Silicon-based negative electrode material, negative electrode plate and battery

By using the core-shell structure of B-doped silicon core and conductive metal carbon shell in silicon-based anode material, the structural breakage problem caused by volume changes in silicon anode material in lithium-ion batteries is solved, and high stability and high rate performance are achieved Improvement.

CN119050292APending Publication Date: 2024-11-29EVE ENERGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411053436.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Large-scale application of silicon anode materials in lithium-ion batteries is caused by structural breakage and loss of electrical contact caused by volume changes during cycles, and existing improvement methods are often at the expense of specific capacity or increased costs.

Method used

Silicon-based anode material with core-shell structure, where the core is B-doped silicon and the outer shell is a conductive metal carbon layer. The conductivity and structural stability are improved through B-doping, and the interface connectivity and mechanical properties are enhanced through conductive metal carbon layer. , relieve volume expansion stress.

Benefits of technology

The structural stability and rate performance of silicon-based negative electrode materials are significantly improved, cycle stability and high-rate fast charging performance are optimized, while maintaining a high specific capacity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119050292A_ABST
    Figure CN119050292A_ABST
Patent Text Reader

Abstract

The invention provides a silicon-based negative electrode material, a negative electrode plate and a battery, the silicon-based negative electrode material comprises an inner core and a shell coating the inner core, the inner core comprises non-metal doped silicon, and the shell comprises a conductive metal carbon layer; in the non-metal doped silicon, the non-metal comprises B; in the conductive metal carbon layer, conductive metal carbon comprises at least one of Ti3C2 (OH) 2 and Ti3AlC2. According to the silicon-based negative electrode material, the volume expansion effect of a silicon material can be effectively relieved, and the structural stability of the silicon-based negative electrode material is effectively improved; and meanwhile, the silicon-based negative electrode material has excellent conductivity. Therefore, the battery prepared by using the silicon-based negative electrode material has relatively good high-rate rapid charging performance and cycle performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of lithium-ion batteries, and in particular relates to a silicon-based negative electrode material, a negative electrode sheet, and a battery. Background Art

[0002] Silicon has great potential as a negative electrode material in secondary batteries. It has the advantages of being green, non-toxic, harmless and abundant in the earth. Especially for lithium-ion batteries, the room temperature theoretical specific capacity of silicon negative electrodes is as high as 3579 mA·h / g, and the working potential is low. It is considered to be one of the ideal negative electrodes. However, the large-scale application of silicon negative electrodes in lithium-ion batteries still faces several key difficulties. Among them, the biggest challenge affecting the industrialization of silicon negative electrodes is the large volume change of silicon during the cycle. Compared with the volume change of only 12% of the graphite negative electrode, the volume change of the silicon negative electrode is as high as 300%, which means that during the charge and discharge cycle, the silicon negative electrode will experience huge expansion and contraction, resulting in its severe crushing and pulverization, causing the silicon particles to lose electrical contact with the current collector, affecting the battery performance.

[0003] In the past few decades, people have addressed the defects of silicon electrodes through methods such as nano-sizing, silicon-carbon composites, and alloying. Both methods effectively improve the volume expansion effect of silicon materials and enhance electrochemical performance, but these are achieved at a higher cost or at the expense of a portion of silicon's specific capacity.

[0004] In view of this, providing a new type of silicon-based negative electrode material to further optimize the structural stability, cycle performance, and rate performance of the silicon-based negative electrode is of great significance for promoting the further development of the lithium battery industry. Summary of the invention

[0005] In order to solve the problems and deficiencies in the prior art, the present invention provides a silicon-based negative electrode material, a negative electrode sheet, and a battery. The silicon-based negative electrode material can effectively alleviate the volume expansion effect of silicon materials and effectively improve the structural stability of the silicon-based negative electrode material; at the same time, the silicon-based negative electrode material has excellent conductivity. Therefore, the battery prepared using the silicon-based negative electrode material has good high-rate fast charging performance and cycle performance.

[0006] According to a first aspect of the present invention, there is provided a silicon-based negative electrode material, comprising a core and a shell covering the core, wherein the core comprises metal-doped silicon, and the shell comprises a conductive metal carbon layer; in the non-metal-doped silicon, the non-metal comprises B; in the conductive metal carbon layer, the conductive metal carbon comprises at least one of Ti3C2(OH)2 and Ti3AlC2.

