High-temperature-resistant and acetic-acid-resistant conductive paste and photovoltaic module

A high temperature and acetic acid resistant conductive paste, using specific glass powders and additives, addresses the corrosion issue caused by EVA decomposition, maintaining battery efficiency and electrical performance in photovoltaic modules.

CN119069158AActive Publication Date: 2024-12-03ZHEJIANG JINKO NEW MATERIAL CO LTD

Patent Information

Application Number
CN202411191361.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-12-03
Estimated Expiration
2044-08-27

AI Technical Summary

Technical Problem

The decomposition of EVA under high temperature conditions in photovoltaic modules produces acetic acid, which corrodes electrodes and reduces battery efficiency by interacting with metallization, causing degradation of the interface between the front metal contact and the silicon substrate, leading to increased contact resistance and dark areas in electroluminescence imaging.

Method used

A high temperature and acetic acid resistant conductive paste is developed, comprising a main glass powder and a secondary glass powder, with specific molar percentages of Bi2O3, TeO2, SiO2, GeO2, B2O3, and Al2O3, along with modifying additives, to improve chemical stability and resist acetic acid corrosion.

Benefits of technology

The paste enhances the resistance of the electrode grid to acetic acid, maintaining electrical performance and reducing the impact of acetic acid on battery efficiency, with improved solubility and corrosion resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069158A_ABST
    Figure CN119069158A_ABST
Patent Text Reader

Abstract

The invention provides high-temperature-resistant and acetic-acid-resistant conductive paste and a photovoltaic module. The high-temperature-resistant and acetic-acid-resistant conductive paste comprises main glass powder and auxiliary glass powder, the mass fraction of the main glass powder in the paste is 1.5-2.5%, the mass fraction of the auxiliary glass powder is 0.2-1%, the auxiliary glass powder is Bi-Si-B-Al series glass, and the total molar percentage content of the auxiliary glass powder is 100%. The auxiliary glass powder comprises the following components in percentage by weight: 10%-50% of Bi2O3 and TeO2, 15%-30% of SiO2 and GeO2, 18%-30% of B2O3, 30%-20% of Al2O3 and 1%-20% of a modified additive. The paste further comprises silver powder and an organic carrier, in the paste, the mass fraction of the silver powder is 83%-90%, and the mass fraction of the organic carrier is 8%-15%. According to the paste disclosed by the invention, the low solubility of the electrode grid line in acetic acid is adjusted through the auxiliary glass, so that the problem that the battery efficiency is influenced by acetic acid generated by EVA decomposition under a high-temperature condition in a double-sided EVA assembly packaging battery is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of photovoltaic technology, and in particular to a high temperature and acetic acid resistant conductive paste and a photovoltaic module. Background Art

[0002] EVA is a transparent colloid with good flexibility and bonding properties, good light transmission and aging resistance. It encapsulates the crystalline silicon wafer group "upper cover and lower pad", and is bonded to the upper protective material glass and the lower protective material TPT by vacuum lamination technology to form a crystalline silicon module. Single-glass photovoltaic modules absorb solar energy from one side of the module; while double-glass photovoltaic modules absorb solar energy from both sides, and are composed of two pieces of tempered glass, POE or EVA films, and solar cells.

[0003] The official name of EVA resin is ethylene-vinyl acetate copolymer. The vinyl acetate content in EVA used in photovoltaic modules is usually 28-33%. Under high temperature and high humidity environment, the hydrolysis of EVA to produce acetic acid is inevitable. The acetic acid slowly accumulated in photovoltaic modules has become an important cause of quality problems in most photovoltaic modules. Under high temperature and high humidity acetic acid environment, the solar minority carrier lifetime is affected, the metal electrode contact site and Ag-Si ohmic contact are greatly reduced, and the power of the module is severely attenuated as the wet and hot time increases. Therefore, the acetic acid produced under high temperature conditions leads to reduced battery performance, interacts with the electrode, causes the metallization site and the cell interface to degrade, the contact resistance increases, and the EL imaging is a dark area, which seriously affects the battery efficiency.

