Preparation method of ultrathin high-entropy nanosheet material
Ultrathin high-entropy nanosheet materials were prepared by ultrasonic treatment and freeze-drying, which solved the problems of complex process and insufficient industrial application in the nano-narcopy of high-entropy alloys, and achieved efficient and controllable nanosheet preparation, suitable for large-scale Large-scale industrial production and high-tech applications.
Patent Information
- Application Number
- CN202411184319.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-12-03
AI Technical Summary
The nano-narrowing research on high-entropy alloys has problems such as complex process and insufficient industrial application, which leads to limited application in actual production and lacks stable, reliable and low-cost batch preparation technology.
Ultrathin high-entropy nanosheet materials are prepared by using nickel, cobalt, iron, molybdenum and auxiliary metal elements (such as ruthenium, manganese, copper, zinc, vanadium). A uniform precursor mix is formed through ultrasonic treatment and centrifugal washing. The solution was sonicated and lyophilized in anhydrous ethanol to obtain ultrathin high entropy alloy nanosheet material with a particle size of 1 to 100 nm and a thickness of 1 to 10 nm.
It realizes mild reaction conditions, reduces energy consumption, simplifies process steps, improves the operability and universality of the process, can accurately adjust the morphology and performance of nanosheets, is suitable for large-scale industrial production, and meets electronics, catalytics and energy. Application requirements in areas such as storage.
Smart Images

Figure CN119061308A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of high entropy alloys, and in particular to a method for preparing an ultra-thin high entropy nanosheet material. Background Art
[0002] my country is accelerating the development of the new materials industry, especially the growing demand for advanced metal materials in special application fields. As a new type of material made of five or more types of metal elements, high entropy alloys are considered to be a new breakthrough in the field of alloys due to their diversity and complexity, opening a new chapter in the synthesis, analysis and control of metal materials. Its unique structure and properties make it one of the most promising advanced metal materials in the future, and it has received widespread attention in related research and application fields.
[0003] Judging from the current research results, the exploration of high entropy alloys by domestic and foreign researchers mainly focuses on the design of alloy systems, the optimization of preparation methods, and the relationship between alloy structure and performance. These studies provide a theoretical basis and technical support for the application of high entropy alloys. However, especially in the field of high entropy alloy nanomaterials, despite the emergence of a large number of research reports, its application still faces huge challenges. At present, most of the research on high entropy alloy nanomaterials is still in the laboratory stage, and there is still a distance from actual industrial application.
[0004] The reason for this phenomenon is that the research on high-entropy alloy nano-sizing involves the intersection of multiple disciplines, the process is complex, and the research is difficult. At the same time, despite the rich research results, there are few discussions on the industrialization of high-entropy alloy nano-sizing, which restricts its application and promotion in actual production. Therefore, how to obtain stable, reliable and industrial reference value experimental data, especially the process technology that can achieve low-cost and batch preparation, has become the key to promoting high-entropy alloys from laboratories to large-scale applications. This will help accelerate the research process of high-entropy alloys and promote their widespread application in various high-tech and industrial fields, ultimately achieving a leap from laboratory technology to large-scale production, and injecting new impetus into the development of the new materials industry.
[0005] In view of this, the present invention is proposed. Summary of the invention
[0006] The technical problem to be solved by the present invention is to overcome the deficiencies of the prior art, provide a method for preparing an ultra-thin high entropy nanosheet material, and solve the problems raised in the above-mentioned background technology.
[0007] In order to solve the above technical problems, the basic concept of the technical solution adopted by the present invention is:
[0008] A method for preparing an ultrathin high entropy nanosheet material, which is processed from the following components: nickel element, cobalt element, iron element, molybdenum element, boron element, and auxiliary metal element; the auxiliary metal element includes one or more of ruthenium element, manganese element, copper element, zinc element, and vanadium element.
[0009] Optionally, the nickel source is 0.1-0.4-0.4 mol / L nickel nitrate, the cobalt source is 0.1-0.4 mol / L cobalt nitrate, the iron source is 0.1-0.4 mol / L iron nitrate, the molybdenum source is 0.1-0.4 mol / L molybdenum chloride, and the auxiliary metal element is 0.1-0.4 mol / L one or more of ruthenium chloride, manganese nitrate, copper nitrate, zinc nitrate or vanadium chloride.
