Electrochemical device and electronic device

By using a combination of lithium-containing transition metal composite oxide and specific compounds in a nonaqueous electrolyte in an electrochemical device, the balance problem between high-temperature performance and low-temperature discharge performance is solved, and excellent high-temperature storage and low-temperature discharge performance are achieved.

CN119069807AActive Publication Date: 2024-12-03NINGDE AMPEREX TECHNOLOGY LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411209671.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-12-03
Estimated Expiration
2044-08-30

AI Technical Summary

Technical Problem

While improving high-temperature performance, existing electrochemical devices often lead to deterioration of low-temperature discharge performance, making it difficult to find a balance between the two.

Method used

LixNazCo1-yMyO2 is used as the cathode material, and specific compounds, such as compounds of formula I, dinitrile substances and trinitrile substances, are added to the nonaqueous electrolyte. By regulating the content and proportion of these compounds, Form a high-stability inorganic rich protective layer to promote the interface transmission of lithium ions, improve low-temperature discharge performance, and maintain high-temperature storage performance.

Benefits of technology

Without affecting the high-temperature storage performance, the low-temperature discharge performance and cycling performance of the electrochemical device are significantly improved, and the stability of the cathode material layer is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069807A_ABST
    Figure CN119069807A_ABST
Patent Text Reader

Abstract

The invention discloses an electrochemical device and an electronic device. An electrochemical device includes a positive electrode including a positive electrode material layer disposed on at least one surface of a positive electrode current collector, the positive electrode material layer including a lithium-containing transition metal composite oxide including LixNazCo1-yMyO2 wherein 0.6 < x < 0.95, 0 < = y < 0.15, 0 < z < = 0.03, M being at least one selected from the group consisting of Al, Mg, Ti, Mn, Fe, Ni, Zn, Cu, Nb, Cr, and Zr, and a non-aqueous electrolyte solution disposed on at least one surface of the positive electrode current collector, the non-aqueous electrolyte comprises a compound shown as a formula I, the mass percentage content of the compound shown as the formula I is A%, and A / z is greater than or equal to 1 and less than or equal to 200. The electrochemical device provided by the invention shows relatively excellent electrochemical performance, especially relatively excellent high-temperature storage performance and low-temperature discharge performance. # imgabs0 #
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of energy storage technology, and in particular to an electrochemical device and an electronic device. Background Art

[0002] As people's demand for electronic products such as mobile phones, laptops, and cameras increases year by year, electrochemical devices play an increasingly important role in our daily lives as power sources for electronic products, thus driving the demand for improved performance of electrochemical devices in a variety of scenarios. Existing technical means often lead to the degradation of low-temperature discharge performance of electrochemical devices while improving the high-temperature performance of electrochemical devices. Therefore, it is imperative to provide electrochemical devices with good high-temperature performance and low-temperature discharge performance. Summary of the invention

[0003] The embodiments of the present application provide an electrochemical device and an electronic device, which achieve better high-temperature storage performance while improving low-temperature discharge performance and cycle performance.

[0004] In a first aspect, an embodiment of the present application provides an electrochemical device, including a positive electrode and a non-aqueous electrolyte, wherein the positive electrode includes a positive electrode material layer disposed on at least one surface of a positive electrode current collector, wherein the positive electrode material layer includes a lithium-containing transition metal composite oxide, wherein the lithium-containing transition metal composite oxide includes Li x Na z Co 1-y M y O2, wherein 0.6<x<0.95, 0≤y<0.15, 0<z≤0.03, M is at least one selected from the group consisting of Al, Mg, Ti, Mn, Fe, Ni, Zn, Cu, Nb, Cr and Zr; the non-aqueous electrolyte comprises a compound of formula I:

[0005] Compounds;

[0006] wherein R is selected from C2 to C6 alkyl which is unsubstituted or substituted by Ra, C2 to C6 alkenyl which is unsubstituted or substituted by Ra, C2 to C6 alkynyl which is unsubstituted or substituted by Ra, C5 to C6 alkyl which is unsubstituted or substituted by Ra, 12 A nitrogen-containing heteroaryl group, a C6 to C 12 The substituent Ra of each group is independently selected from fluorine or C1 to C6 fluoroalkyl. Wherein, based on the total mass of the non-aqueous electrolyte, the mass percentage of the compound of formula I is A%, 1≤A / z≤200.