[0004] In order to solve the problem that acetic acid produced by the decomposition of EVA under high temperature conditions affects the efficiency of double-sided EVA module encapsulated batteries, the present application provides a high temperature and acetic acid resistant conductive paste and photovoltaic module. Summary of the invention

[0005] In order to solve the problem that the acetic acid produced by the decomposition of EVA under high temperature conditions affects the efficiency of the battery in the double-sided EVA component packaging battery, the present application provides a high temperature resistant and acetic acid resistant conductive paste, the paste includes a main glass powder and a secondary glass powder, the mass fraction of the main glass powder in the paste is 1.5% to 2.5%, the mass fraction of the secondary glass powder is 0.2% to 1%, the secondary glass powder is Bi-Si-B-Al glass, and the total molar percentage content of the secondary glass powder is 100%, the secondary glass powder includes Bi 2 O 3 and TeO 2 Total 10% to 50%, SiO 2 and GeO 2 Total 15% to 30%, B 2 O 3 18%~30%,Al 2 O3 0%~20% and modified additives 1%~20%.

[0006] Acetic acid is a decomposition product of ethylene vinyl acetate (EVA), a common module encapsulation material, which interacts with metallization, often causing degradation of the interface between the front metal contact and the underlying silicon (Si) substrate. This leads to loss of cell performance and contact adhesion, increased contact resistance, and dark areas seen in electroluminescence (EL) imaging, so it is imperative to develop new metallization pastes that are more resistant to acetic acid. The introduction of Ti can improve the acetic acid performance of glass. This application adjusts the low solubility of the electrode grid in acetic acid through the secondary glass (Pb-Ti-Si-B series glass), improves the good chemical stability of the electrode, and resists acetic acid corrosion, aiming to achieve high temperature and high humidity resistance of the electrode grid and provide component reliability.

[0007] Optionally, the elements in the modifying additive include one or more of W, Ca, Mg, Zn, Pb, Ba, Y, Li, Na, K and Zr, and the modifying additive is a compound.

[0008] Optionally, the main glass powder is a Pb-Si-B system glass, and based on the total molar percentage content of the main glass powder being 100%, the main glass powder includes SiO 2 15%~40%, B 2 O 3 18%~40%,Al 2 O 3 0%~20%, PbO and BaO total 15%~45%, modifying additives 1%~20%.

[0009] Optionally, based on the total molar percentage content of the auxiliary glass powder being 100%, the Bi 2 O 3 10%~49.3%,TeO 2 0%~25%,SiO 2 8%~29.5%,GeO 2 0%~7%; taking the total molar percentage content of the main glass powder as 100%, in the main glass powder, PbO13%~42%, BaO0%~7%.

[0010] Optionally, the elements in the modifying additive include one or more of W, Ca, Mg, Se, Ag, Zn, P, Ga, Li, Na, K and Fe, and the modifying additive is a compound.

[0011] Optionally, the slurry further comprises silver powder and an organic carrier. In the slurry, the mass fraction of the silver powder is 83% to 90%, and the mass fraction of the organic carrier is 8% to 15%.

[0012] Optionally, the organic carrier comprises an organic solvent, an organic resin and an additive, wherein the mass fraction of the organic solvent in the organic carrier is 60% to 90%, the mass fraction of the organic resin is 5% to 20%, and the mass fraction of the additive is 5% to 20%.

[0013] Optionally, the glass powder includes a main glass powder and a secondary glass powder, and the preparation method of the glass powder includes:

[0014] The raw materials of various components are uniformly mixed, heated until melted, and cooled to obtain glass frit;

[0015] The glass material is ground and sieved to obtain glass powder.

[0016] Optionally, the preparation method specifically comprises:

[0017] The raw materials of various components are uniformly mixed, loaded into a platinum crucible, melted at 900-1300°C for 30-90 minutes, and then cooled to obtain glass material;

[0018] The glass material is ground and screened to obtain glass powder, and the glass powder has a D100 of less than or equal to 6 um.

[0019] Optionally, the slurry is applied to an N-type solar cell processed by a laser enhanced contact optimization process.

[0020] The present application also provides a photovoltaic module, which includes a first cover plate, a first adhesive film, a battery string, a second adhesive film and a second cover plate which are stacked, wherein the first adhesive film and the second adhesive film are EVA; the battery string includes a plurality of electrically connected solar cells, and the electrodes of the solar cells are formed by applying any of the high temperature and acetic acid resistant conductive pastes described above.