[0007] The silicon-based negative electrode material provided by the present invention is a core-shell structure, wherein the core is B-doped silicon. The non-metallic element B is doped in the silicon lattice, which can increase the active sites and lithium storage performance of the silicon material, so that the doped silicon becomes p-type silicon, thereby significantly improving the conductivity of silicon, and then effectively improving the rate capability and electrochemical cycle stability of the silicon-based negative electrode material. Moreover, the non-metallic element B can also form a "buffer skeleton" in the core, thereby effectively alleviating the volume expansion stress, greatly improving the structural stability of the silicon-based negative electrode material, thereby improving the cycle stability and high-rate fast charging performance of the silicon-based negative electrode material. The use of conductive metal carbon as the outer shell of the silicon-based negative electrode material can further improve the structural stability of the silicon-carbon negative electrode and optimize the rate performance. This is because, firstly, the conductive metal carbon has good electrical conductivity and can enhance Li + It shuttles between the electrode material and the electrolyte interface, and has good rate performance. Secondly, conductive metal carbon can form metal-Si and C-Si with silicon. The dual effects of metal-Si and C-Si can improve the close connectivity between the interface of the non-metallic doped silicon core and the conductive metal carbon layer, which is beneficial to further improve the stability of the material and better inhibit the volume expansion of silicon. Thirdly, the conductive metal carbon itself has excellent mechanical properties, good thermodynamic properties and corrosion resistance, so it can reduce the side reactions on the surface of the silicon negative electrode and better protect the non-metallic doped silicon core, thereby further improving the structural stability of the silicon-based negative electrode material and optimizing the rate performance.

[0008] Preferably, the mass proportion of B in the silicon-based negative electrode material is 0.5-2.0%. If the proportion of non-metallic elements is too small, the conductivity of the silicon-based negative electrode material cannot be effectively improved. At the same time, the buffer skeleton formed in the non-metallic doped silicon core will have some effect on resisting the volume expansion stress of silicon. If the proportion of non-metallic elements is too small, the conductivity and structural stability of the silicon-based negative electrode material will be reduced. If the proportion of non-metallic elements is too high, the proportion of silicon will be relatively small, which will reduce the specific capacity of the silicon-based negative electrode material, and is also not conducive to the cycle performance and high-rate fast charging performance of the silicon-based negative electrode material.

[0009] Preferably, the mass proportion of the conductive metal carbon in the silicon-based negative electrode material is 2-5%. Controlling the mass proportion of the conductive metal carbon in the silicon-based negative electrode material within a certain range can ensure that the outer layer of the conductive metal carbon has a certain thickness, which can effectively protect the non-metallic doped silicon and improve the conductivity of the silicon-based negative electrode material, and ensure that the overall capacity of the silicon-based negative electrode material will not be excessively reduced.

[0010] Preferably, the D50 of the silicon-based negative electrode material is 0.5 to 1.5 μm. The particle size of the silicon-based negative electrode material has a significant effect on its electrochemical performance. If the D50 of the silicon-based negative electrode material is too small, it is easy to aggregate, and the overall structural stability deteriorates, which is not conducive to ensuring the processing of the pole piece, and is also not conducive to the performance and life of the pole piece. At the same time, the D50 is small and the specific surface area is large, the expansion and contraction are more intense, and the capacity loss is also greater. If the D50 of the silicon-based negative electrode material is too large, the specific surface area is small, the electrolyte infiltration performance is poor, the electron conduction and lithium ion deintercalation ability are deteriorated, and the cycle performance and high-rate fast charging performance of the silicon-based negative electrode material will also be degraded. Moreover, if the D50 is large, the silicon volume expansion stress is large, and the ability of the silicon-based negative electrode material to relieve the volume expansion stress is limited, and the silicon volume expansion stress cannot be relieved to a greater extent, which is easy to cause the structure of the silicon-based negative electrode material to rupture and degrade the cycle stability of the silicon-based negative electrode material.