[0007] Based on the electrochemical device of the embodiment of the present application, the inventors found that when the positive electrode material layer includes a lithium-containing transition metal composite oxide Li x Naz Co 1-y M y O2, wherein the M element is selected from at least one of Al, Mg, Ti, Mn, Fe, Ni, Zn, Cu, Nb, Cr and Zr, and the compound of formula I is added to the non-aqueous electrolyte in the electrochemical device, and the mass percentage A of the compound of formula I in the non-aqueous electrolyte is controlled to be equal to the mass percentage A of the lithium-containing transition metal composite oxide Li x Na z Co 1-y M y The value z of the Na atomic ratio in O2 satisfies the above range, which enables the lone pair of electrons in the sulfone functional group of the compound of formula I to specifically bind to the lithium-containing transition metal composite oxide Li x Na z Co 1-y M y The cobalt atoms and M atoms on O2 form a highly stable inorganic protective thin layer containing fluoride and sulfonic acid / sulfate during the battery formation process, thereby reducing the interfacial impedance without affecting the high-temperature storage performance, promoting the interfacial transmission of lithium ions at low temperatures, improving the low-temperature discharge performance of the electrochemical device, and also helping to improve the stability of the positive electrode material layer under high temperature conditions, so that the electrochemical device has excellent high-temperature storage performance.

[0008] In some of the embodiments, for the mass percentage A% of the compound of formula I in the electrochemical device and the lithium-containing transition metal composite oxide Li x Na z Co 1-y M y The content z of Na in O2 satisfies at least one of the following conditions: (1) 5≤A / z≤100; (2) 0.1≤A≤5; (3) 0.005≤z≤0.02. Based on the above embodiment, by adjusting the mass percentage A% of the compound of formula I and the content z of Na in the lithium-containing transition metal composite oxide to satisfy any of the above conditions, the lithium-containing transition metal composite oxide can better cooperate with the compound of formula I in the electrolyte, and the sulfone functional group in the compound of formula I can more completely react with the lithium transition metal composite oxide Li x Na z Co 1-y M y The cobalt atoms on O2 combine with the M atoms, thereby further improving the high-temperature storage performance and low-temperature discharge performance of the electrochemical device.

[0009] In some embodiments, the compound of formula I comprises at least one of the following compounds:

[0010]

[0011] Based on the above embodiments, by selecting the above-mentioned type of compound of formula I, the R group in its structure can better promote the sulfone functional group and the lithium transition metal composite oxide Li x Na z Co 1-y M y The cobalt atoms on O2 combine with the M atoms to improve both the high-temperature storage performance and the low-temperature discharge performance of the electrochemical device.

[0012] In some embodiments, the non-aqueous electrolyte further comprises a dinitrile substance as shown in the compound of formula II and a trinitrile substance as shown in the compound of formula III:

[0013] Compounds,

[0014] Wherein, R0 is selected from C2 to C 10 Chain alkylene, C2 to C 10 Alkenylene or -R a -(OR b ) n -R c -, R a , R b and R c Each is independently selected from C1 to C3 alkylene or C2 to C3 alkenylene, and n is an integer from 1 to 3;

[0015] Compounds,

[0016] Among them, R 11 , R 12 and R 13 are each independently selected from C1 to C3 alkylene or -R A -(OR B ) n -R C -, R A , R B and R C are each independently selected from a single bond, a C1 to C2 alkylene group, n is an integer from 1 to 3, R 21 Selected from hydrogen atoms, C1 to C3 alkylene groups; based on the total mass of the non-aqueous electrolyte, the mass percentage of the compound of formula II is B%, the mass percentage of the compound of formula III is C%, and 0.05≤A / (B+C)≤50. Based on the above embodiments, the electrochemical device of the present application further adds a certain amount of dinitrile substances and trinitrile substances to the electrolyte. Among them, when controlling to meet 0.05≤A / (B+C)≤50, the nitrile molecules in the dinitrile substances and trinitrile substances can be combined with the lithium transition metal composite oxide Li in the positive electrode material layer. x Na z Co1-y The cobalt atoms of MyO2 form a cyanide-rich antioxidant covering layer, and the combination of dinitriles and trinitriles can also improve the surface coverage, fully passivate the material interface, and effectively block the electrolyte molecules from reaching the interface to undergo continuous oxidation reactions, thereby further improving the high-temperature storage performance and low-temperature discharge performance of the electrochemical device.

[0017] In some of the embodiments, the mass percentage content A% of the compound of formula I, the mass percentage content B% of the compound of formula II and the mass percentage content C% of the compound of formula III in the electrochemical device meet at least one of the following conditions: (1) 0.5≤B+C≤8; (2) 0.1≤A / (B+C)≤2; (3) 0.1≤B≤6; (4) 0.1≤C≤6. Based on the above embodiments, the electrochemical device of the present application adjusts the content parameters of the mass percentage content A% of the compound of formula I, the mass percentage content B% of the compound of formula II and the mass percentage content C% of the compound of formula III within the above range, so that the content of each compound, especially the content ratio of dinitrile substances and trinitrile substances, is within a suitable range, which is more conducive to the synergistic effect of dinitrile substances and trinitrile substances, further improves the surface coverage, and more fully passivates the material interface, thereby further improving the high temperature storage performance and low temperature discharge performance of the electrochemical device.

[0018] In some embodiments, the compound of formula II is selected from at least one of succinonitrile, glutaronitrile, methylglutaronitrile, adiponitrile, pimelonitrile, suberonitrile, fumaronitrile or 1,2-bis(cyanoethoxy)ethane.