[0021] The present application provides a high temperature resistant and acetic acid resistant conductive paste and a photovoltaic module. The paste includes a main glass powder and a secondary glass powder. The mass fraction of the main glass powder in the paste is 1.5% to 2.5%, the mass fraction of the secondary glass powder is 0.2% to 1%, the secondary glass powder is Bi-Si-B-Al glass, and the total molar percentage content of the secondary glass powder is 100%. The secondary glass powder includes Bi 2 O 3 and TeO 2 Total 10% to 50%, SiO 2 and GeO 2 Total 15% to 30%, B 2 O 3 18%~30%,Al 2 O 30% to 20% and modified additives 1% to 20%. The slurry also includes silver powder and an organic carrier. In the slurry, the mass fraction of the silver powder is 83% to 90%, and the mass fraction of the organic carrier is 8% to 15%. The slurry in the present application adjusts the low solubility of the electrode grid in acetic acid through the auxiliary glass to solve the problem that the acetic acid produced by the decomposition of EVA under high temperature conditions affects the battery efficiency of the double-sided EVA component packaging battery. The present application also provides a photovoltaic component using the above slurry. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] In order to more clearly illustrate the technical solution of the present application, the drawings required for use in the embodiments are briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without any creative work.

[0023] Figure 1 This is the EL image of B1 cell in acetic acid atmosphere;

[0024] Figure 2 This is the EL image of the B1 cell in acetic acid atmosphere;

[0025] Figure 3 This is the EL image of A2 cell in acetic acid atmosphere;

[0026] Figure 4 This is the EL image of the A2 cell in acetic acid atmosphere. DETAILED DESCRIPTION

[0027] The following embodiments are described in detail, and examples thereof are shown in the accompanying drawings. When the following description refers to the drawings, unless otherwise indicated, the same numbers in different drawings represent the same or similar elements. The implementations described in the following embodiments do not represent all implementations consistent with the present application. They are only examples of systems and methods consistent with some aspects of the present application as detailed in the claims.

[0028] In order to solve the problem that the acetic acid produced by the decomposition of EVA under high temperature conditions affects the efficiency of the battery in the double-sided EVA component packaging battery, the present application provides a high temperature and acetic acid resistant conductive paste and photovoltaic component. The paste includes a main glass powder and a secondary glass powder. The mass fraction of the main glass powder in the paste is 1.5% to 2.5%, and the mass fraction of the secondary glass powder is 0.2% to 1%. The secondary glass powder is Bi-Si-B-Al glass. The total molar percentage content of the secondary glass powder is 100%. The secondary glass powder includes Bi 2 O 3 and TeO 2 Total 10% to 50%, SiO 2 and GeO 2Total 15% to 30%, B 2 O 3 18%~30%,Al 2 O 3 0%~20% and modified additives 1%~20%.

[0029] EVA acts as an air and electrical insulator in the component, protecting it from mechanical damage and preventing corrosion from the external environment. However, under the action of photosynthetic heat, acetic acid is a decomposition product of the module packaging material ethylene-vinyl acetate (EVA). Acetic acid solution basically does not corrode pure aluminum at room temperature, but as the temperature rises, the corrosion rate accelerates. The corrosion rate of 1% dilute acetic acid solution on aluminum at boiling temperature is 100 times that of room temperature; the corrosion rate of acetic acid on aluminum is also related to the purity of aluminum. Low-purity aluminum, such as aluminum containing impurities such as iron, silicon, and aluminum salts on the surface, forms a loose and dense oxide protective film, and has low corrosion resistance.

[0030] The minority carrier lifetime of solar cells is also increasing, that is, the diffusion length of minority carriers is growing. When the diffusion length of minority carriers is equal to or exceeds the thickness of silicon wafers, the recombination rate of the back surface has a significant impact on the characteristics of solar cells. After sintering, the back field forms a silicon-aluminum alloy. Aluminum is doped as a P-type in silicon, which can reduce the minority carrier recombination at the junction of metal and silicon, thereby increasing the open circuit voltage and short circuit current. The quality of the aluminum back field directly affects the output characteristics of solar cells.

[0031] After soaking the solder strip at 60°C for one week in a dilute acetic acid solution, the main grid line on the front of the cell turned yellow, the grid line on the back of the cell turned black, and the aluminum back field on the back of the cell fell off. The acetic acid produced by EVA will cause electrochemical corrosion of the tin-coated copper solder strip, corrode and oxidize the silver grid line on the surface of the cell to make it black, and corrode the aluminum back field of the cell while reducing the adhesion between the aluminum back field and the silicon wafer, seriously affecting the electrical performance of the battery. This will in turn reduce the electrical performance of the module. Therefore, in the future development of photovoltaic modules, it is necessary to study new packaging materials, new EVA formulations, or other measures to reduce the generation of acetic acid by EVA aging, so as to protect the battery from the harm of acetic acid and have a longer life.