[0010] A method for preparing an ultrathin high entropy nanosheet material, characterized in that it comprises the following steps:
[0011] Step (1), adding a nickel source, a cobalt source, an iron source, a molybdenum source and an auxiliary metal element into an organic solvent in an equal molar ratio, and performing ultrasonic treatment to form a uniform precursor mixed solution①;
[0012] Step (2), adding a reducing agent dropwise to the precursor mixed solution and continuing ultrasonic treatment to obtain a mixed solution ②;
[0013] Step (3), centrifugally washing the mixed solution ② obtained after ultrasonication to obtain a solid ①;
[0014] Step (4), mixing the washed solid ① with an organic solvent and then subjecting it to ultrasonic treatment again to form a dispersion;
[0015] Step (5), quickly adding an alkaline solution to the dispersion and stirring, stirring evenly to obtain a solid ② and centrifuging and washing the solid ② to obtain a sample;
[0016] Step (6), freeze-drying the washed sample, and the solid obtained after drying is the ultra-thin high entropy alloy nanosheet material.
[0017] Optionally, the organic solvent in step (1) and step (4) is anhydrous ethanol with a volume of 50 mL, the ultrasonic time in step (1) and step (4) is 10 to 45 min, and the ultrasonic power is 700 to 900 watts.
[0018] Optionally, the reducing agent in step (2) is 0.5-1 mol / L sodium borohydride.
[0019] Optionally, the alkaline solution in step (5) is 0.3-1 mol / L potassium hydroxide, the stirring time is 20-30 min, and the stirring speed is 300-500 rpm / min.
[0020] Optionally, detergent is used for centrifugal washing in both step (3) and step (5), and the detergent is anhydrous ethanol. The centrifugation time of step (3) and step (5) is 1 to 3 minutes, and the rotation speed is 6000 to 8000 rpm / min.
[0021] Optionally, the freeze-drying process in step (6) is carried out at -50°C to -80°C, and the freeze-drying time is 20 to 24 hours.
[0022] Optionally, the particle size of the ultra-thin high entropy nanosheet material ranges from 1 to 100 nm, and the thickness is from 1 to 10 nm.
[0023] After adopting the above technical solution, the present invention has the following beneficial effects compared with the prior art. Of course, any product implementing the present invention does not necessarily need to achieve all the advantages described below at the same time:
[0024] 1. The reaction conditions of the present invention are relatively mild, avoiding the need for harsh conditions such as high temperature and high pressure, reducing energy consumption and reducing the complexity of operation. The entire process is simple and clear, easy to operate, and does not require complex equipment or cumbersome operating procedures, which greatly improves the operability and universality of the process. At the same time, the method shows extremely high accuracy and controllability in controlling the morphology of nanosheet materials, and can accurately adjust the thickness, size and morphology of the nanosheets according to specific needs. In addition, the process has high repeatability, ensuring the performance consistency of different batches of products, and is suitable for large-scale, efficient industrial production.
[0025] 2. The present invention is not only practical and economical in the production process, but also can achieve effective regulation of the elemental composition and microstructure of the alloy. This regulation capability is crucial for the performance optimization of alloy materials, so that key indicators such as mechanical properties, conductivity, and magnetism of the final product can meet the design requirements. Through this process, high-quality ultra-thin high-entropy nanosheet materials can be prepared to meet the application needs in high-tech fields such as electronics, catalysis, and energy storage.
[0026] The specific implementation modes of the present invention are further described in detail below with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] The drawings described below are only some embodiments. For those skilled in the art, other drawings can be obtained based on these drawings without creative work. In the drawings:
[0028] Figure 1 This is a scanning electron microscope image of the ultrathin (NiCoFeMoBRu)OH high entropy nanosheet obtained in Example 1 of the present invention;
[0029] Figure 2 X-ray diffraction patterns of ultrathin (NiCoFeCrMoBCu)OH and (NiCoFeCrMoBRu)OH high entropy nanosheets.