[0019] In some embodiments, the compound of formula III is selected from at least one of 1,3,5-pentane trinitrile, 1,3,6-hexane trinitrile or 1,2,3-tri(2-cyanoethoxy)propane. The use of the compound of formula II and / or formula III can enhance the bonding between the nitrile molecules and the lithium transition metal composite oxide Li in the positive electrode material layer. x Na z Co 1-y M y The binding efficiency of cobalt atoms in O2 is improved, the surface coverage of the cyanide-rich antioxidant covering layer is increased, and the material interface is more fully passivated, thereby further improving the high-temperature storage performance and low-temperature discharge performance of the electrochemical device.

[0020] In some embodiments, the non-aqueous electrolyte further comprises a cyclic carbonate, which is selected from at least two of ethylene carbonate, propylene carbonate or fluoroethylene carbonate; based on the total mass of the non-aqueous electrolyte, the mass percentage of the cyclic carbonate is 1% to 30%. Preferably, the mass percentage of the cyclic carbonate is 2% to 15%. Based on the above embodiments, the above cyclic carbonate is selected in the electrolyte, and the content of the cyclic carbonate is regulated within the above range, which can further improve the high temperature storage performance, while further taking into account the improvement of the low temperature discharge performance of the electrochemical device.

[0021] In some embodiments, the non-aqueous electrolyte further comprises a linear ester, and the linear ester comprises a fluorinated linear ester and a non-fluorinated linear ester. The linear ester satisfies at least one of the following conditions: (1) the fluorinated linear ester is selected from at least one of methyl difluoroethyl carbonate, methyl trifluoroethyl carbonate, ethyl trifluoroethyl carbonate, methyl hexafluoroisopropyl carbonate, di(2,2,2-trifluoroethyl) carbonate, 2,2-difluoroethyl acetate, 2,2,2-trifluoroethyl acetate, hexafluoroisopropyl acetate, 2,2-difluoroethyl propionate, 2,2,2-trifluoroethyl propionate or hexafluoroisopropyl propionate. (2) the non-fluorinated linear ester is selected from at least one of dimethyl carbonate, ethyl methyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate or propyl propionate. (3) Based on the total mass of the non-aqueous electrolyte, the mass percentage of the linear ester is X0%, 10≤X0≤70, preferably 15≤X0≤50. Based on the above embodiment, the above linear esters including the fluorinated linear esters and the non-fluorinated linear esters are selected in the electrolyte, and the content of the cyclic carbonate is regulated within the above range, which can further improve the high temperature storage performance, while further improving the low temperature discharge performance of the electrochemical device.

[0022] In some embodiments, the mass percentage of linear ester X0%, the mass percentage of fluorinated linear ester X1%, and the mass percentage of non-fluorinated linear ester X2% in the above non-aqueous electrolyte meet at least one of the following conditions: (1) 10≤X1≤50; (2) 5≤X2≤50. Based on the above embodiments, the electrochemical device of the present application adjusts the content parameters of the mass percentage of fluorinated linear ester X1% and the mass percentage of non-fluorinated linear ester X2% in the non-aqueous electrolyte within the above range, so that the content of each compound, especially the content of fluorinated linear ester, is within a suitable range, which is more conducive to further improving the high-temperature storage performance, while further considering improving the low-temperature discharge performance of the electrochemical device.

[0023] In some embodiments, the non-aqueous electrolyte further comprises an internal salt substance, specifically comprising a compound of formula IV and / or a compound of formula V:

[0024] Compounds, Compound.

[0025] Wherein R1 to R5 are independently selected from hydrogen atoms, fluorine atoms, vinyl groups, acetylene groups or anhydride groups; based on the total mass of the non-aqueous electrolyte, the sum of the mass percentages of the above-mentioned compounds of formula IV and formula V is 0.1% to 1%; any two adjacent groups among R1 to R5 exist independently, or are connected by covalent bonds and connected to the parent ring to form a ring. Based on the above embodiments, the electrochemical device of the present application further adds a certain amount of inner salt substances in the electrolyte, and the inner salt substances can complex the lithium-containing transition metal composite oxide Li x Na z Co 1-y M y O2 dissolves and frees transition metal ions in the electrolyte, greatly reducing the deposition of transition metal ions at the negative electrode and improving SEI stability, thereby improving the cycle performance, high-temperature storage performance and low-temperature discharge performance of the electrochemical device.

[0026] In some embodiments, the compound of formula IV comprises at least one of the following compounds:

[0027]

[0028] The compound of formula V comprises at least one of the following compounds:

[0029]

[0030] Based on the above embodiments, the above inner salt substances can be used to more efficiently complex the lithium-containing transition metal composite oxide Li x Na z Co 1-y M y The transition metal ions dissolved in O2 and freed in the electrolyte reduce the deposition of transition metal ions at the negative electrode, improve the stability of SEI, and further improve the cycle performance, high temperature storage performance and low temperature discharge performance of the electrochemical device.