[0032] More importantly, acetic acid interacts with metallization, often causing degradation of the interface between the front metal contact and the underlying silicon (Si) substrate. This leads to loss of cell performance and contact adhesion, increased contact resistance, and dark areas seen in electroluminescence (EL) imaging, so it is imperative to develop new pastes that are more resistant to acetic acid.

[0033] The introduction of Ti can improve the acetic acid performance of glass. The present application adjusts the low solubility of the electrode grid in acetic acid through the secondary glass (Pb-Ti-Si-B glass), improves the good chemical stability of the electrode, and resists acetic acid corrosion.

[0034] In some embodiments, the elements in the modifying additive include one or more of W, Ca, Mg, Zn, Pb, Ba, Y, Li, Na, K and Zr, and the modifying additive is a compound.

[0035] In some embodiments, the main glass powder is a Pb-Si-B glass. Taking the total molar percentage of the main glass powder as 100%, the main glass powder includes SiO 2 15%~40%, B 2 O 3 18%~40%,Al 2 O 3 0%~20%, PbO and BaO total 15%~45%, modifying additives 1%~20%.

[0036] In some embodiments, based on the total molar percentage content of the auxiliary glass powder as 100%, Bi in the auxiliary glass powder 2 O 3 10%~49.3%,TeO 2 0%~25%,SiO 2 8%~29.5%,GeO 2 0%~7%; taking the total molar percentage content of the main glass powder as 100%, in the main glass powder, PbO13%~42%, BaO0%~7%.

[0037] In some embodiments, the elements in the modifying additive include one or more of W, Ca, Mg, Se, Ag, Zn, P, Ga, Li, Na, K and Fe, and the modifying additive is a compound.

[0038] In some embodiments, the slurry further comprises silver powder and an organic vehicle. In the slurry, the mass fraction of the silver powder is 83% to 90%, and the mass fraction of the organic vehicle is 8% to 15%.

[0039] In some embodiments, the silver powder is spherical silver powder, and the D50 of the silver powder is 1.4-2.0um. D50 refers to the particle size corresponding to when the cumulative particle size distribution percentage of a sample reaches 50%. Its physical meaning is that particles with a particle size larger than it account for 50%, and particles with a particle size smaller than it also account for 50%. D50 is also called the median diameter or median particle size.

[0040] In some embodiments, the organic vehicle comprises an organic solvent, an organic resin and an additive, wherein the mass fraction of the organic solvent in the organic vehicle is 60% to 90%, the mass fraction of the organic resin is 5% to 20%, and the mass fraction of the additive is 5% to 20%.

[0041] In some embodiments, the glass powder includes a main glass powder and a secondary glass powder, and the preparation method of the glass powder includes:

[0042] The raw materials of various components are uniformly mixed, heated until melted, and cooled to obtain glass frit;

[0043] The glass material is ground and sieved to obtain glass powder.

[0044] In some embodiments, the preparation method specifically comprises:

[0045] The raw materials of various components are uniformly mixed, put into a platinum crucible, melted at 900-1300°C for 30-90 minutes, and then cooled to obtain glass material;

[0046] The glass material is ground and screened to obtain glass powder, and the glass powder has a D100 of less than or equal to 6 um.

[0047] In some embodiments, the slurry is applied to an N-type solar cell processed by a laser enhanced contact optimization process.

[0048] The present application also provides a photovoltaic module, which includes a first cover plate, a first adhesive film, a battery string, a second adhesive film and a second cover plate which are stacked, wherein the first adhesive film and the second adhesive film are EVA; the battery string includes a plurality of electrically connected solar cells, and the electrodes of the solar cells are formed by applying any of the high temperature and acetic acid resistant conductive pastes described above.

[0049] In some embodiments, solar cells include, but are not limited to, PERC cells (Passivated Emitter Rear Cell), IBC (Interdigitated Back Contact), TOPCon (Tunnel Oxide Passivated Contact), HIT / HJT (Heterojunction Technology) cells, solar thin-film cells, and stacked cells, or any combination thereof. Among them, solar thin-film cells include, but are not limited to, perovskite solar thin-film cells, copper indium selenide solar thin-film cells, gallium arsenide solar thin-film cells, and cadmium sulfide solar thin-film cells. Stacked cells include, but are not limited to, perovskite cells superimposed on crystalline silicon cells, perovskite cells superimposed on perovskite cells, and perovskite cells superimposed on thin-film cells.