[0030] It should be noted that these drawings and textual descriptions are not intended to limit the conceptual scope of the present invention in any way, but are intended to illustrate the concept of the present invention for those skilled in the art by referring to specific embodiments. DETAILED DESCRIPTION
[0031] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0032] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0033] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0034] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present application description and examples are exemplary only.
[0035] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0036] See also Figure 1-2 As shown, in this embodiment, an ultrathin high entropy nanosheet material is provided, which is processed by the following components: nickel element, cobalt element, iron element, molybdenum element, boron element, and auxiliary metal element; the auxiliary metal element includes one or more of ruthenium element, manganese element, copper element, zinc element, and vanadium element.
[0037] In some embodiments of the present invention, the nickel source is 0.1-0.4-0.4 mol / L nickel nitrate, the cobalt source is 0.1-0.4 mol / L cobalt nitrate, the iron source is 0.1-0.4 mol / L iron nitrate, the molybdenum source is 0.1-0.4 mol / L molybdenum chloride, and the auxiliary metal element is 0.1-0.4 mol / L one or more of ruthenium chloride, manganese nitrate, copper nitrate, zinc nitrate or vanadium chloride.
[0038] A method for preparing an ultrathin high entropy nanosheet material comprises the following steps:
[0039] Step (1), adding a nickel source, a cobalt source, an iron source, a molybdenum source and an auxiliary metal element into an organic solvent in an equal molar ratio, and performing ultrasonic treatment to form a uniform precursor mixed solution①;
[0040] Step (2), adding a reducing agent dropwise to the precursor mixed solution and continuing ultrasonic treatment to obtain a mixed solution ②;
[0041] Step (3), centrifugally washing the mixed solution ② obtained after ultrasonication to obtain a solid ①;
[0042] Step (4), mixing the washed solid ① with an organic solvent and then subjecting it to ultrasonic treatment again to form a dispersion;
[0043] Step (5), quickly adding an alkaline solution to the dispersion and stirring, stirring evenly to obtain a solid ② and centrifuging and washing the solid ② to obtain a sample;
[0044] Step (6), freeze-drying the washed sample, and the solid obtained after drying is the ultra-thin high entropy alloy nanosheet material.
[0045] In some embodiments of the present invention, the organic solvent in step (1) and step (4) is anhydrous ethanol with a volume of 50 mL, the ultrasonic time in step (1) and step (4) is 10 to 45 min, and the ultrasonic power is 700 to 900 watts.
[0046] The method for preparing an ultrathin high entropy nanosheet material according to claim 2, characterized in that the reducing agent in step (2) is 0.5 mol / L sodium borohydride.
[0047] In some embodiments of the present invention, the alkaline solution in step (5) is 1 mol / L potassium hydroxide, the stirring time is 20 to 30 min, and the stirring speed is 300 to 500 rpm / min.
[0048] In some embodiments of the present invention, detergent is used for centrifugal washing in step (3) and step (5), and the detergent is anhydrous ethanol. The centrifugation time of step (3) and step (5) is 3 minutes, and the rotation speed is 6000-8000 rpm / min.
[0049] In some embodiments of the present invention, the freeze-drying process in step (6) is carried out at -50°C to -80°C, and the freeze-drying time is 20 to 24 hours.
[0050] In some embodiments of the present invention, the particle size of the ultra-thin high entropy nanosheet material is in the range of 100 nm and the thickness is 10 nm.
[0051] The present invention will now be further described in detail with reference to embodiments.
[0052] It should be noted that all raw materials in the examples of the present invention were obtained through commercial sources.