[0011] Preferably, the thickness of the conductive metal carbon layer is 5 to 80 nm. If the conductive metal carbon layer is too thin, it cannot effectively protect the non-metallic doped silicon core, increase the interface side reaction, deteriorate the stability of the silicon-based negative electrode material, and cannot further improve the conductivity of the silicon-based composite material. If the conductive metal carbon layer is too thick, firstly, the surface porosity is reduced, which is not conducive to efficient lithium ion transmission, and at the same time, it will also reduce the overall capacity of the silicon-based negative electrode material, which is not conducive to the performance of the silicon-based material.

[0012] Preferably, the preparation of the above silicon-based negative electrode material includes the following steps: S1. Mix silicon powder and B oxide, and heat treat the obtained mixture at 900℃~1200℃ for 2~5h under a protective atmosphere to obtain a calcined product; S2. Remove silicon oxide in the calcined product to obtain non-metallic doped silicon; S3. Prepare a conductive metal carbon solution, disperse the non-metallic doped silicon in the conductive metal carbon solution, stir at 30~100℃ for 4~8h, and spray dry the obtained mixed system to obtain a silicon-based negative electrode material. The non-metallic oxide is reduced to a non-metallic element during the calcination process in S1, and silicon is oxidized to silicon oxide. After removing the silicon oxide by S2, non-metallic doped silicon is obtained. The above reaction steps enable non-metallic elements to be more incorporated into the silicon lattice, greatly increasing the number of majority carriers, i.e., free electrons (or holes) in the lattice, and the more majority carriers there are, the stronger the conductivity of the impurity semiconductor is, thereby greatly enhancing the conductivity of the silicon-based negative electrode material.

[0013] Preferably, in S1, the feeding amounts of silicon powder and B oxide are calculated based on the molar ratio of Si:B of (400-600):(2-8).

[0014] Preferably, in S1, the silicon powder particles D50 are 0.5-1 μm.

[0015] Preferably, in S1, during the heat treatment, the temperature is increased to 900°C to 1200°C at a heating rate of 4°C / min.

[0016] Preferably, in S1, during the heat treatment, the flow rate of the protective atmosphere is 3 L / min; the protective atmosphere includes nitrogen.

[0017] Preferably, in S1, the B oxide includes B2O3.

[0018] Preferably, in S2, hydrofluoric acid is used to remove silicon oxide in the calcined product.

[0019] Preferably, in S2, the specific operation of using hydrofluoric acid to remove silicon oxide in the calcined product is as follows: after the calcined product obtained in S1 is cooled to room temperature, it is added to hydrofluoric acid with a concentration of 3-6%, stirred into a slurry at 65-75°C, and then moved into a vacuum oven at 70-100°C overnight; S1 is repeated three times, that is, the hydrofluoric acid pickling is repeated three times.

[0020] Preferably, in S3, the mass fraction of the conductive metal carbon in the conductive metal carbon solution is 8-35%.

[0021] Preferably, in S3, the mass ratio of the non-metal-doped silicon to the conductive metal carbon solution is 2 to 12:1.

[0022] Preferably, in S3, the solvent used to prepare the conductive metal carbon solution includes at least one of ethanol and water.

[0023] According to the second aspect of the present invention, a negative electrode sheet is provided, comprising the above-mentioned silicon-based negative electrode material. The negative electrode sheet prepared by using the silicon-based negative electrode material improved by the present invention has excellent structural stability and conductivity, and the particle size of the silicon-based negative electrode material used can take into account the performance of the electrode sheet processability, electrolyte wettability, particle dispersibility, etc. Therefore, the negative electrode sheet prepared in this way also has excellent structural stability and conductivity, and there are no obvious cracks or structural defects on the surface after multiple charge and discharge cycles, so it has good cycle stability and high-rate fast charging performance.

[0024] According to a third aspect of the present invention, a battery is provided, comprising the above-mentioned negative electrode sheet. The battery prepared from the above-mentioned negative electrode sheet exhibits good room temperature cycle stability, high first efficiency and good high-rate fast charging performance because the overall structural stability and conductivity of the negative electrode sheet are significantly improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 It is a schematic diagram of the structure of the silicon negative electrode material in the present invention.