[0031] In a second aspect, an embodiment of the present application provides an electronic device, which includes the above-mentioned electrochemical device. DETAILED DESCRIPTION

[0032] In order to make the purpose, technical solution and advantages of the present application more clear, the present application is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described here are only used to explain the present application and are not used to limit the present application.

[0033] An embodiment of the present application provides an electrochemical device, including a positive electrode, a non-aqueous electrolyte, a negative electrode and a separator.

[0034] positive electrode

[0035] The positive electrode includes a positive electrode current collector and a positive electrode material layer disposed on at least one surface of the positive electrode current collector. The positive electrode material layer includes a lithium-containing transition metal composite oxide, and the lithium-containing transition metal composite oxide includes Li x Na z Co 1-y M y O2, wherein 0.6<x<0.95, 0≤y<0.15, 0<z≤0.03, M is at least one selected from the group consisting of Al, Mg, Ti, Mn, Fe, Ni, Zn, Cu, Nb, Cr and Zr. For example, the above subscripts may be 0.6<x<0.7, 0≤y<0.10, and 0<z<0.01; 0.7<x<0.8, 0.05<y<0.10, and 0<z<0.02; 0.8<x<0.9, 0.06<y<0.09, and 0<z≤0.03; 0.9<x<0.95, 0.07<y<0.08, and 0.01<z<0.02; 0.6<x<0.9, 0.08<y<0.15, and 0.01<z≤0.03. By adding the above-mentioned lithium-containing transition metal composite oxide to the positive electrode material layer in the electrochemical device, and controlling the content ratio of each metal atom in the lithium-containing transition metal composite oxide, especially controlling the content ratio of sodium atoms to meet the above-mentioned range, it is possible to improve both the high-temperature storage performance and the low-temperature discharge performance of the electrochemical device.

[0036] In some embodiments, the positive electrode material layer includes a positive electrode conductive material; the type of the positive electrode conductive material is not limited, and any known conductive material can be used. Examples of positive electrode conductive materials may include, but are not limited to, carbon black such as acetylene black and Super-P; amorphous carbon materials such as needle coke; carbon nanotubes; graphene, etc. The above positive electrode conductive materials may be used alone or in any combination.

[0037] In some embodiments, the positive electrode material layer includes a positive electrode binder; the type of the positive electrode binder is not particularly limited, and in the case of a coating method, any material that can be dissolved or dispersed in a liquid medium used in electrode manufacturing can be used. Examples of positive electrode binders may include, but are not limited to, one or more of the following: resin polymers such as polyethylene, polypropylene, polyethylene terephthalate, polymethyl methacrylate, polyimide, aromatic polyamide, cellulose, nitrocellulose, etc.; rubber polymers such as styrene-butadiene rubber, nitrile rubber, fluororubber, isoprene rubber, polybutadiene rubber, ethylene-propylene rubber, etc.; thermoplastic elastomer polymers such as styrene-butadiene-styrene block copolymers or their hydrides, ethylene-propylene-diene terpolymers, styrene-ethylene-butadiene-ethylene copolymers, styrene-isoprene-styrene block copolymers or their hydrides; soft resin polymers such as syndiotactic-1,2-polybutadiene, polyvinyl acetate, ethylene-vinyl acetate copolymers, propylene-α-olefin copolymers; fluorine polymers such as polyvinylidene fluoride, polytetrafluoroethylene, fluorinated polyvinylidene fluoride, polytetrafluoroethylene-ethylene copolymers; polymer compositions having ion conductivity of alkali metal ions, etc. The above positive electrode binders may be used alone or in any combination.

[0038] There is no limitation on the type of solvent used to form the positive electrode slurry, as long as it is a solvent that can dissolve or disperse the positive electrode active material, the conductive material, the positive electrode binder, and the thickener used as needed. Examples of solvents used to form the positive electrode slurry may include any of aqueous solvents and organic solvents. Examples of aqueous media may include, but are not limited to, a mixed medium of alcohol and water or water, etc. Examples of organic media may include, but are not limited to, aliphatic hydrocarbons such as hexane; aromatic hydrocarbons such as benzene, toluene, xylene, methylnaphthalene; heterocyclic compounds such as quinoline and pyridine; ketones such as acetone, methyl ethyl ketone, and cyclohexanone; esters such as methyl acetate and methyl acrylate; amines such as diethylenetriamine and N,N-dimethylaminopropylamine; ethers such as diethyl ether, propylene oxide, and tetrahydrofuran; amides such as N-methylpyrrolidone, dimethylformamide, and dimethylacetamide; aprotic polar solvents such as hexamethylphosphoramide and dimethyl sulfoxide, etc.

[0039] Thickeners are generally used to adjust the viscosity of the slurry. In the case of using an aqueous medium, the thickener and styrene-butadiene rubber emulsion can be used for slurrying. The type of thickener is not particularly limited, and examples thereof may include, but are not limited to, carboxymethyl cellulose, methyl cellulose, hydroxymethyl cellulose, ethyl cellulose, polyvinyl alcohol, oxidized starch, phosphorylated starch, casein, and salts thereof. The above thickeners may be used alone or in any combination.

