Corrosion fatigue simulation system for marine environment under cathode protection

By combining environmental simulation units and cathode protection units in the corrosion fatigue simulation system, it simulates the environment of multiple marine corrosion areas and provides cathode protection, and solves the problem of corrosion fatigue under complex marine environments and cathode protection conditions in the existing technology, and realizes the More accurate corrosion fatigue test.

CN119044042APending Publication Date: 2024-11-29TIANJIN UNIV
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411166081.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing corrosion fatigue testing devices cannot simulate the complex environment under a variety of marine corrosion areas, especially under cathodic protection conditions, and it is difficult to explain the corrosion fatigue mechanism under actual service conditions.

Method used

A corrosion fatigue simulation system including corrosion unit, environmental simulation unit and cathode protection unit is designed to simulate the atmosphere, splash area, and tidal difference area through salt spray generation components, tidal difference components, splashing components, heating components and ventilation components. and the corrosion environment in the entire immersion area, and cathodic protection is provided according to service conditions. The pH and Cl ion content of the corrosion liquid are monitored and adjusted by sensors to ensure the accuracy of the test environment.

Benefits of technology

Accurate simulation of environments in various marine corrosion areas is achieved, simulation results are provided closer to actual service conditions, and the corrosion fatigue action mechanism under cathode protection is explained, which improves the accuracy and reliability of the test.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119044042A_ABST
    Figure CN119044042A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of fatigue tests, and particularly discloses a corrosion fatigue simulation system for a marine environment under cathode protection, the corrosion fatigue simulation system comprises a corrosion unit, an environment simulation unit, a cathode protection unit and a fatigue testing machine, the corrosion unit is used for penetrating through a to-be-tested sample and providing different corrosion environments for the to-be-tested sample; the environment simulation unit comprises a salt mist generation assembly, a liquid containing box, a tidal range assembly, a splashing assembly, a heating assembly and a ventilation assembly which are used for controlling the salt mist deposition amount and the water level height of corrosive liquid in the corrosion unit, simulating spray splashing and controlling the temperature and humidity. The cathode protection unit is connected with the to-be-tested sample and is used for providing cathode protection for the to-be-tested sample; and the fatigue testing machine is connected with two ends of the to-be-tested sample through the sample chuck. According to the invention, the corrosion environment of the atmosphere zone, the splash zone, the tidal range zone and the total immersion zone can be simulated, and the cathode protection environment is provided for the total immersion zone and the tidal range zone according to the service condition, so that the simulation result is closer to the actual service condition.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the field of fatigue testing, and more specifically, relates to a corrosion fatigue simulation system for a marine environment under cathodic protection. Background Art

[0002] With the imbalance of global oil supply and demand and the intensification of the energy crisis, the development of marine energy has become an increasingly important means to ensure national energy security. According to relevant reports and statistics, my country's marine crude oil production will exceed 62 million tons in 2023, becoming a key increase in my country's crude oil. As an important tool for energy exploration and oil and gas extraction, the sudden failure of offshore platforms during service will cause immeasurable losses to the marine environment and economic benefits. Among the reasons for the failure of offshore platform steel, the proportion of failure caused by corrosion in the marine environment is as high as 90%. At the same time, offshore platform steel has to withstand mechanical vibration loads in harsh corrosive environments. The accelerated coupling effect of the two greatly increases the probability of failure of offshore platform steel. This failure phenomenon is called corrosion fatigue. Corrosion fatigue failure in the marine environment often occurs in pitting pits on the steel surface, and the service life is much lower than the air fatigue life.

[0003] The marine environment can be divided into five areas according to the degree of corrosion: atmospheric zone, splash zone, tidal zone, full immersion zone and sea mud zone. The corrosion characteristics of the five areas are different. There is often a layer of electrolyte film on the surface of the structure in the atmospheric zone, and the oxygen content in the atmosphere is sufficient. Under the action of strong electrolyte and high oxygen content, the metal corrosion rate in this area will be accelerated; the splash zone is between the atmospheric zone and the tidal zone. It not only has the corrosion characteristics of the atmospheric zone, but also has the effect of splashing waves and more sufficient humidity. The corrosion rate of the splash zone is the fastest in the five areas; the tidal zone is affected by the rise and fall of tides and the atmospheric environment, and the corrosion environment is complex and changeable. However, due to the formation of a macroscopic battery with the atmospheric zone and the protection of the cathode, its corrosion rate is lower than that of the atmospheric zone; the metal in the full immersion zone faces seawater corrosion at all times, and microorganisms, seawater pH, salt content, etc. will affect it. Due to the low oxygen content in seawater, its corrosion phenomenon is relatively not serious; the characteristic of the sea mud zone is that it is seriously affected by anaerobic microorganisms and has a high sensitivity to stress corrosion. Since the characteristics of the five major corrosion areas are significantly different, conducting corrosion fatigue tests in different areas requires simulating specific corrosion environments. Existing corrosion fatigue testing machines can only simulate a single corrosion environment, and cannot simulate the multi-variable corrosion environments such as temperature, humidity, wave splashing, salt spray, etc. in various marine corrosion areas for standard specimens. It is difficult to explain the corrosion fatigue fracture process in various marine corrosion domains. There is an urgent need for a corrosion fatigue testing device that can simulate multi-region marine corrosion environments.