[0053] Example 1: A method for preparing an ultrathin high entropy nanosheet (NiCoFeMoBRu)OH, the method specifically comprising the following steps:
[0054] Step (1), adding 0.1 mol / L nickel nitrate, 0.1 mol / L cobalt nitrate, 0.1 mol / L iron nitrate, 0.1 mol / L molybdenum chloride and 0.1 mol / L ruthenium chloride in an equal molar ratio into anhydrous ethanol for ultrasonic treatment to form a uniform precursor mixed solution ①, the ultrasonic time during the ultrasonic treatment is 45 min; the ultrasonic power is 900 watts;
[0055] Step (2), adding 0.5 mol / L sodium borohydride dropwise to the precursor mixed solution and continuing ultrasonic treatment to obtain a mixed solution ②, wherein the ultrasonic treatment time is 45 min; the ultrasonic power is 900 watts;
[0056] Step (3), the mixed solution ② obtained after ultrasonic treatment is centrifuged and washed using a centrifuge and anhydrous ethanol to obtain a solid ①, wherein the centrifugation time is 3 minutes and the rotation speed is 8000 rpm / min;
[0057] Step (4), mixing the washed solid ① with anhydrous ethanol and then subjecting it to ultrasonic treatment again to form a dispersion, wherein the ultrasonic treatment time is 45 minutes; the ultrasonic power is 900 watts;
[0058] Step (5), quickly adding an alkaline solution to the dispersion and stirring at a speed of 500 rpm / min for 30 minutes, stirring evenly to obtain a solid ②, and after obtaining the solid ②, centrifuging and washing the solid ② using a centrifuge and anhydrous ethanol to obtain a sample, wherein the centrifugation time is 3 minutes and the rotation speed is 8000 rpm / min;
[0059] Step (6), freeze-drying the washed sample, and the solid obtained after drying is the ultra-thin high entropy alloy nanosheet material. The freeze-drying process is carried out at -80°C for 24 hours.
[0060] Example 2: A method for preparing an ultrathin high entropy nanosheet (NiCoFeMoBCu)OH, the method specifically comprising the following steps:
[0061] Step (1), adding 0.1 mol / L nickel nitrate, 0.1 mol / L cobalt nitrate, 0.1 mol / L iron nitrate, 0.1 mol / L molybdenum chloride and 0.1 mol / L copper nitrate in an equal molar ratio into anhydrous ethanol for ultrasonic treatment to form a uniform precursor mixed solution ①, the ultrasonic time during the ultrasonic treatment is 45 min; the ultrasonic power is 900 watts;
[0062] Step (2), adding 0.5 mol / L sodium borohydride dropwise to the precursor mixed solution and continuing ultrasonic treatment to obtain a mixed solution ②, wherein the ultrasonic treatment time is 45 min; the ultrasonic power is 900 watts;
[0063] Step (3), the mixed solution ② obtained after ultrasonic treatment is centrifuged and washed using a centrifuge and anhydrous ethanol to obtain a solid ①, wherein the centrifugation time is 3 minutes and the rotation speed is 8000 rpm / min;
[0064] Step (4), mixing the washed solid ① with anhydrous ethanol and then subjecting it to ultrasonic treatment again to form a dispersion, wherein the ultrasonic treatment time is 45 minutes; the ultrasonic power is 900 watts;
[0065] Step (5), quickly adding an alkaline solution to the dispersion and stirring at a speed of 500 rpm / min for 30 minutes, stirring evenly to obtain a solid ②, and after obtaining the solid ②, centrifuging and washing the solid ② using a centrifuge and anhydrous ethanol to obtain a sample, wherein the centrifugation time is 3 minutes and the rotation speed is 8000 rpm / min;
[0066] Step (6), freeze-drying the washed sample, and the solid obtained after drying is the ultra-thin high entropy alloy nanosheet material. The freeze-drying process is carried out at -80°C for 24 hours.
[0067] Example 3: A method for preparing an ultrathin high entropy nanosheet (NiCoFeMoBMn)OH, the method specifically comprising the following steps:
[0068] Step (1), adding 0.1 mol / L nickel nitrate, 0.1 mol / L cobalt nitrate, 0.1 mol / L iron nitrate, 0.1 mol / L molybdenum chloride and 0.1 mol / L manganese nitrate in an equal molar ratio into anhydrous ethanol for ultrasonic treatment to form a uniform precursor mixed solution ①, the ultrasonic time during the ultrasonic treatment is 45 min; the ultrasonic power is 900 watts;
[0069] Step (2), adding 0.5 mol / L sodium borohydride dropwise to the precursor mixed solution and continuing ultrasonic treatment to obtain a mixed solution ②, wherein the ultrasonic treatment time is 45 min; the ultrasonic power is 900 watts;
[0070] Step (3), the mixed solution ② obtained after ultrasonic treatment is centrifuged and washed using a centrifuge and anhydrous ethanol to obtain a solid ①, wherein the centrifugation time is 3 minutes and the rotation speed is 8000 rpm / min;
[0071] Step (4), mixing the washed solid ① with anhydrous ethanol and then subjecting it to ultrasonic treatment again to form a dispersion, wherein the ultrasonic treatment time is 45 minutes; the ultrasonic power is 900 watts;
[0072] Step (5), quickly adding an alkaline solution to the dispersion and stirring at a speed of 500 rpm / min for 30 minutes, stirring evenly to obtain a solid ②, and after obtaining the solid ②, centrifuging and washing the solid ② using a centrifuge and anhydrous ethanol to obtain a sample, wherein the centrifugation time is 3 minutes and the rotation speed is 8000 rpm / min;
[0073] Step (6), freeze-drying the washed sample, and the solid obtained after drying is the ultra-thin high entropy alloy nanosheet material. The freeze-drying process is carried out at -80°C for 24 hours.