[0040] The type of positive electrode current collector is not particularly limited, and it can be any material known to be suitable for use as a positive electrode current collector. Examples of positive electrode current collectors may include, but are not limited to, metal materials such as aluminum, stainless steel, nickel plating, titanium, tantalum, and materials such as carbon cloth and carbon paper. In some embodiments, the positive electrode current collector is a metal material. In some embodiments, the positive electrode current collector is aluminum.

[0041] In order to reduce the electronic contact resistance between the positive electrode current collector and the positive electrode material layer, the surface of the positive electrode current collector may include a conductive additive or a conductive coating. Examples of conductive additives may include, but are not limited to, carbon and precious metals such as gold, platinum, and silver. Examples of conductive coatings may include a mixture layer containing an inorganic oxide, a conductive agent, and a binder.

[0042] Non-aqueous electrolyte

[0043] The non-aqueous electrolyte used in the electrochemical device of the present application embodiment includes an electrolyte and a solvent that dissolves the electrolyte. In some embodiments, the non-aqueous electrolyte of the present application includes a compound of formula I:

[0044] Compounds;

[0045] wherein R is selected from C2 to C6 alkyl which is unsubstituted or substituted by Ra, C2 to C6 alkenyl which is unsubstituted or substituted by Ra, C2 to C6 alkynyl which is unsubstituted or substituted by Ra, C5 to C6 alkyl which is unsubstituted or substituted by Ra, 12 A nitrogen-containing heteroaryl group, a C6 to C 12 The substituents Ra of each group are independently selected from fluorine or C1 to C6 fluoroalkyl. For example, R is selected from C2 alkyl, C4 alkyl, C6 alkyl, fluorine-substituted C5 alkenyl, fluorine-substituted C7 alkynyl, fluorine-substituted C 10 a nitrogen-containing heteroaryl group, a C6 alkyl group substituted with a C2 fluoroalkyl group, a C2 fluoroalkyl group substituted with a C 12 The aromatic group.

[0046] In some embodiments, based on the total mass of the non-aqueous electrolyte, the mass percentage of the compound of formula I is A%, and the positive electrode material layer contains lithium transition metal composite oxide Li x Na z Co 1-y M yIn some embodiments, 1≤A / z≤200. In some embodiments, 5≤A / z≤100. In some embodiments, 10≤A / z≤20. In some embodiments, 50≤A / z≤80. In some embodiments, 25≤A / z≤70. In some embodiments, 35≤A / z≤55. In some embodiments, 0.1≤A≤5, for example, A is 0.1, 0.2, 0.5, 1.0, 2.0, 2.5, 3.0, 4.0, 5.0, or a value within a range consisting of any two of these values. In some embodiments, 0.005≤z≤0.03. For example, z is 0.005, 0.01, 0.015, 0.02, 0.023, 0.028, 0.03, or a value within a range consisting of any two of these values. By adding the compound of formula I to the non-aqueous electrolyte in the electrochemical device, and controlling the A value in the mass percentage of the compound of formula I in the non-aqueous electrolyte and the z value in the lithium-containing transition metal composite oxide and their ratio to meet the above-mentioned range, the high-temperature storage performance of the electrochemical device can be improved, while also improving the low-temperature discharge performance of the electrochemical device.

[0047] In some embodiments, the compound of formula I comprises at least one of the following compounds:

[0048]

[0049] For example, the compound of formula I is a mixture of a compound of formula I-1, a compound of formula I-8, a compound of formula I-13, a compound of formula I-2, and a compound of formula I-7, a mixture of a compound of formula I-4 and a compound of formula I-11, and a mixture of a compound of formula I-2 and a compound of formula I-14. By selecting the above-mentioned compounds of formula I, it is possible to improve both the high temperature storage performance and the low temperature discharge performance of the electrochemical device.

[0050] In some embodiments, the non-aqueous electrolyte further comprises a dinitrile substance as shown in the compound of formula II and a trinitrile substance as shown in the compound of formula III:

[0051] Compound.

[0052] Wherein, R0 is selected from C2 to C 10 Chain alkylene, C2 to C 10 Alkenylene or -R a -(OR b ) n -R c -, R a , R b and R c Each is independently selected from a C1 to C3 alkylene group or a C2 to C3 alkenylene group, and n is an integer of 1 to 3.

[0053] Compound.