[0050] Example:

[0051] The auxiliary glass powders GH001 to GH007 are prepared according to the material ratios in Table 1, and the main glass powders BL001 to BL005 are prepared according to the material ratios in Table 2. The material ratios of the glass powders in Tables 1 and 2 are all expressed in molar percentages. For example, in the auxiliary glass powder GH001, Bi 2 O 3 49.3 mol%SiO 2 28.5mol%B 2 O 3 18 mol%Al 2 O 3 3mol%CaO1mol%Y 2 O 3 0.2mol%.

[0052] Each component material is weighed by weight in mole percentage and mixed in a mixer; the material is put into a platinum crucible and melted at 900-1300°C using a lifting furnace for 30-90 minutes. After the glass state is homogenized, the glass material is obtained by molten water quenching or cold rolling; after the glass material is ground and sieved, the secondary glass GH001-GH007 and the main glass powder BL001-BL005 are obtained, and the glass powder D100 is ≤6um.

[0053] Among them, GH001~GH004, BL001~BL002 are melted at 1000℃ and kept warm for 60min; GH005 and BL003 are melted at 900℃ and kept warm for 30min; GH006, GH007, BL004 and BL005 are melted at 1300℃ and kept warm for 90min.

[0054] Table 1 Material ratio of auxiliary glass powder

[0055] raw material GH001 GH002 GH003 GH004 GH005 GH006 GH007 <![CDATA[TeO 2 ]]> 0 5 0 10 25 12 0 <![CDATA[Bi 2 THE 3 ]]> 49.3 15 33 30 10 38 10 <![CDATA[SiO 2 ]]> 28.5 29.5 20 18 12 8 29.5 <![CDATA[GeO 2 ]]> 0 0.5 0 2 3 7 0.5 <![CDATA[B 2 THE 3 ]]> 18 28 25 22 30 18 30 PbO 0 0 5 4.5 2 0.5 3 ZnO 0 0 2 1 3 0.5 2 <![CDATA[Al 2 THE 3 ]]> 3 18 13 10 0 16 20 <![CDATA[Li 2 CO 3 ]]> 0 1 0 1 2 0 1 <![CDATA[WO 3 ]]> 0 0 0 0.5 3 0 0.5 <![CDATA[Na 2 CO 3 ]]> 0 0 0 0.2 0 0 2 <![CDATA[K 2 CO 3 ]]> 0 0.5 0 0 2 0 0 BaO 0 2.5 0 0 8 0 1 MgO 0 0 0 0.6 0 0 0.5 CaO 1 0 2 0 0 0 0 <![CDATA[ZrO 2 ]]> 0 0 0 0.2 0 0 0 <![CDATA[Y 2 THE 3 ]]> 0.2 0 0 0 0 0 0

[0056] Table 2 Main glass powder material ratio

[0057] raw material BL001 BL002 BL003 BL004 BL005 PbO 30.4 42 13 40 21 BaO 2 0 2 5 7 <![CDATA[SiO 2 ]]> 24 20 40 15 17 <![CDATA[B 2 THE 3 ]]> 32 25 40 19 18 <![CDATA[Al 2 THE 3 ]]> 1.5 7 0 20 17 ZnO 3 4.5 1 0.5 1 <![CDATA[P 2 THE 5 ]]> 0 0.3 1 0 2 <![CDATA[Fe 2 THE 3 ]]> 3 0 0.5 0 0 <![CDATA[Ga 2 THE 3 ]]> 1 0 0 0.5 2 <![CDATA[Li 2 CO 3 ]]> 1.2 0 0 0 1 <![CDATA[Na 2 CO 3 ]]> 0.2 0 0 0 1 <![CDATA[K 2 CO 3 ]]> 0 0.2 0.5 0 2.5 MgO 0 0.5 0 0 3 CaO 0 0.5 1 0 3 <![CDATA[Ag 2 The]]> 0.2 0 0 0 1.5 <![CDATA[SeO 2 ]]> 1.5 0 1 0 3

[0058] Embodiment 1:

[0059] Weigh 88.5wt% silver powder, 9wt% organic carrier, 2.0wt% glass powder BL001, and 0.5wt% glass powder GH001. The organic carrier includes 75wt% organic solvent, 15wt% organic resin, and 10wt% additive. Premix the silver powder and organic with a planetary mixer, grind the slurry 6 times with a ceramic three-roll grinder, test the grinding fineness with a scraper fineness meter, the slurry fineness is <10um, and filter with a 250-mesh filter cloth to obtain the front electrode silver paste A1.