[0004] On the other hand, cathodic protection has always been one of the most effective means of corrosion protection for marine structures. Domestic cathodic protection technology is widely used in the field of corrosion control of pipelines, docks and ships in soil or seawater. However, marine pipelines and ships in service will inevitably suffer from mechanical vibration loads in specific marine corrosion areas, which are very likely to cause corrosion fatigue failure under the coupling of specific corrosive media and alternating loads. A large number of studies have shown that the corrosion under cathodic protection is significantly different from the traditional corrosion mechanism. The difference in corrosion mechanism will significantly change the corrosion fatigue effect under the same environment, but the current corrosion fatigue device for marine environment lacks consideration of the impact of cathodic protection on corrosion fatigue, and cannot explain the corrosion fatigue mechanism under the widely used cathodic protection technology in the actual environment. Summary of the invention

[0005] In view of the defects of the prior art, the present application provides a corrosion fatigue simulation system for a marine environment under cathodic protection, aiming to solve the problem that the existing corrosion fatigue test cannot approach the actual service conditions.

[0006] The present application provides a corrosion fatigue simulation system for a marine environment under cathodic protection, which specifically includes a corrosion unit, an environment simulation unit, a cathodic protection unit and a fatigue testing machine, wherein:

[0007] The corrosion unit is used to pass through the sample to be tested and provide different corrosion environments for the sample to be tested;

[0008] The environmental simulation unit includes a salt mist generating component, a liquid storage tank, a tidal difference component, a splash component, a heating component and a ventilation component. The salt mist generating component is connected to the corrosion unit and is used to control the amount of salt mist deposition in the corrosion unit; the liquid storage tank is used to hold the corrosive liquid; one end of the tidal difference component is connected to the liquid storage tank, and the other end thereof is connected to the corrosion unit, and is used to control the water level of the corrosive liquid in the corrosion unit; one end of the splash component is connected to the liquid storage tank, and the other end thereof is arranged in the corrosion unit, and is used to spray the corrosive liquid to the sample to be tested to simulate the splashing of waves; the heating component is arranged on the outside of the corrosion unit, and is used to control the temperature of the corrosion unit; the ventilation component is connected to the corrosion unit, and is used to control the humidity of the corrosion unit;

[0009] The cathodic protection unit is connected to the sample to be tested and is used to provide cathodic protection for the sample to be tested;

[0010] The fatigue testing machine is connected to two ends of the sample to be tested through a sample chuck, and is used to perform fatigue simulation on the sample to be tested under different corrosion environments and cathodic protection.

[0011] The above technical scheme conceived by the present application, compared with the prior art, can simulate the corrosion environment of the atmospheric zone, splash zone, tidal zone and full immersion zone, and provide a cathodic protection environment for the full immersion zone and tidal zone according to the service conditions, so that the simulation results are closer to the actual service conditions.

[0012] As further preferred, the cathodic protection unit includes a potentiostat, a calomel electrode and a platinum sheet electrode, the working electrode port of the potentiostat is connected to the sample to be tested, the reference electrode port of the potentiostat is connected to the calomel electrode, the auxiliary electrode port of the potentiostat is connected to the platinum sheet electrode, and the calomel electrode and the platinum sheet electrode extend into the corrosion unit.

[0013] As a further preferred embodiment, the corrosion unit includes an environmental box assembly and a sensor assembly, wherein the upper and lower openings of the environmental box assembly are used to pass the sample to be tested, and the environmental box assembly is connected to the environmental simulation unit to provide different corrosion environments for the sample to be tested therein; the sensor assembly extends into the interior of the environmental box assembly to detect the corrosion environment of the environmental box assembly; preferably, the sensor assembly includes a liquid level sensor, a temperature sensor, a humidity sensor, a pH sensor and a Cl ion sensor, wherein the liquid level sensor is used to detect the water level of the environmental box assembly, the temperature sensor is used to detect the temperature of the environmental box assembly, the humidity sensor is used to detect the humidity of the environmental box assembly, the pH sensor is used to detect the pH of the corrosive liquid, and the Cl ion sensor is used to detect the Cl ion content of the corrosive liquid, so as to determine whether the corrosive liquid needs to be replaced based on the pH and Cl ion content of the corrosive liquid.

[0014] As further preferred, the fatigue testing machine further comprises two insulating rings and two ceramic gaskets, the two insulating rings are respectively arranged on the inner wall of the sample chuck, and the two ceramic gaskets are arranged between the sample chuck and the sample to be tested.

[0015] As a further preference, the corrosion unit is connected to the fatigue testing machine via a metal bracket, thereby achieving fixation of the corrosion unit.

[0016] As a further preferred embodiment, the corrosion fatigue simulation system also includes a liquid receiving unit, which includes a liquid receiving tank and a waste liquid tank. The liquid receiving tank is arranged directly below the corrosion unit to receive the leaked liquid of the corrosion unit; the waste liquid tank is connected to the liquid receiving tank to store the waste liquid in the liquid receiving tank.