[0074] Example 4: A method for preparing an ultrathin high entropy nanosheet (NiCoFeMoBZn)OH, the method specifically comprising the following steps:
[0075] Step (1), adding 0.1 mol / L nickel nitrate, 0.1 mol / L cobalt nitrate, 0.1 mol / L iron nitrate, 0.1 mol / L molybdenum chloride and 0.1 mol / L zinc nitrate in an equal molar ratio into anhydrous ethanol for ultrasonic treatment to form a uniform precursor mixed solution ①, the ultrasonic time during the ultrasonic treatment is 45 min; the ultrasonic power is 900 watts;
[0076] Step (2), adding 0.5 mol / L sodium borohydride dropwise to the precursor mixed solution and continuing ultrasonic treatment to obtain a mixed solution ②, wherein the ultrasonic treatment time is 45 min; the ultrasonic power is 900 watts;
[0077] Step (3), the mixed solution ② obtained after ultrasonic treatment is centrifuged and washed using a centrifuge and anhydrous ethanol to obtain a solid ①, wherein the centrifugation time is 3 minutes and the rotation speed is 8000 rpm / min;
[0078] Step (4), mixing the washed solid ① with anhydrous ethanol and then subjecting it to ultrasonic treatment again to form a dispersion, wherein the ultrasonic treatment time is 45 minutes; the ultrasonic power is 900 watts;
[0079] Step (5), quickly adding an alkaline solution to the dispersion and stirring at a speed of 500 rpm / min for 30 minutes, stirring evenly to obtain a solid ②, and after obtaining the solid ②, centrifuging and washing the solid ② using a centrifuge and anhydrous ethanol to obtain a sample, wherein the centrifugation time is 3 minutes and the rotation speed is 8000 rpm / min;
[0080] Step (6), freeze-drying the washed sample, and the solid obtained after drying is the ultra-thin high entropy alloy nanosheet material. The freeze-drying process is carried out at -80°C for 24 hours.
[0081] Example 5: A method for preparing an ultrathin high entropy nanosheet (NiCoFeMoBV)OH, the method specifically comprising the following steps:
[0082] Step (1), adding 0.1 mol / L nickel nitrate, 0.1 mol / L cobalt nitrate, 0.1 mol / L iron nitrate, 0.1 mol / L molybdenum chloride and 0.1 mol / L vanadium chloride in an equal molar ratio to anhydrous ethanol for ultrasonic treatment to form a uniform precursor mixed solution ①, the ultrasonic time during the ultrasonic treatment is 45 min; the ultrasonic power is 900 watts;
[0083] Step (2), adding 0.5 mol / L sodium borohydride dropwise to the precursor mixed solution and continuing ultrasonic treatment to obtain a mixed solution ②, wherein the ultrasonic treatment time is 45 min; the ultrasonic power is 900 watts;
[0084] Step (3), the mixed solution ② obtained after ultrasonic treatment is centrifuged and washed using a centrifuge and anhydrous ethanol to obtain a solid ①, wherein the centrifugation time is 3 minutes and the rotation speed is 8000 rpm / min;
[0085] Step (4), mixing the washed solid ① with anhydrous ethanol and then subjecting it to ultrasonic treatment again to form a dispersion, wherein the ultrasonic treatment time is 45 minutes; the ultrasonic power is 900 watts;
[0086] Step (5), quickly adding an alkaline solution to the dispersion and stirring at a speed of 500 rpm / min for 30 minutes, stirring evenly to obtain a solid ②, and after obtaining the solid ②, centrifuging and washing the solid ② using a centrifuge and anhydrous ethanol to obtain a sample, wherein the centrifugation time is 3 minutes and the rotation speed is 8000 rpm / min;
[0087] Step (6), freeze-drying the washed sample, and the solid obtained after drying is the ultra-thin high entropy alloy nanosheet material. The freeze-drying process is carried out at -80°C for 24 hours.