[0054] Among them, R 11 , R 12 and R 13 are each independently selected from C1 to C3 alkylene or -R A -(OR B ) n -R C -, R A , R B and R C are each independently selected from a single bond, a C1 to C2 alkylene group, n is an integer from 1 to 3, R 21 Selected from hydrogen atom, C1 to C3 alkylene. In some embodiments, the mass percentage of the compound of formula II is B%, the mass percentage of the compound of formula III is C%, and 0.05≤A / (B+C)≤50. In some embodiments, 1≤A / (B+C)≤30. In some embodiments, 10≤A / (B+C)≤20. In some embodiments, 5≤A / (B+C)≤25. In some embodiments, 0.1≤A / (B+C)≤2. Adding the compound of formula II and the compound of formula III to the non-aqueous electrolyte in the electrochemical device, and controlling the ratio of the sum of the mass percentage of the compound of formula II and the compound of formula III in the non-aqueous electrolyte to the A value in the mass percentage of the compound of formula I to meet the above range, can take into account the improvement of the high temperature storage performance and low temperature discharge performance of the electrochemical device.

[0055] In some embodiments, the mass percentage B% of the compound of formula II and the mass percentage C% of the compound of formula III are 0.5≤B+C≤8. In some embodiments, 2≤B+C≤8. In some embodiments, 5≤B+C≤7. In some embodiments, 4≤B+C≤6. In some embodiments, 0.5≤B+C≤3. In some embodiments, 0.1≤B≤6, for example, B is 0.1, 0.5, 1, 2, 3.5, 4, 6 or a value within the range of any two of these values. In some embodiments, 0.1≤C≤6. For example, C is 0.1, 0.3, 1, 2, 4, 5, 6 or a value within the range of any two of these values. By controlling the mass percentage B% of the compound of formula II in the non-aqueous electrolyte, the mass percentage C% of the compound of formula III and the sum of their mass percentages to meet the above range, it is possible to take into account both the improvement of the high temperature storage performance and the low temperature discharge performance of the electrochemical device.

[0056] In some embodiments, the compound of formula II is selected from at least one of succinonitrile, glutaronitrile, methylglutaronitrile, adiponitrile, pimelonitrile, suberonitrile, trans-butene dinitrile or 1,2-bis(cyanoethoxy)ethane. In some embodiments, the compound of formula III is selected from at least one of 1,3,5-pentane trinitrile, 1,3,6-hexane trinitrile or 1,2,3-tri(2-cyanoethoxy)propane. By selecting the above-mentioned types of compounds of formula II and compounds of formula III, it is possible to improve both the high temperature storage performance and the low temperature discharge performance of the electrochemical device.

[0057] In some embodiments, the non-aqueous electrolyte further comprises a cyclic carbonate, which is selected from at least two of ethylene carbonate, propylene carbonate or fluoroethylene carbonate. In some embodiments, based on the total mass of the non-aqueous electrolyte, the mass percentage of the cyclic carbonate is 1% to 30%. In some embodiments, for example, the mass percentage of the cyclic carbonate is 2%, 5%, 10%, 17%, 22%, 29% or a value within the range of any two of these values. In some embodiments, preferably, the mass percentage of the cyclic carbonate is 2% to 15%. Adding cyclic carbonate to the non-aqueous electrolyte in the electrochemical device and controlling the mass percentage of the cyclic carbonate in the non-aqueous electrolyte to meet the above range can take into account the improvement of the high temperature storage performance and low temperature discharge performance of the electrochemical device.

[0058] In some embodiments, the non-aqueous electrolyte further comprises linear esters, and the linear esters comprise fluorinated linear esters and non-fluorinated linear esters. The fluorinated linear esters are selected from at least one of methyl difluoroethyl carbonate, methyl trifluoroethyl carbonate, ethyl trifluoroethyl carbonate, methyl hexafluoroisopropyl carbonate, di(2,2,2-trifluoroethyl) carbonate, 2,2-difluoroethyl acetate, 2,2,2-trifluoroethyl acetate, hexafluoroisopropyl acetate, 2,2-difluoroethyl propionate, 2,2,2-trifluoroethyl propionate or hexafluoroisopropyl propionate. The non-fluorinated linear esters are selected from at least one of dimethyl carbonate, ethyl methyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate or propyl propionate. In some embodiments, based on the total mass of the non-aqueous electrolyte, the mass percentage of the linear ester is X0%, 10≤X0≤70, preferably 15≤X0≤50. For example, X0 is 10, 15, 25, 22, 31, 45, 50, 70 or a value in the range formed by any two of these values. By selecting the above-mentioned types of linear esters and controlling the mass percentage of the linear esters in the non-aqueous electrolyte to meet the above-mentioned range, it is possible to improve both the high temperature storage performance and the low temperature discharge performance of the electrochemical device.

[0059] In some embodiments, the mass percentage of the fluorinated linear ester in the non-aqueous electrolyte is X1%, 10≤X1≤50. For example, X1 is 10, 12, 26, 35, 41, 47, 50, or a value in the range of any two of these values. In some embodiments, the mass percentage of the non-fluorinated linear ester is X2%, 5≤X2≤50. For example, X2 is 5, 9, 18, 24, 33, 40, 50, or a value in the range of any two of these values. By controlling the mass percentage of the fluorinated linear ester and the non-fluorinated linear ester in the non-aqueous electrolyte to meet the above range, it is possible to improve both the high temperature storage performance and the low temperature discharge performance of the electrochemical device.