[0017] As further preferred, the liquid receiving tank is fixedly connected to the sample chuck.

[0018] As a further preferred embodiment, the tidal difference component includes a tidal difference water pump, an inlet pipe and an outlet pipe, one end of the tidal difference water pump is connected to the liquid storage tank, and the other end is connected to the inlet pipe, and the inlet pipe extends into the corrosion unit to introduce the corrosion liquid into the corrosion unit; the outlet pipe is connected to the bottom of the corrosion unit, and an outlet valve is provided on the outlet pipe, and the outlet valve is used to control the opening and closing of the outlet pipe, which is used to cooperate with the inlet pipe to control the water level of the corrosion unit.

[0019] As a further preference, the splash assembly includes a splash water pump, a left nozzle and a right nozzle, one end of the splash water pump is connected to the liquid storage tank, and the other end is connected to the left nozzle and the right nozzle to deliver the corrosive liquid into the left nozzle and the right nozzle; the left nozzle and the right nozzle are arranged on the left and right sides of the sample to be tested, and are used to spray the corrosive liquid on the sample to be tested to simulate wave splashing.

[0020] As further preferred, the corrosion fatigue simulation system also includes a control unit, which is connected to the corrosion unit and the environmental simulation unit and is used to control the environmental simulation unit according to the corrosion environment of the corrosion unit. The control unit is also connected to the cathodic protection unit and is used to control the cathodic protection unit.

[0021] In general, the above technical solutions conceived by this application have the following technical advantages compared with the prior art:

[0022] 1. The present application optimizes the composition of the environmental simulation unit. By setting a salt spray generating component, a tidal range component, a splash component, a heating component and a ventilation component, the corrosion environment of the corrosion unit can be accurately adjusted to simulate the corrosion environment of the atmospheric zone, the splash zone, the tidal range zone and the full immersion zone. In addition, by setting a cathodic protection unit, a cathodic protection environment can be provided for the full immersion zone and the tidal range zone according to the service conditions, so that the simulation results are closer to the actual service conditions.

[0023] 2. In particular, according to the requirements of cathodic protection, the present application sets a pH sensor and a Cl ion sensor in the sensing component of the corrosion unit, which can judge whether the corrosion solution needs to be replaced according to the pH and Cl ion content of the corrosion solution, thereby avoiding the change of the physical and chemical properties of the corrosion solution caused by long-term testing, thereby affecting the effect of cathodic protection, and further causing the test environment to deviate from the actual working conditions, affecting the accuracy of the simulation results;

[0024] 3. In addition, by adding insulating rings and ceramic gaskets to the fatigue testing machine, the present application can ensure the insulated connection between the test sample and the fatigue testing machine, avoid uneven current on the surface of the test sample, affect the cathodic protection effect, and cause data fluctuations, and can also avoid current leakage that causes damage to the constant potentiostat or fatigue testing machine. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 It is a schematic diagram of the structure of a corrosion fatigue simulation system for a marine environment under cathodic protection provided by an embodiment of the present application;

[0026] Figure 2 It is an enlarged schematic diagram of a corrosion unit in a corrosion fatigue simulation system for a marine environment under cathodic protection provided in an embodiment of the present application;

[0027] Figure 3 It is a schematic diagram of a left cover plate and a right cover plate in a corrosion fatigue simulation system for a marine environment under cathodic protection provided in an embodiment of the present application;

[0028] Figure 4 It is the SN curve of the test sample provided in the embodiment of the present application in seawater and under cathodic protection.

[0029] Throughout the drawings, the same reference numerals are used to denote the same elements or structures, wherein:

[0030] 101-salt spray generating assembly, 102-ventilation assembly, 103-heating assembly, 104-potentiostat, 105-tidal range water pump, 106-splash water pump, 107-liquid receiving tank, 108-liquid storage tank, 109-waste liquid tank, 110-electrically controlled water valve, 111-control unit, 112-fatigue testing machine, 113-metal bracket, 200-glass opening box, 201-air outlet, 202-air inlet, 203-salt spray outlet, 204-water outlet, 205-left nozzle, 206-right nozzle, 207-inlet Water pipe, 208-liquid level sensor, 209-temperature sensor, 210-humidity sensor, 211-test sample, 212-calomel electrode, 213-platinum electrode, 214-pH sensor, 215-Cl ion sensor, 301-right cover, 302-left cover, 303-right cover sealing ring, 304-left cover sealing ring, 305-upper sealing rubber plug, 305-lower sealing rubber plug, 307-back mother, 308-sleeve, 309-ceramic gasket, 310-insulating ring, 311-sample chuck. DETAILED DESCRIPTION

[0031] In order to make the purpose, technical solution and advantages of the present application more clearly understood, the present application is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.