[0060] Embodiment 2:

[0061] Weigh 85.7wt% silver powder, 12wt% organic carrier, 1.8wt% glass powder BL002, and 0.8wt% glass powder GH002. The organic carrier includes 75wt% organic solvent, 15wt% organic resin, and 10wt% additive. Premix the silver powder and organic with a planetary mixer, grind the slurry 6 times with a ceramic three-roll grinder, test the grinding fineness with a scraper fineness meter, the slurry fineness is <10um, and filter with a 250-mesh filter cloth to obtain the front electrode silver paste A2.

[0062] Embodiment three:

[0063] Weigh 87.4wt% silver powder, 10wt% organic carrier, 2.2wt% glass powder BL002, and 0.4wt% glass powder GH003. The organic carrier includes 75wt% organic solvent, 15wt% organic resin, and 10wt% additive. Premix the silver powder and organic with a planetary mixer, grind the slurry 6 times with a ceramic three-roll grinder, test the grinding fineness with a scraper fineness meter, the slurry fineness is less than 10um, and filter with a 250-mesh filter cloth to obtain the front electrode silver paste A3.

[0064] Embodiment 4:

[0065] Weigh 88.8wt% silver powder, 9wt% organic carrier, 1.9wt% glass powder BL002, and 0.3wt% glass powder GH004. The organic carrier includes 75wt% organic solvent, 15wt% organic resin, and 10wt% additive. Premix the silver powder and organic with a planetary mixer, grind the slurry 6 times with a ceramic three-roll grinder, test the grinding fineness with a scraper fineness meter, the slurry fineness is less than 10um, and filter with a 250-mesh filter cloth to obtain the front electrode silver paste A4.

[0066] Embodiment five:

[0067] Weigh 90wt% silver powder, 8wt% organic carrier, 1.5wt% glass powder BL003, and 0.5wt% glass powder GH005. The organic carrier includes 60wt% organic solvent, 20wt% organic resin, and 20wt% additive. The D50 of the silver powder is 2.0μ. Premix the silver powder and organic with a planetary mixer, grind the slurry 6 times with a ceramic three-roll grinder, test the grinding fineness with a scraper fineness meter, the slurry fineness is <10um, and filter with a 250-mesh filter cloth to obtain the front electrode silver paste A5.

[0068] Embodiment six:

[0069] Weigh 87.3wt% silver powder, 10wt% organic carrier, 2.5wt% glass powder BL004, and 0.2wt% glass powder GH006. The organic carrier includes 90wt% organic solvent, 5wt% organic resin, and 5wt% additive. The D50 of the silver powder is 1.7μ. Premix the silver powder and organic with a planetary mixer, grind the slurry 6 times with a ceramic three-roll grinder, test the grinding fineness with a scraper fineness meter, the slurry fineness is <10um, and filter with a 250-mesh filter cloth to obtain the front electrode silver paste A6.

[0070] Embodiment seven:

[0071] Weigh 83wt% silver powder, 15wt% organic carrier, 1wt% glass powder BL005, and 1wt% glass powder GH007. The organic carrier includes 90wt% organic solvent, 5wt% organic resin, and 5wt% additive. The D50 of the silver powder is 1.4μ. The D50 of the silver powder is 1.7μ. Premix the silver powder and the organic with a planetary mixer, grind the slurry 6 times with a ceramic three-roll grinder, test the grinding fineness with a scraper fineness meter, the slurry fineness is <10um, filter with a 250-mesh filter cloth to obtain the front electrode silver paste A7.

[0072] Comparative Example 1:

[0073] Weigh 89wt% silver powder, 9wt% organic carrier, and 2.0wt% glass powder BL001. The organic carrier includes 75wt% organic solvent, 15wt% organic resin, and 10wt% additive. Premix the silver powder and organic with a planetary mixer, grind the slurry 6 times with a ceramic three-roll grinder, test the grinding fineness with a scraper fineness meter, the slurry fineness is <10um, and filter with a 250-mesh filter cloth to obtain the front electrode silver paste B1.