[0026] The reference numerals are: 1-core, 2-shell. DETAILED DESCRIPTION

[0027] In order to enable those skilled in the art to better understand the solutions of the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only embodiments of a part of the present invention, rather than all embodiments.

[0028] Example 1

[0029] 1. Preparation of silicon-based negative electrode materials

[0030] The silicon-based negative electrode material of this embodiment is prepared according to the following steps:

[0031] S1. Silicon powder and B2O3 were mixed, and the mixture was heated to 1150°C at a heating rate of 4°C / min for 3.5h in a nitrogen atmosphere at a flow rate of 3L / min to obtain a calcined product; the D50 of the silicon powder particles was 0.7; the amount of silicon powder and B2O3 was calculated based on a molar ratio of Si:B of 500:5;

[0032] S2. After the calcined product obtained in S1 is cooled to room temperature, it is added to hydrofluoric acid having a concentration of 3 to 6%, stirred at 70°C to form a slurry, and then moved into a vacuum oven at 85°C overnight; the hydrofluoric acid pickling is repeated three times and dried to obtain non-metallic doped silicon;

[0033] S3. Prepare a conductive metal carbon solution, disperse non-metallic doped silicon in the conductive metal carbon solution, stir at 60°C for 6 hours, and then spray-dry the resulting mixed system to obtain a silicon-based negative electrode material; the conductive metal carbon is Ti3C2(OH)2; in the conductive metal carbon solution, the mass fraction of the conductive metal carbon is 20wt%, and the mass ratio of the non-metallic doped silicon to the conductive metal carbon solution is 5:1, so that the D50 of the final silicon negative electrode material is 1.0 (μm, the thickness of the conductive metal carbon shell is 30-50nm, and the mass proportion of B in the silicon-based negative electrode material is 1.3%.

[0034] The schematic diagram of the structure of the silicon-based negative electrode material prepared in the above steps is shown in FIG. Figure 1 Except for Comparative Example 2, the structural diagrams of the silicon negative electrode materials in other embodiments and comparative examples are all referenced to Figure 1 , the silicon-based negative electrode material in Comparative Example 2 only has a core.

[0035] 2. Preparation of negative electrode and battery

[0036] (1) Preparation of negative electrode

[0037] The silicon negative electrode material, conductive agent SP, conductive agent SWCNT and binder PAA prepared above were dissolved in a solvent in a mass percentage of 90:3:1:6, mixed, and the solid content was controlled at 20-50%, coated on a copper foil current collector, and vacuum dried to obtain a negative electrode sheet.

[0038] (2) Preparation of batteries

[0039] The above-mentioned negative electrode sheet, the ternary positive electrode sheet prepared by traditional mature process (positive electrode active material is NCM811, NCM811, conductive SP, binder PVDF mass ratio is 93:3:4, 1 mol / L LiPF6 / EC+DMC+EMC (v / v=1:1:1) electrolyte, PE+alumina separator, shell are assembled into soft-pack batteries using conventional production processes.

[0040] Example 2

[0041] 1. Preparation of silicon-based negative electrode materials

[0042] In the preparation of the silicon-based negative electrode material in this embodiment, the difference from that in embodiment 1 is that in S3, the conductive metal carbon is Ti3AlC2. The remaining operations are the same as those in embodiment 1.

[0043] 2. Preparation of negative electrode and battery

[0044] The preparation of the negative electrode sheet and the battery of this embodiment is consistent with that of embodiment 1.

[0045] Example 3

[0046] 1. Preparation of silicon-based negative electrode materials

[0047] In the preparation of the silicon-based negative electrode material in this embodiment, the difference from the embodiment 1 is that in S1, the amount of B2O3 added is too small. Specifically, the amount of silicon powder and B2O3 added is calculated based on the molar ratio of Si:B of 500:2, so that the final mass proportion of B in the silicon-based negative electrode material is 0.5%. The rest of the operations are the same as in the embodiment 1.

[0048] 2. Preparation of negative electrode and battery

[0049] The preparation of the negative electrode sheet and the battery of this embodiment is consistent with that of embodiment 1.