[0032] like Figures 1 to 3 As shown, the present application provides a corrosion fatigue simulation system for a marine environment under cathodic protection, which specifically includes a corrosion unit, an environment simulation unit, a cathodic protection unit, a fatigue testing machine 112 and a control unit 111, wherein:

[0033] The corrosion unit is used to pass through the test sample 211 and provide the test sample 211 with a simulated corrosion environment of the marine atmosphere zone, the splash zone, the tidal range zone and the full immersion zone. The corrosion unit is connected to the fatigue testing machine 112 through a metal bracket 113, so as to fix the corrosion unit;

[0034] The environmental simulation unit is used to control the salt mist deposition amount, temperature, humidity, splashing speed, splashing frequency, dry-wet alternation time, air flow rate, etc. of the corrosion unit, and specifically includes a salt mist generating component 101, a liquid tank 108, a tidal difference component, a splashing component, a heating component 103 and a ventilation component 102. The salt mist generating component 101 is connected to the corrosion unit to control the salt mist deposition amount in the corrosion unit; the liquid tank 108 is used to hold the corrosive liquid; one end of the tidal difference component is connected to the liquid tank 108, and the other end thereof is connected to the corrosion unit to control the water level of the corrosive liquid in the corrosion unit; one end of the splashing component is connected to the liquid tank 108, and the other end thereof is arranged in the corrosion unit to spray the corrosive liquid to the sample to be tested 211 to simulate the splashing of waves; the heating component 103 is arranged on the outside of the corrosion unit to heat the corrosion unit to control the temperature of the corrosion unit; the ventilation component 102 is connected to the corrosion unit to control the humidity of the corrosion unit;

[0035] The cathodic protection unit is connected to the test sample 211 and is used to provide cathodic protection for the test sample 211. During the test, a cathodic protection environment can be provided for the full immersion area and the tidal range area according to actual service conditions;

[0036] The fatigue testing machine 112 is connected to both ends of the test sample 211 through the sample chuck 311, and is used to perform fatigue simulation on the test sample under different corrosion environments and cathodic protection.

[0037] The present application can simulate the corrosion environment of the atmospheric zone, splash zone, tidal zone and full immersion zone by arranging a salt spray generating component, a tidal difference component, a splash component, a heating component and a ventilation component in the environmental simulation unit, so that the test sample 211 is subjected to alternating loads under multiple corrosion variables and fatigue failure occurs. The corrosion environment provided by the present application controls parameters such as salt spray deposition amount, temperature, humidity, splashing speed, splashing frequency, cathodic protection potential, dry-wet alternation time, and air flow rate, so as to make the test environment close to the real marine corrosion environment. At the same time, considering that the corrosion under the cathodic protection state is significantly different from the traditional corrosion mechanism, the present application adds a cathodic protection unit to the corrosion fatigue simulation system, which can provide a cathodic protection environment for the full immersion zone and the tidal difference zone according to the service conditions, so that the simulation results are closer to the actual service conditions, and can better explain the corrosion fatigue mechanism under the cathodic protection technology that is widely used in the actual environment.

[0038] Furthermore, the cathodic protection unit includes a potentiostat 104, a calomel electrode 212 and a platinum electrode 213, the working electrode port of the potentiostat 104 is connected to the test sample 211, the reference electrode port of the potentiostat 104 is connected to the calomel electrode 212, the auxiliary electrode port of the potentiostat 104 is connected to the platinum electrode 213, and the calomel electrode 212 and the platinum electrode 213 extend into the corrosion unit.

[0039] Furthermore, the corrosion unit includes an environmental box assembly and a sensor assembly. The upper and lower openings of the environmental box assembly are used to pass the sample to be tested 211. At the same time, the environmental box assembly is connected to the environmental simulation unit to provide different corrosion environments for the sample to be tested 211 inside it; the sensor assembly extends into the interior of the environmental box assembly to detect the corrosion environment of the environmental box assembly, and includes a liquid level sensor 208, a temperature sensor 209, a humidity sensor 210, a pH sensor 214 and a Cl ion sensor 215. The liquid level sensor 208 is used to detect the water level of the corrosive liquid in the environmental box assembly, the temperature sensor 209 is used to detect the temperature of the environmental box assembly, the humidity sensor 210 is used to detect the humidity of the environmental box assembly, the pH sensor 214 is used to detect the pH of the corrosive liquid, and the Cl ion sensor 215 is used to detect the Cl ion content of the corrosive liquid, so as to determine whether the corrosive liquid needs to be replaced according to the pH and Cl ion content of the corrosive liquid. The corrosive liquid needs to be replaced when the pH is ≥9 or the Cl ion concentration is ≥4%, so as to avoid changes in the physical and chemical properties of the corrosive liquid caused by long-term testing, which affects the effect of cathodic protection, and further causes the test environment to deviate from the actual working conditions, affecting the accuracy of the simulation results.

[0040] Furthermore, the corrosion fatigue simulation system further includes a liquid receiving unit, which includes a liquid receiving tank 107 and a waste liquid tank 109. The liquid receiving tank 107 is arranged directly below the corrosion unit and is used to receive the leaked liquid of the corrosion unit to prevent the corrosion unit from accidentally leaking liquid and causing corrosion of the fatigue testing machine 112. The waste liquid tank 109 is connected to the liquid receiving tank 107 and is used to store the waste liquid in the liquid receiving tank 107. Preferably, the liquid receiving tank 107 is connected to the sample chuck 311 by bolts, so as to fix the liquid receiving tank 107.