[0088] The present invention is not limited to the above-mentioned embodiments. Anyone should be aware that any structural changes made under the enlightenment of the present invention, and any technical solutions that are the same or similar to the present invention, fall within the protection scope of the present invention. The technology, shape, and structural parts not described in detail in the present invention are all well-known technologies.
Claims
1. An ultra-thin high entropy nanosheet material, It is characterized in that Made from the following components: Nickel, cobalt, iron, molybdenum, boron, and auxiliary metal elements; the auxiliary metal elements include one or more of ruthenium, manganese, copper, zinc, and vanadium.
2. The ultrathin high entropy nanosheet material according to claim 1, It is characterized in that The nickel source is 0.1-0.4-0.4 mol / L nickel nitrate, the cobalt source is 0.1-0.4 mol / L cobalt nitrate, the iron source is 0.1-0.4 mol / L iron nitrate, the molybdenum source is 0.1-0.4 mol / L molybdenum chloride, and the auxiliary metal element is 0.1-0.4 mol / L one or more of ruthenium chloride, manganese nitrate, copper nitrate, zinc nitrate or vanadium chloride.
3. A method for preparing ultrathin high entropy nanosheet materials, It is characterized in that The following steps are involved: Step (1), adding a nickel source, a cobalt source, an iron source, a molybdenum source and an auxiliary metal element into an organic solvent in an equal molar ratio, and performing ultrasonic treatment to form a uniform precursor mixed solution①; Step (2), adding a reducing agent dropwise to the precursor mixed solution and continuing ultrasonic treatment to obtain a mixed solution ②; Step (3), centrifugally washing the mixed solution ② obtained after ultrasonication to obtain a solid ①; Step (4), mixing the washed solid ① with an organic solvent and then subjecting it to ultrasonic treatment again to form a dispersion; Step (5), quickly adding an alkaline solution to the dispersion and stirring, stirring evenly to obtain a solid ② and centrifuging and washing the solid ② to obtain a sample; Step (6), freeze-drying the washed sample, and the solid obtained after drying is the ultra-thin high entropy alloy nanosheet material.
4. The method for preparing an ultrathin high entropy nanosheet material according to claim 2, It is characterized in that The organic solvent in step (1) and step (4) is anhydrous ethanol with a volume of 50 mL. The ultrasonic time in step (1) and step (4) is 10 to 45 min, and the ultrasonic power is 700 to 900 watts.
5. The method for preparing an ultrathin high entropy nanosheet material according to claim 2, It is characterized in that The reducing agent in step (2) is 0.5-1 mol / L sodium borohydride.
6. The method for preparing an ultrathin high entropy nanosheet material according to claim 2, It is characterized in that The alkaline solution in step (5) is 0.3-1 mol / L potassium hydroxide, the stirring time is 20-30 min, and the stirring speed is 300-500 rpm / min.
7. The method for preparing an ultrathin high entropy nanosheet material according to claim 2, It is characterized in that In step (3) and step (5), detergent is used for washing during centrifugal washing, and the detergent is anhydrous ethanol. The centrifugal time of step (3) and step (5) is 1 to 3 minutes, and the rotation speed is 6000 to 8000 rpm / min.
8. The method for preparing an ultrathin high entropy nanosheet material according to claim 2, It is characterized in that The freeze-drying process in step (6) is carried out at -50°C to -80°C, and the freeze-drying time is 20 to 24 hours.
9. The method for preparing an ultrathin high entropy nanosheet material according to claim 2, It is characterized in that The particle size of the ultra-thin high entropy nanosheet material ranges from 1 to 100 nm, and the thickness ranges from 1 to 10 nm.