[0060] In some embodiments, the non-aqueous electrolyte further comprises an internal salt substance, specifically comprising a compound of formula IV and / or a compound of formula V:

[0061] Compounds, Compound.

[0062] Wherein R1 to R5 are each independently selected from a hydrogen atom, a fluorine atom, a vinyl group, an acetylene group or an anhydride group; based on the total mass of the non-aqueous electrolyte, the sum of the mass percentages of the above-mentioned compound of formula IV and the compound of formula V is 0.1% to 1%. For example, the sum of the mass percentages of the compound of formula IV and the compound of formula V is 0.1%, 0.3%, 0.5%, 0.6%, 0.9%, 1% or a value in the range composed of any two of these values. In some embodiments, any two adjacent groups of R1 to R5 exist independently or are connected by covalent bonds to form a ring with the parent ring. By selecting the above-mentioned types of compounds of formula IV and formula V, and controlling the sum of the mass percentages of the compounds of formula IV and formula V in the non-aqueous electrolyte to meet the above range, it is possible to take into account the improvement of the high temperature storage performance, low temperature discharge performance and cycle performance of the electrochemical device.

[0063] In some embodiments, the compound of formula IV comprises at least one of the following compounds:

[0064]

[0065] The compound of formula V comprises at least one of the following compounds:

[0066]

[0067] By selecting the above-mentioned compounds of formula IV and formula V, it is possible to improve the high-temperature storage performance, low-temperature discharge performance and cycle performance of the electrochemical device.

[0068] The non-aqueous electrolyte may also include a lithium salt and a non-aqueous solvent. The present application does not particularly limit the type of lithium salt, as long as the purpose of the present application can be achieved. For example, the lithium salt may include but is not limited to at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium difluorophosphate, lithium bistrifluoromethanesulfonyl imide, lithium bis(fluorosulfonyl)imide, lithium bisoxalate borate or lithium difluorooxalate borate. Based on the mass of the non-aqueous electrolyte, the mass percentage of the lithium salt may be 8% to 15%, for example, the mass percentage of the lithium salt may be 8%, 9%, 10%, 11%, 12.5%, 13%, 15% or a range consisting of any two of the values. The present application does not particularly limit the type of the above-mentioned non-aqueous solvent, as long as the purpose of the present application can be achieved, for example, it may include but is not limited to at least one of ether compounds or other organic solvents. The above-mentioned ether compound may include but is not limited to at least one of ethylene glycol dimethyl ether, dibutyl ether, tetraethylene glycol dimethyl ether, diethylene glycol dimethyl ether, 1,2-dimethoxyethane, 1,2-diethoxyethane, 1-ethoxy-1-methoxyethane, 2-methyltetrahydrofuran or tetrahydrofuran. The above-mentioned other organic solvents may include but are not limited to at least one of dimethyl sulfoxide, 1,2-dioxolane, cyclopentane, methyl cyclopentane, 1,3-dimethyl-2-imidazolidinone, N-methyl-2-pyrrolidone, dimethylformamide, acetonitrile, trimethyl phosphate, triethyl phosphate or trioctyl phosphate.

[0069] negative electrode

[0070] The negative electrode comprises a negative electrode current collector and a negative electrode material layer disposed on at least one surface of the negative electrode current collector, wherein the negative electrode material layer comprises a negative electrode active material. In some embodiments, the chargeable capacity of the negative electrode active material is greater than the discharge capacity of the positive electrode active material to prevent lithium metal from being accidentally precipitated on the negative electrode during charging.

[0071] The negative electrode active material may include natural graphite, artificial graphite, mesophase microcarbon beads (MCMB), silicon, silicon-carbon composites, SiO x (0.5<x<1.6), Li-Sn alloy, Li-Sn-O alloy, Sn, SnO, SnO2, spinel structure lithium titanate Li4Ti5O 12 , Li-Al alloy or metallic lithium, etc. Optionally, the negative electrode active material may further include an amorphous carbon material, and the amorphous carbon may be soft carbon (low temperature calcined carbon), hard carbon, mesophase pitch carbide or calcined coke, etc.

[0072] The negative electrode material layer of the present application also includes a negative electrode binder. The negative electrode binder can improve the bonding between the negative electrode active material particles and the bonding between the negative electrode active material and the current collector. The type of negative electrode binder is not particularly limited, as long as it is a material that is stable to the solvent used in the manufacture of the electrolyte or electrode. In some embodiments, the negative electrode binder includes a resin binder. Examples of resin binders include, but are not limited to, fluororesins, polyacrylonitrile (PAN), polyimide resins, acrylic resins, polyolefin resins, and the like. When an aqueous solvent is used to prepare the negative electrode mixture slurry, the negative electrode binder includes, but is not limited to, carboxymethyl cellulose (CMC) or its salt, styrene-butadiene rubber (SBR), polyacrylic acid (PAA) or its salt, polyvinyl alcohol, and the like.