[0041] Furthermore, the tidal difference component includes a tidal difference water pump 105, an inlet pipe 207 and an outlet pipe 204. One end of the tidal difference water pump 105 is connected to the liquid storage tank 108, and the other end of the tidal difference water pump 105 is connected to the inlet pipe 207. At the same time, the inlet pipe 207 extends into the corrosion unit to introduce corrosion liquid into the corrosion unit; the outlet pipe 204 is connected to the bottom of the corrosion unit, and an outlet valve 110 is provided on the outlet pipe 204. The outlet valve 110 controls the opening and closing of the outlet pipe 204, which is used to cooperate with the inlet pipe 207 to control the water level of the corrosion unit.

[0042] Furthermore, the splash assembly includes a splash water pump 106, a left nozzle 205 and a right nozzle 206, one end of the splash water pump 106 is connected to the liquid storage tank 108, and the other end of the splash water pump 106 is connected to the left nozzle 205 and the right nozzle 206 to deliver the corrosive liquid into the left nozzle 205 and the right nozzle 206; the left nozzle 205 and the right nozzle 206 are arranged on the left and right sides of the sample to be tested 211, and are used to spray the corrosive liquid on the sample to be tested 211 to simulate the splashing of waves.

[0043] Furthermore, the fatigue testing machine 112 also includes two insulating rings 310 and two ceramic gaskets 309. The two insulating rings 310 are respectively arranged on the inner wall of the sample clamp 311, and the two ceramic gaskets 309 are arranged between the sample clamp 311 and the test sample 211, so as to ensure that the test sample 211 is insulated from the fatigue testing machine 112, avoid uneven current on the surface of the test sample, affect the cathodic protection effect, cause data fluctuations, and also avoid current leakage causing damage to the constant potentiostat or fatigue testing machine.

[0044] Further, the environmental chamber assembly includes a glass opening chamber 200, a left cover plate 302, a right cover plate 301, an upper sealing rubber plug 305, a lower sealing rubber plug 306, a sleeve 308 and a back nut 307. The glass opening chamber 200 cooperates with the left cover plate 302 and the right cover plate 301 to form the main body of the environmental chamber. In order to improve the sealing performance, a left cover sealing ring 304 is provided between the left cover plate 302 and the glass opening chamber 200, and a right cover sealing ring 303 is provided between the right cover plate 301 and the glass opening chamber 200. The glass opening box 200 is made of heat-resistant glass such as high borosilicate. The bottom opening of the glass opening box 200 is used to connect with the water outlet pipe 204. The central openings of the left cover plate 302 and the right cover plate 301 and the bottom central opening of the glass opening box 200 are respectively used to pass the sample to be tested 211. The left cover plate 302 is provided with a plurality of through holes for passing the water inlet pipe 207, the platinum electrode 213, and the calomel electrode 212. At the same time, the left cover plate 302 is also provided with a salt spray port 203 and an air inlet 202. The salt spray port 203 is connected to the salt spray generating assembly 101, and the air inlet 202 is connected to the ventilation assembly 102; a plurality of through holes are opened on the right cover plate 301 for passing the humidity sensor 210, the temperature sensor 209 and the liquid level sensor 208, and an air outlet 201 is also provided on the right cover plate 301, and the air outlet 201 is connected to the ventilation assembly 102; the upper sealing rubber plug 305 is used to seal the openings of the left cover plate 302 and the right cover plate 301, and the lower sealing rubber plug 306 is used to seal the glass opening box The opening of 200 is sealed, and the sealing of the environmental box assembly is ensured by the cooperation of the upper sealing rubber plug 305 and the lower sealing rubber plug 306. During use, the corrosion fatigue test of the test sample 211 with different rod sizes can be carried out by replacing the upper sealing rubber plug 305 and the lower sealing rubber plug 306; the sleeve 308 is arranged below the lower sealing rubber plug 306, and the inner part of the back nut abuts the sleeve 308 and is connected to the glass opening box 200 through threads to realize the fixation of the lower bearing rubber plug 306.

[0045] Furthermore, the corrosion fatigue simulation system also includes a control unit 111, which is connected to the corrosion unit and the environmental simulation unit for controlling the environmental simulation unit according to the corrosion environment of the corrosion unit. The control unit 111 is also connected to the cathodic protection unit for controlling the cathodic protection unit. Among them: the control unit 111 is connected to the heating component 103, and can control the heating temperature under different simulation conditions; the control unit 111 is connected to the ventilation component 102, and can ensure that the airflow variables are controllable when simulating the atmospheric zone, splash zone and tidal zone; the control unit is connected to the liquid level sensor 208, the temperature sensor 209, and the humidity sensor 210, and can monitor and control the humidity, temperature and water level of the corrosion unit in real time; the control unit 111 is connected to the constant potentiostat 104, and can adjust the cathodic protection under specific simulation conditions; the control unit 111 is connected to the tidal pump 105 and the outlet valve 110, and can control the dry-wet alternation time of the tidal environment and the drainage process under other conditions; the control unit 111 is connected to the splash pump 106, and can control the wave impact speed and impact frequency in the splash environment; the control unit 111 is connected to the ventilation component 102, and can adjust the humidity of the environmental simulation unit.