[0050] Example 4

[0051] 1. Preparation of silicon-based negative electrode materials

[0052] In the preparation of the silicon-based negative electrode material in this embodiment, the difference from the embodiment 1 is that in S1, the amount of B2O3 added is too much, specifically, the amount of silicon powder and B2O3 added is calculated based on the molar ratio of Si:B being 550:8. The rest of the operations are the same as in the embodiment 1.

[0053] 2. Preparation of negative electrode and battery

[0054] The preparation of the negative electrode sheet and the battery of this embodiment is consistent with that of embodiment 1.

[0055] Example 5

[0056] 1. Preparation of silicon-based negative electrode materials

[0057] In the preparation of the silicon-based negative electrode material in this embodiment, the difference from the embodiment 1 is that in S1, the amount of B2O3 added is too small. Specifically, the amount of silicon powder and B2O3 added is calculated based on the molar ratio of Si:B of 600:1.5, so that the final mass proportion of B in the silicon-based negative electrode material is 0.05%. The rest of the operations are the same as in the embodiment 1.

[0058] 2. Preparation of negative electrode and battery

[0059] The preparation of the negative electrode sheet and the battery of this embodiment is consistent with that of embodiment 1.

[0060] Example 6

[0061] 1. Preparation of silicon-based negative electrode materials

[0062] In the preparation of the silicon-based negative electrode material in this embodiment, the difference from the embodiment 1 is that in S1, the amount of B2O3 added is too small. Specifically, the amount of silicon powder and B2O3 added is calculated based on the molar ratio of Si:B of 600:15, so that the final mass proportion of B in the silicon-based negative electrode material is 2.3%. The rest of the operations are the same as in the embodiment 1.

[0063] 2. Preparation of negative electrode and battery

[0064] The preparation of the negative electrode sheet and the battery of this embodiment is consistent with that of embodiment 1.

[0065] Example 7

[0066] 1. Preparation of silicon-based negative electrode materials

[0067] In the preparation of the silicon-based negative electrode material in this embodiment, the difference from that in embodiment 1 is that in S3, the mass fraction of the conductive metal carbon in the conductive metal carbon solution is 13wt%, so that the thickness of the conductive metal carbon shell in the final silicon negative electrode material is 5-15nm. The rest of the operations are the same as in embodiment 1.

[0068] 2. Preparation of negative electrode and battery

[0069] The preparation of the negative electrode sheet and the battery of this embodiment is consistent with that of embodiment 1.

[0070] Example 8

[0071] 1. Preparation of silicon-based negative electrode materials

[0072] In the preparation of the silicon-based negative electrode material in this embodiment, the difference from that in embodiment 1 is that in S3, the mass fraction of the conductive metal carbon in the conductive metal carbon solution is 35wt%, so that the thickness of the conductive metal carbon shell in the final silicon negative electrode material is 65-80nm. The rest of the operations are the same as in embodiment 1.

[0073] 2. Preparation of negative electrode and battery

[0074] The preparation of the negative electrode sheet and the battery of this embodiment is consistent with that of embodiment 1.

[0075] Example 9

[0076] 1. Preparation of silicon-based negative electrode materials

[0077] In the preparation of the silicon-based negative electrode material in this embodiment, the difference from that in embodiment 1 is that in S3, during the spray drying process, the mass fraction of the conductive metal carbon in the conductive metal carbon solution is 45wt%, so that the thickness of the conductive metal carbon shell in the final silicon negative electrode material is 85-100nm. The remaining operations are consistent with embodiment 1.

[0078] 2. Preparation of negative electrode and battery

[0079] The preparation of the negative electrode sheet and the battery of this embodiment is consistent with that of embodiment 1.

[0080] Example 10

[0081] 1. Preparation of silicon-based negative electrode materials

[0082] In the preparation of the silicon-based negative electrode material in this embodiment, the difference from that in embodiment 1 is that in S1, the D50 of the silicon powder particles is 0.3 μm, so that the D50 of the final silicon negative electrode material is 0.4 μm. The rest of the operations are the same as those in embodiment 1.

[0083] 2. Preparation of negative electrode and battery

[0084] The preparation of the negative electrode sheet and the battery of this embodiment is consistent with that of embodiment 1.

