 0.1-0.3% of SRN-618 hydrophilic agent and the balance of water; S6, Thermal Stability Baking: Baking the printed fabric at 95-105° C. for 2-3 minutes to obtain a baked fabric; S7, re-shaping: The baked fabric is placed in a setting machine and set again at 145-155° C. and 15-20 m / min for 1.5-2.5 min to obtain a PCM cool fabric.
6. The method for preparing a constant temperature microcapsule PCM cool fabric according to claim 1, characterized in that: After obtaining the baking fabric in step S6, the baking fabric is strengthened by: The printed side of the baking fabric is used as the base, and the base is divided into several 0.003-0.005m 2 The square area of 0.003~0.005m 2 The anti-dyeing baffles are spaced and distributed in each square area one by one, and the square areas corresponding to the printing area are all distributed with the anti-dyeing baffles, After the distribution is completed, phase change microcapsules are sprayed on the blank part of the baking fabric. The distance between the nozzle and the baking fabric is 40-60 cm, the spraying pressure is 0.2-0.5 MPa, and the spraying amount is 1.5-1.8 times the average distribution density of the phase change microcapsules added in the printing. After the spraying is completed, the anti-dyeing baffle is removed, and the baked fabric is baked at 95-105°C for 2-3 minutes to complete the strengthening treatment.
7. The method for preparing a constant temperature microcapsule PCM cool fabric according to claim 1, characterized in that: In step S2, the nylon anti-yellowing powder is Revonox 608 anti-yellowing powder; in step S3, the nylon anti-yellowing agent is LD-RPY anti-yellowing agent.