[0046] The working process of the corrosion fatigue simulation system for marine environment under cathodic protection provided by the present application is further described below.

[0047] When conducting corrosion fatigue tests in a simulated marine atmosphere environment with high temperature, high humidity, large air flow and ion deposition, first, the test sample 211 and the lower sealing rubber plug 306 are tightly assembled and loaded into the glass opening box 200, and the sleeve 308 and the back nut 307 are assembled. The metal bracket 113 is adjusted to place the glass opening box 200 in a suitable position of the fatigue testing machine 112, the test sample 211 is clamped in the sample chuck 311, and the right cover plate 301 and the left cover plate 302 are assembled. The fatigue testing machine 112 is adjusted to make the stress ratio and stress level reach specific values. The salt spray generating component 101 and the electric control water valve 110 are set to be in a normally open state through the control unit 111. The temperature sensor 209 and the humidity sensor 210 automatically collect data. Specific temperature and humidity parameters are set on the control unit 111. When the temperature and humidity values ​​do not reach the values, the control unit 111 turns on the heating component 103 and the ventilation component 102 to control the temperature and humidity. When the temperature and humidity values ​​reach the values, the control unit 111 turns off the heating component 103 and the ventilation component 102. The test ends when the test sample 211 breaks, and the control unit 111 turns off the above components.

[0048] A corrosion fatigue test is conducted in a simulated environment of an ocean splash zone with high temperature and humidity, seawater splashing, and alternating dry and wet conditions. First, the test sample 211 is tightly assembled with the lower sealing rubber plug 306 and loaded into the glass opening box 200, and the sleeve 308 and the back nut 307 are assembled. The metal bracket 113 is adjusted to place the glass opening box 200 in a suitable position of the testing machine, the sample is clamped in the sample chuck 311, and the right cover plate 301 and the left cover plate 302 are assembled. The fatigue testing machine 112 is adjusted to make the stress ratio and stress level reach specific values. The electric control water valve 110 is set to be in a normally open state through the control unit 111, and the opening frequency of the splash water pump 106 is adjusted to simulate the period and frequency of wave splashing. The splashing flow rate is adjusted by adjusting the speed knob of the splash water pump 106. The temperature sensor 209 and the humidity sensor 210 automatically collect data. Specific temperature and humidity parameters are set on the control unit 111. When the temperature and humidity values ​​do not reach this value, the control unit 111 turns on the heating component 103 and the ventilation component 102 to control temperature and humidity. When the temperature and humidity values ​​reach this value, the control unit 111 turns off the heating component 103 and the ventilation component 102. The test ends when the sample breaks, and the control unit 111 turns off the above components.

[0049] The corrosion fatigue test of the simulated environment of the marine tidal range zone with alternating dry and wet conditions is carried out. First, the test sample 211 and the lower sealing rubber plug 306 are tightly assembled and loaded into the glass opening box 200, and the sleeve 308 and the back nut 307 are assembled. The metal bracket 113 is adjusted to place the glass opening box 200 in a suitable position of the fatigue testing machine 112. The test sample 211 is clamped in the sample chuck 311, and the right cover plate 301 and the left cover plate 302 are assembled. The fatigue testing machine 112 is adjusted to make the stress ratio and stress level reach specific values. The ventilation component 102 is always open to balance the air pressure, and the speed knob of the tidal range water pump 105 is opened and adjusted to adjust the seawater flow rate. The float of the liquid level sensor 208 changes with the rise and fall of the liquid level. When the high liquid level is reached, the liquid level sensor 208 sends a signal to the control unit 111, and the control unit 111 turns off the tidal range water pump 105. After a specific time, the control unit 111 opens the electric control water valve 110 and connects the liquid outlet of the glass opening box 200 with the liquid storage box 108, and the corrosive liquid flows back into the liquid storage box 108. When the liquid level reaches the low water level, the liquid level sensor 208 sends a signal to the control unit 111, and the control unit 111 closes the electric control water valve 110. The constant potential instrument 104 starts and stops according to the change of the water level. After setting the cathode potential, when the high liquid level is reached, the control unit 111 starts the constant potential instrument 104, and when the low liquid level is reached, the control unit 111 closes the constant potential instrument 104. During the whole process, the temperature sensor 209 automatically collects data, and a specific temperature parameter is set on the control unit 111. When the temperature value does not reach the value, the control unit 111 turns on the heating component 103 for temperature control. When the temperature value reaches the value, the control unit 111 turns off the heating component 103, and the test ends when the sample breaks, and the control unit 111 turns off the above components.