[0074] Comparative Example 2:

[0075] Weigh 89wt% silver powder, 9wt% organic carrier, and 2.0wt% glass powder BL002. The organic carrier includes 75wt% organic solvent, 15wt% organic resin, and 10wt% additive. Premix the silver powder and organic with a planetary mixer, grind the slurry 6 times with a ceramic three-roll grinder, test the grinding fineness with a scraper fineness meter, the slurry fineness is less than 10um, and filter with a 250-mesh filter cloth to obtain the front electrode silver paste B2.

[0076] The slurries prepared in Examples 1-7 and Comparative Examples 1-2 were printed on N-type 182 silicon wafers using a Maiwei automatic printer, 100 wafers were printed with each slurry, sintered in a sintering furnace, and then processed by laser-enhanced contact optimization (LECO), and the cell IV test was performed to record the data.

[0077] Acetic acid test conditions:

[0078] 1) Place the cells to be corroded into a basket of corresponding size in a spacer-by-spacer manner; place two companion cells at the edge of the basket;

[0079] 2) Prepare acetic acid solution as required and pour it into a PP fresh-keeping box; then put the flower basket in the center of the fresh-keeping box, cover the box with the lid, buckle the buckle, and seal it with plastic film;

[0080] 3) Place the prepared acetic acid box in an 85℃ oven, keep it warm for 8 hours, then take out the battery cell for testing

[0081] Formula: Eta attenuation value = (1-Eta after acetic acid / Eta before acetic acid) × 100%.

[0082] The experimental temperature, test time and acetic acid solution preparation method are shown in Table 3, and the measurement data are shown in Table 4.

[0083] Table 3 Acetic acid test experimental conditions

[0084]

[0085] "With fan" in Table 3 means that a fan is installed in the acetic acid box container to make the atmosphere concentration in the acetic acid box container uniform; "test time 8 hours" means that the battery cells are kept in the acetic acid box container for 8 hours.

[0086] Table 4 Experimental measurement data

[0087]

[0088] like Figure 1 The EL image of B1 cell in acetic acid atmosphere is shown as follows: Figure 2 The following is the EL image of the B1 cell in acetic acid atmosphere. Figure 3 The EL image of A2 cell in acetic acid atmosphere is shown as follows: Figure 4 The following is the EL image of A2 cell in acetic acid atmosphere. Figure 1-Figure 4 As shown, before acetic acid, the EL of the embodiment and the comparative example are roughly equivalent. After acetic acid, the EL dark spots of the comparative example due to the acetic acid atmosphere are deeper and more than those of the embodiment.

[0089] As shown in Table 4, Uoc is the open circuit voltage, FF is the fill factor, and Eta is the photoelectric conversion efficiency. The cell prepared by the slurry provided in the present application, after being placed in an acetic acid atmosphere, not only does the change in the open circuit voltage and fill factor of the cell be smaller, but also the attenuation value of the photoelectric conversion efficiency of the cell be smaller, and the photoelectric conversion efficiency of the cell after being placed in an acetic acid atmosphere remains above 20%. It can be seen that the slurry provided in the present application is more resistant to acetic acid.

[0090] The present application provides a high temperature resistant and acetic acid resistant conductive paste and a photovoltaic module. The paste includes a main glass powder and a secondary glass powder. The mass fraction of the main glass powder in the paste is 1.5% to 2.5%, the mass fraction of the secondary glass powder is 0.2% to 1%, the secondary glass powder is Bi-Si-B-Al glass, and the total molar percentage content of the secondary glass powder is 100%. The secondary glass powder includes Bi 2 O 3 and TeO 2 Total 10% to 50%, SiO 2 and GeO 2 Total 15% to 30%, B 2 O 3 18%~30%,Al 2 O 30% to 20% and modified additives 1% to 20%. The slurry also includes silver powder and an organic carrier. In the slurry, the mass fraction of the silver powder is 83% to 90%, and the mass fraction of the organic carrier is 8% to 15%. The slurry in the present application adjusts the low solubility of the electrode grid in acetic acid through the auxiliary glass to solve the problem that the acetic acid produced by the decomposition of EVA under high temperature conditions affects the battery efficiency of the double-sided EVA component packaging battery. The present application also provides a photovoltaic component using the above slurry.