[0085] Embodiment 11

[0086] 1. Preparation of silicon-based negative electrode materials

[0087] In the preparation of the silicon-based negative electrode material in this embodiment, the difference from that in embodiment 1 is that in S1, the D50 of the silicon powder particles is 1.6 μm, so that the D50 of the final silicon negative electrode material is 1.8 μm. The rest of the operations are the same as those in embodiment 1.

[0088] 2. Preparation of negative electrode and battery

[0089] The preparation of the negative electrode sheet and the battery of this embodiment is consistent with that of embodiment 1.

[0090] Comparative Example 1

[0091] 1. Preparation of silicon-based negative electrode materials

[0092] In the preparation of the silicon-based negative electrode material of this comparative example, the difference from Example 1 is that steps S1 to S2 are not performed, and in S3, the silicon particles are directly mixed with the conductive polymer solution and spray-dried.

[0093] 2. Preparation of negative electrode and battery

[0094] The preparation of the negative electrode sheet and the battery in this comparative example is consistent with that in Example 1.

[0095] Comparative Example 2

[0096] 1. Preparation of silicon-based negative electrode materials

[0097] In the preparation of the silicon-based negative electrode material of this comparative example, the difference from Example 1 is that step S3 is not performed, and the non-metal-doped silicon prepared in S3 is directly used as the silicon negative electrode material.

[0098] 2. Preparation of negative electrode and battery

[0099] The preparation of the negative electrode sheet and the battery in this comparative example is consistent with that in Example 1.

[0100] Comparative Example 3

[0101] 1. Preparation of silicon-based negative electrode materials

[0102] In the preparation of the silicon-based negative electrode material of this comparative example, the difference from Example 1 is that the non-metal-doped silicon obtained in S3 is coated with a carbon layer shell, that is, the operation of S3 is changed to the following: the non-metal-doped silicon is introduced into a fluidized bed atmosphere furnace, heated to 700°C under an inert atmosphere, and carbon source gas ethylene is introduced, kept warm for 6 hours, and then the carbon source gas is turned off and cooled to room temperature to obtain a silicon negative electrode material. In the above process, the flow rate of the carbon source gas ethylene is controlled to be 50L / min, and the amount of non-metal-doped silicon is consistent with that in Example 1, so that the D50, shell thickness, and mass proportion of non-metal B in the silicon-based negative electrode material obtained are consistent with those in Example 1. The rest of the operations are consistent with Example 1.

[0103] 2. Preparation of negative electrode and battery

[0104] The preparation of the negative electrode sheet and the battery in this comparative example is consistent with that in Example 1.

[0105] Comparative Example 4

[0106] 1. Preparation of silicon-based negative electrode materials

[0107] In the preparation of the silicon-based negative electrode material of this comparative example, the difference from Example 1 is that the B oxide obtained in S1 is replaced by arsenic pentoxide (As2O5). The remaining operations are consistent with Example 1.

[0108] 2. Preparation of negative electrode and battery

[0109] The preparation of the negative electrode sheet and the battery in this comparative example is consistent with that in Example 1.

[0110] Test Case

[0111] 1. Experimental Construction Method

[0112] The batteries prepared in all the above embodiments and comparative examples were subjected to relevant electrochemical performance tests, specifically, the tests were conducted on the LAND battery test system of Wuhan Jinnuo Electronics Co., Ltd. at room temperature (25°C), and the charge and discharge voltage was limited to 2.5V to 4.2V. The calculation method or test conditions for the first efficiency (first charge and discharge efficiency), cycle performance and rate performance are as follows:

[0113] (1) Initial efficiency: total capacity of battery discharged at 0.33C for the first time / total capacity of battery charged at 0.33C for the first time

[0114] (2) Capacity retention rate after 500 cycles of 2C / 2C at room temperature

[0115] At 25℃, charge at 2C constant current and constant voltage to 4.2V, cut off at 0.05C, let stand for 10min, discharge at 2C constant current to 2.5V, let stand for 10min, cycle for 500 weeks, and record the battery 2C / 2C cycle 500-week capacity retention rate.

[0116] (3) 6C rate performance at room temperature

[0117] 6C rate charging: at 25℃, discharge at 1C constant current to 2.5V, let stand for 10min, charge at 6C constant current and constant voltage to 4.2V, cut off at 0.05C, record the battery constant current charging capacity, constant current and constant voltage charging total capacity and the highest temperature during fast charging, constant current charging ratio = constant current charging capacity / constant current and constant voltage charging total capacity.