[0050] To conduct a corrosion fatigue test in a simulated marine immersion zone environment, first, the test sample 211 and the lower sealing rubber plug 306 are tightly assembled and loaded into the glass opening box 200, and the sleeve 308 and the back nut 307 are assembled. The metal bracket 113 is adjusted to place the glass opening box 200 in a suitable position in the fatigue testing machine 112, and the test sample 211 is clamped in the sample chuck 311, and the right cover plate 301 and the left cover plate 302 are assembled. The fatigue testing machine 112 is adjusted to make the stress ratio and stress level reach specific values. The ventilation assembly 102 is normally open to balance the air pressure, the tidal pump 105 is turned on, and the float of the liquid level sensor 208 changes with the rise and fall of the liquid level. When the high liquid level is reached, the liquid level sensor 208 sends a signal to the control unit 111, and the control unit 111 turns off the tidal pump 105. When the test needs to replace the corrosive liquid, the electric control water valve 110 is opened and the liquid outlet of the glass opening box 200 is connected to the waste liquid tank 109, and the corrosive liquid flows into the waste liquid tank 109. When the liquid level reaches the low water level, the liquid level sensor 208 sends a signal to the control unit 111, and the control unit 111 turns off the electric control water valve 110 and immediately turns on the tidal pump 105 to complete the process of replacing the corrosive liquid. The constant potential instrument 104 is in the normally open state. After setting the cathode potential, the test sample 211 is subjected to long-term cathodic protection. During the whole process, the temperature sensor 209 automatically collects data and sets specific temperature parameters on the control unit 111. When the temperature value does not reach the value, the control unit 111 turns on the heating component 103 for temperature control. When the temperature value reaches the value, the control unit 111 turns off the heating component 103. The test ends when the sample breaks, and the control unit 111 turns off the above components.

[0051] To conduct the corrosion fatigue test in the simulated environment of the marine full immersion zone, firstly, the test sample 211 made of EH36 welded joint and parallel section diameter of 6.5mm is tightly assembled with the lower sealing rubber plug 306 and loaded into the glass opening box 200, and the sleeve 308 and the back nut 307 are assembled. The metal bracket 113 is adjusted to place the glass opening box 200 in the appropriate position of the fatigue testing machine 112, and the test sample 211 is clamped in the sample chuck 311, and the right cover plate 301 and the left cover plate 302 are assembled. The fatigue testing machine 112 is adjusted to make the stress ratio 0.1, the stress level 450MPa, 430MPa, 410MPa, 400MPa, 390Mpa, the test frequency 1Hz, and the sine wave is adopted. The ventilation assembly 102 is normally open to balance the air pressure, the tidal pump 105 is turned on, and the float of the liquid level sensor 208 changes with the rise and fall of the liquid level. When the high liquid level is reached, the liquid level sensor 208 sends a signal to the control unit 111, and the control unit 111 turns off the tidal pump 105. When the pH is ≥9 or the Cl ion concentration is ≥4%, the pH sensor 214 and the Cl ion sensor 215 transmit electrical signals to the control unit 111, and the control unit 111 turns on the electric control valve 110, and the corrosive liquid flows into the waste liquid tank 109. When the liquid level reaches the low water level, the liquid level sensor 208 sends a signal to the control unit 111, and the control unit 111 turns off the electric control valve 110 and immediately turns on the tidal pump 105 to complete the process of replacing the corrosive liquid. The constant potential meter 104 is in a normally open state, and the constant potential meter 104 is used to provide a cathodic protection potential of -1050mV / SCE to the sample to be tested 211, and the sample to be tested 211 is subjected to long-term cathodic protection. During the whole process, the temperature sensor 209 automatically collects data and sets the temperature parameter to 28°C on the control unit 111. When the temperature value does not reach 28°C, the control unit 111 turns on the heating component 103 for temperature control. When the temperature value reaches 28°C, the control unit 111 turns off the heating component 103. When the test sample 211 breaks, the test ends and the control unit 111 turns off the above components. The full immersion zone simulation results obtained in this embodiment are as follows: Figure 4 The solid line is the final fitting result.

[0052] In another embodiment of the present application, the cathodic protection is not turned on in the full immersion area, and the simulation results are as follows: Figure 4 The dotted line is the final fitting result. Figure 4 It can be seen that the corrosion fatigue simulation system provided by the present application can better simulate the actual service conditions. At the same time, the test results also show that cathodic protection can significantly improve the corrosion resistance of materials.

[0053] It will be easily understood by those skilled in the art that the above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application shall be included in the scope of protection of the present application.

Claims

1. A corrosion fatigue simulation system for marine environment under cathodic protection, characterized in that: The corrosion fatigue simulation system comprises a corrosion unit, an environment simulation unit, a cathodic protection unit and a fatigue testing machine (112), wherein: The corrosion unit is used to pass through the sample to be tested (211) and provide different corrosion environments for the sample to be tested (211); The environmental simulation unit comprises a salt mist generating component (101), a liquid storage tank (108), a tidal difference component, a splash component, a heating component (103) and a ventilation component (102); the salt mist generating component (101) is connected to the corrosion unit and is used to control the amount of salt mist deposition in the corrosion unit; the liquid storage tank (108) is used to store the corrosive liquid; one end of the tidal difference component is connected to the liquid storage tank (108), and the other end thereof is connected to the corrosion unit and is used to control the water level of the corrosive liquid in the corrosion unit; one end of the splash component is connected to the liquid storage tank (108), and the other end thereof is arranged in the corrosion unit and is used to spray the corrosive liquid onto the sample to be tested (211) to simulate the splashing of waves; the heating component (103) is arranged outside the corrosion unit and is used to control the temperature of the corrosion unit; the ventilation component (102) is connected to the corrosion unit and is used to control the humidity of the corrosion unit; The cathodic protection unit is connected to the sample to be tested (211) and is used to provide cathodic protection for the sample to be tested (211); The fatigue testing machine (112) is connected to both ends of the sample to be tested (211) via a sample chuck (311) and is used to perform fatigue simulation on the sample to be tested under different corrosion environments and cathodic protection.