[0091] Similar parts between the embodiments provided in this application can be referenced to each other. The specific implementation methods provided above are only a few examples under the general concept of this application and do not constitute a limitation on the protection scope of this application. For those skilled in the art, any other implementation methods expanded based on the scheme of this application without creative work belong to the protection scope of this application.

Claims

1. A high temperature and acetic acid resistant conductive paste, characterized in that: The slurry includes a main glass powder and a secondary glass powder. In the slurry, the mass fraction of the main glass powder is 1.5% to 2.5%, the mass fraction of the secondary glass powder is 0.2% to 1%, the secondary glass powder is Bi-Si-B-Al glass, and based on the total molar percentage content of the secondary glass powder as 100%, the secondary glass powder includes Bi2O3 and TeO2 totaling 10% to 50%, SiO2 and GeO2 totaling 15% to 30%, B2O3 18% to 30%, Al2O3 0% to 20% and modified additives 1% to 20%.

2. The high temperature resistant and acetic acid resistant conductive paste according to claim 1, characterized in that: The elements in the modifying additive include one or more of W, Ca, Mg, Zn, Pb, Ba, Y, Li, Na, K and Zr, and the modifying additive is a compound.

3. The high temperature and acetic acid resistant conductive paste according to claim 1, characterized in that: The main glass powder is Pb-Si-B glass. Taking the total molar percentage content of the main glass powder as 100%, the main glass powder includes SiO2 15% to 40%, B2O3 18% to 40%, Al2O 30% to 20%, PbO and BaO totaling 15% to 45%, and modified additives 1% to 20%.

4. The high temperature and acetic acid resistant conductive paste according to claim 3, characterized in that: Taking the total molar percentage content of the auxiliary glass powder as 100%, the auxiliary glass powder contains 10% to 49.3% Bi2O3, 20% to 25% TeO, 8% to 29.5% SiO2, and 20% to 7% GeO; taking the total molar percentage content of the main glass powder as 100%, the main glass powder contains 13% to 42% PbO, and 0% to 7% BaO.

5. The high temperature and acetic acid resistant conductive paste according to claim 4, characterized in that: The elements in the modifying additive include one or more of W, Ca, Mg, Se, Ag, Zn, P, Ga, Li, Na, K and Fe, and the modifying additive is a compound.

6. The high temperature and acetic acid resistant conductive paste according to claim 5, characterized in that: The slurry further comprises silver powder and an organic carrier. In the slurry, the mass fraction of the silver powder is 83% to 90%, and the mass fraction of the organic carrier is 8% to 15%.

7. The high temperature and acetic acid resistant conductive paste according to claim 6, characterized in that: The organic carrier comprises an organic solvent, an organic resin and an additive. In the organic carrier, the mass fraction of the organic solvent is 60% to 90%, the mass fraction of the organic resin is 5% to 20%, and the mass fraction of the additive is 5% to 20%.

8. The high temperature and acetic acid resistant conductive paste according to claim 1, characterized in that: The glass powder includes a main glass powder and a secondary glass powder, and the preparation method of the glass powder includes: The raw materials of various components are uniformly mixed, heated until melted, and cooled to obtain glass frit; The glass material is ground and sieved to obtain glass powder.

9. The high temperature and acetic acid resistant conductive paste according to claim 8, characterized in that: The preparation method specifically comprises: The raw materials of various components are uniformly mixed, loaded into a platinum crucible, melted at 900-1300°C for 30-90 minutes, and then cooled to obtain glass material; The glass material is ground and screened to obtain glass powder, and the glass powder has a D100 of less than or equal to 6 um.

10. A photovoltaic module, characterized in that: The photovoltaic module includes a first cover plate, a first adhesive film, a battery string, a second adhesive film and a second cover plate which are stacked, and the first adhesive film and the second adhesive film are EVA; the battery string includes a plurality of electrically connected solar cells, and the electrodes of the solar cells are formed by applying the high temperature and acetic acid resistant conductive paste described in any one of claims 1 to 9.

Citation Information

Patent Citations

  • Glass paste for conductive silver paste, conductive silver paste and preparation method thereof, and solar cell

    CN114944238A

  • Conductive silver aluminum paste, preparation method, electrode and N-type Topcon battery

    CN116759133A

  • Conductive silver aluminum paste, preparation method, electrode and cell

    US11756699B1

  • Conductive paste for solar cell electrode

    US20100126565A1

Cited By

  • Acetic acid-resistant glass powder for front silver paste of TOPCon cell

    CN119285240A