[0118] 2. Experimental results

[0119] The test results of the first efficiency (first charge and discharge efficiency), cycle performance and rate performance of the batteries prepared in all the above embodiments and comparative examples are shown in Table 1.

[0120] Table 1 Related performance test results of the batteries prepared in the examples and comparative examples

[0121]

[0122]

[0123] It can be seen from Table 1 that the battery prepared using the silicon-based negative electrode material provided by the present invention can effectively alleviate the volume expansion stress of silicon during the charge and discharge cycle because the silicon-based negative electrode material has excellent conductivity and the silicon-based negative electrode material itself has a stable structure. Therefore, the battery's first efficiency, room temperature cycle performance and high-rate fast charging performance are optimized. Please refer to Examples 1 to 11 for details.

[0124] In the silicon-based negative electrode material in Comparative Example 1, non-metal B is not doped in the core, so the conductivity of silicon cannot be effectively improved, and the "buffer skeleton" function of the non-metallic elements is lost, resulting in a decrease in the conductivity and structural stability of the silicon-based negative electrode material, thereby causing a decrease in the battery's first efficiency, room temperature cycle performance, high-rate fast charging performance, and high-rate fast charging thermal stability.

[0125] In the silicon-based negative electrode material in Comparative Example 2, there is only a non-metal-doped silicon core, but no conductive metal carbon layer is coated. The protective effect of the core is reduced, the core is in direct contact with the electrolyte, and the degree of side reactions increases, which will lead to a decrease in the structural stability of the silicon-based negative electrode material. At the same time, without the conductive metal carbon layer coated on the outside, the overall volume expansion mitigation performance of the silicon-based negative electrode material is also reduced. As a result, the battery prepared with the silicon-based negative electrode material has a decrease in the first effect, room temperature cycle performance, high-rate fast charging performance, high-rate fast charging thermal stability and other aspects.

[0126] In the silicon-based negative electrode material in Comparative Example 3, the outer shell is a carbon layer. Compared with the conductive metal carbon layer, due to the lack of the metal-Si effect, the connection tightness between the carbon layer and the non-metal doped silicon core is reduced, which will cause the overall structural stability of the silicon-based negative electrode material to decrease during the charge and discharge cycle. At the same time, the material capacity will be reduced when the carbon layer is used compared with the conductive metal carbon layer. The above reasons cause the battery prepared with the silicon-based negative electrode material to have a decline in performance in various aspects.

[0127] In the silicon-based negative electrode material in Comparative Example 4, the doped non-metallic element is arsenic As. As has limited effect on further improving the conductivity of silicon and will affect the capacity of the silicon material, thereby causing a decrease in various aspects of the performance of the battery prepared with the silicon-based negative electrode material.

[0128] Further observation of Example 1 and Example 2 shows that when the type of conductive metal carbon is changed, the silicon-based negative electrode material still has good conductivity and structural stability, as can be seen from the fact that the batteries prepared corresponding to these silicon-based negative electrode materials have higher first efficiency, better room temperature cycle performance, and high rate performance.

[0129] Comparing Example 1 with Examples 3 to 6, it can be found that the doping amount of non-metallic elements such as B has a certain influence on the performance of silicon-based negative electrode materials, and thus affects the electrochemical performance of the battery. The non-metallic element B in Examples 5 and 6 is 0.05% and 2.3%, respectively, which is too little and too much relative to Examples 1 and 3 to 4. Too little non-metallic elements cannot effectively improve the conductivity of silicon, and have limited effect on alleviating silicon volume expansion, resulting in a decrease in various aspects of battery performance; too much non-metallic elements will affect the capacity of silicon, and is not conducive to the material properties of silicon-based negative electrode materials, and ultimately cause a decrease in various aspects of battery performance.