2. The corrosion fatigue simulation system according to claim 1, characterized in that: The cathodic protection unit comprises a constant potential instrument (104), a calomel electrode (212) and a platinum sheet electrode (213); the working electrode port of the constant potential instrument (104) is connected to the sample to be tested (211); the reference electrode port of the constant potential instrument (104) is connected to the calomel electrode (212); the auxiliary electrode port of the constant potential instrument (104) is connected to the platinum sheet electrode (213); and the calomel electrode (212) and the platinum sheet electrode (213) extend into the corrosion unit.

3. The corrosion fatigue simulation system according to claim 1, characterized in that: The corrosion unit comprises an environmental box component and a sensor component. The upper and lower openings of the environmental box component are used to pass through the sample to be tested (211). The environmental box component is connected to the environmental simulation unit to provide different corrosion environments for the sample to be tested (211) inside the environmental box component. The sensor component extends into the interior of the environmental box component to detect the corrosion environment of the environmental box component. Preferably, the sensor component comprises a liquid level sensor (208), a temperature sensor (209), a humidity sensor (210), a pH sensor (214) and a Cl ion sensor (215). The liquid level sensor (208) is used to detect the water level of the environmental box component. The temperature sensor (209) is used to detect the temperature of the environmental box component. The humidity sensor (210) is used to detect the humidity of the environmental box component. The pH sensor (214) is used to detect the pH of the corrosion liquid. The Cl ion sensor (215) is used to detect the Cl ion content of the corrosion liquid, so as to judge whether the corrosion liquid needs to be replaced according to the pH and Cl ion content of the corrosion liquid.

4. The corrosion fatigue simulation system according to claim 1, characterized in that: The fatigue testing machine (112) further comprises two insulating rings (310) and two ceramic gaskets (309), wherein the two insulating rings (310) are respectively arranged on the inner wall of the sample chuck (311), and the two ceramic gaskets (309) are arranged between the sample chuck (311) and the sample to be tested (211).

5. The corrosion fatigue simulation system according to claim 1, characterized in that: The corrosion unit is connected to the fatigue testing machine (112) via a metal bracket (113), thereby achieving fixation of the corrosion unit.

6. The corrosion fatigue simulation system according to claim 1, characterized in that: The corrosion fatigue simulation system also includes a liquid receiving unit, which includes a liquid receiving tank (107) and a waste liquid tank (109). The liquid receiving tank (107) is arranged directly below the corrosion unit and is used to receive liquid leakage from the corrosion unit; the waste liquid tank (109) is connected to the liquid receiving tank (107) and is used to store waste liquid in the liquid receiving tank (107).

7. The corrosion fatigue simulation system according to claim 6, characterized in that: The liquid receiving tank (107) is fixedly connected to the sample chuck (311).

8. The corrosion fatigue simulation system according to claim 1, characterized in that: The tidal difference component comprises a tidal difference water pump (105), an inlet pipe (207) and an outlet pipe (204); one end of the tidal difference water pump (105) is connected to a liquid storage tank (108), and the other end is connected to the inlet pipe (207); the inlet pipe (207) extends into the corrosion unit and is used to introduce corrosion liquid into the corrosion unit; the outlet pipe (204) is connected to the bottom of the corrosion unit, and an outlet valve (110) is provided on the outlet pipe (204); the outlet valve (110) is used to control the opening and closing of the outlet pipe (204) and is used to cooperate with the inlet pipe (207) to control the water level of the corrosion unit.

9. The corrosion fatigue simulation system according to claim 1, characterized in that: The splash assembly comprises a splash water pump (106), a left nozzle (205) and a right nozzle (206); one end of the splash water pump (106) is connected to a liquid storage tank (108), and the other end is connected to the left nozzle (205) and the right nozzle (206) so as to deliver the corrosive liquid to the left nozzle (205) and the right nozzle (206); the left nozzle (205) and the right nozzle (206) are arranged on the left and right sides of the sample to be tested (211) and are used to spray the corrosive liquid onto the sample to be tested (211) to simulate the spraying of waves.

10. The corrosion fatigue simulation system according to any one of claims 1 to 9, characterized in that: The corrosion fatigue simulation system also includes a control unit (111), which is connected to the corrosion unit and the environmental simulation unit and is used to control the environmental simulation unit according to the corrosion environment of the corrosion unit. The control unit (111) is also connected to the cathode protection unit and is used to control the cathode protection unit.

Citation Information

Patent Citations

  • Corrosion fatigue test system and method for large-scale model of ocean engineering structure

    CN112924369A

  • Accelerated corrosion simulation test device and method in marine environment

    CN117723479A

  • Large offshore corrosion experiment comprehensive platform

    CN215525463U