[0130] By comparing Example 1 with Examples 7 to 9, it can be found that when the thickness of the conductive metal carbon layer shell is changed, the structural stability or conductivity of the silicon-based negative electrode material will also be significantly affected, which is specifically manifested as the electrochemical performance of the battery is also affected. For example, in Example 8, if the thickness of the conductive metal carbon shell is too thick, the surface porosity will be reduced, which is not conducive to efficient lithium ion transmission, and will also reduce the overall capacity of the silicon-based negative electrode material, and will not be conducive to the performance of the silicon-based material, thus causing the performance of the battery in Example 8 to decline in all aspects. Similarly, if the conductive metal carbon layer shell is too thin, it is also proportional to the overall performance of the silicon-based negative electrode material, because the thickness of the conductive metal carbon layer is too thin, it cannot effectively protect the non-metallic doped silicon core, increase the interface side reaction, deteriorate the stability of the silicon-based negative electrode material, and cannot further improve the conductivity of the silicon-based composite material. At the same time, it is also difficult to coat a thinner conductive metal carbon layer shell, which can easily cause uneven coating, and the performance of the conductive metal carbon coating cannot be exerted, and even cause the conductive metal carbon coating to fall off easily, deteriorating the structural stability of the silicon-based negative electrode material.

[0131] Comparing Example 1 with Examples 10 to 11, it can be found that the silicon-based negative electrode material D50 finally prepared will also affect the electrochemical performance of the final battery. This is because if D50 is too small, it is easy to aggregate, and the overall structural stability deteriorates, which is not conducive to ensuring the processing of the pole piece, and is also not conducive to the performance and life of the pole piece, resulting in a decrease in various aspects of the battery performance. If D50 is too large, the silicon volume expansion stress is large, and the silicon-based negative electrode material has limited ability to alleviate the volume expansion stress, and cannot alleviate the silicon volume expansion stress to a greater extent, resulting in a decrease in the structural stability of the silicon-based negative electrode material, and causing the battery performance to decline in various aspects.

[0132] The above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit the protection scope of the present invention. Although the present invention is described in detail with reference to the above embodiments, ordinary technicians in the relevant field should understand that the technical solutions of the present invention can be modified or equivalently replaced, but these modifications or replacements are all within the protection scope of the present invention.

Claims

1. A silicon-based negative electrode material, characterized in that: It comprises a core and a shell covering the core, wherein the core comprises non-metallic doped silicon, and the shell comprises a conductive metal carbon layer; In the non-metal doped silicon, the non-metal includes B; In the conductive metal carbon layer, the conductive metal carbon includes at least one of Ti3C2(OH)2 and Ti3AlC2.

2. The silicon-based negative electrode material according to claim 1, characterized in that: The mass proportion of B in the silicon-based negative electrode material is 0.5-2.0%.

3. The silicon-based negative electrode material according to claim 1, characterized in that: The conductive metal carbon accounts for 2-5% by mass in the silicon-based negative electrode material.

4. The silicon-based negative electrode material according to claim 1, characterized in that: The D50 of the silicon-based negative electrode material is 0.5-1.5 μm.

5. The silicon-based negative electrode material according to claim 1, characterized in that: The thickness of the conductive metal carbon layer is 5-80 nm.

6. The silicon-based negative electrode material according to claim 1, characterized in that: The preparation thereof comprises the following steps: S1. Mix silicon powder and B oxide, and heat treat the resulting mixture at 900°C to 1200°C for 2 to 5 hours under a protective atmosphere to obtain a calcined product; S2. removing silicon oxide from the calcined product to obtain the non-metal-doped silicon; S3. Prepare a conductive metal carbon solution, disperse the non-metallic doped silicon in the conductive metal carbon solution, stir at 30-100° C. for 4-8 hours, and then spray-dry the obtained mixed system to obtain the silicon-based negative electrode material.

7. The silicon-based negative electrode material according to claim 6, characterized in that: In S1, the feeding amounts of the silicon powder and the B oxide are calculated based on the molar ratio of Si:B of (400-600):(2-8).

8. The silicon-based negative electrode material according to claim 6, characterized in that: In S3, the mass ratio of the non-metal doped silicon to the conductive metal carbon solution is 2 to 12:

1.

9. A negative electrode sheet, characterized in that: It comprises the silicon-based negative electrode material as claimed in any one of claims 1 to 8.

10. A battery, characterized in that: Comprising the negative electrode sheet as claimed in claim 9.