[0073] The negative electrode material layer of the present application also includes a conductive agent. The present application has no particular restrictions on the type of the negative electrode conductive agent, as long as the purpose of the present application can be achieved. For example, the negative electrode conductive agent can be at least one of acetylene black, Ketjen black, carbon nanotubes, carbon fibers, carbon dots or graphene, and the above-mentioned carbon nanotubes can include but are not limited to at least one of single-walled carbon nanotubes or multi-walled carbon nanotubes.

[0074] The present application has no particular restrictions on the negative electrode current collector, as long as the purpose of the present application can be achieved. For example, the negative electrode current collector may include copper foil, aluminum foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam or a polymer substrate covered with a conductive metal, etc. Among them, the conductive metal includes but is not limited to copper, nickel or titanium, and the material of the polymer substrate includes but is not limited to at least one of polyethylene, polypropylene, ethylene propylene copolymer, polyethylene terephthalate, polyethylene naphthalate or poly(p-phenylene terephthalamide). In the present application, there is no particular restriction on the thickness of the negative electrode current collector and the negative electrode material layer, as long as the purpose of the present application can be achieved. For example, the thickness of the negative electrode current collector is 4μm to 12μm, and the thickness of the single-sided negative electrode material layer is 30μm to 160μm. In the present application, the negative electrode mixture layer can be arranged on one surface in the thickness direction of the negative electrode current collector, or on two surfaces in the thickness direction of the negative electrode current collector. It should be noted that the "surface" here can be the entire area of ​​the negative electrode current collector or a partial area of ​​the negative electrode current collector. This application has no special restrictions as long as the purpose of this application can be achieved.

[0075] The present application has no particular restrictions on the compaction density of the negative electrode sheet, as long as the purpose of the present application can be achieved. For example, the compaction density of the negative electrode sheet can be 1.0 g / cm 3 Up to 1.85g / cm 3 The present application has no particular limitation on the cold pressing pressure of the negative electrode sheet, as long as the purpose of the present application can be achieved. For example, the cold pressing pressure of the negative electrode sheet can be 3 tons to 30 tons.

[0076] Optionally, the negative electrode plate may further include a conductive layer, which is located between the negative electrode current collector and the negative electrode material layer. The present application has no particular restrictions on the composition of the conductive layer, which may be a conductive layer commonly used in the art. The conductive layer includes a conductive agent and a binder. The present application has no particular restrictions on the conductive agent and the binder in the conductive layer, which may be at least one of the above conductive agent and the above binder. The present application has no particular restrictions on the mass ratio of the conductive agent and the binder in the conductive layer, and those skilled in the art can choose according to actual needs, as long as the purpose of the present application can be achieved. The present application has no particular restrictions on the thickness of the conductive layer, as long as the purpose of the present application can be achieved, for example, the thickness of the conductive layer is 1μm to 10μm.

[0077] Diaphragm

[0078] In the present application, a diaphragm is usually provided between the positive electrode and the negative electrode, and the diaphragm is used to separate the positive electrode plate and the negative electrode plate to prevent internal short circuit of the secondary battery, allow electrolyte ions to pass freely, and do not affect the electrochemical charge and discharge process.

[0079] The present application has no particular restrictions on the separator, as long as the purpose of the present application can be achieved. For example, the material of the separator may include but is not limited to polyethylene (PE), polypropylene (PP)-based polyolefins (PO), polyester (e.g., polyethylene terephthalate (PET) film), cellulose, polyimide (PI), polyamide (PA), spandex or aramid; the type of the separator may include at least one of woven membrane, non-woven membrane, microporous membrane, composite membrane, rolled membrane or spun membrane.

[0080] In the present application, the diaphragm may include a substrate and a surface treatment layer. The substrate may be a non-woven fabric or a composite film having a porous structure, and the material of the substrate may include at least one of polyethylene, polypropylene, polyethylene terephthalate or polyimide. Optionally, a polypropylene porous film, a polyethylene porous film, a polypropylene non-woven fabric, a polyethylene non-woven fabric or a polypropylene-polyethylene-polypropylene porous composite film may be used. Optionally, a surface treatment layer is provided on at least one surface of the substrate, and the surface treatment layer may be a polymer layer or an inorganic layer, or a layer formed by a mixed polymer and an inorganic substance. For example, the inorganic layer includes inorganic particles and a binder, and the present application has no particular restrictions on the above-mentioned inorganic particles, for example, it may include at least one of aluminum oxide, silicon oxide, magnesium oxide, titanium oxide, hafnium dioxide, tin oxide, cerium dioxide, nickel oxide, zinc oxide, calcium oxide, zirconium oxide, yttrium oxide, silicon carbide, boehmite, aluminum hydroxide, magnesium hydroxide, calcium hydroxide or barium sulfate. The present application has no particular restrictions on the above-mentioned binder, for example, it may be at least one of the aforementioned binders. The polymer layer contains a polymer, and the material of the polymer includes at least one of polyamide, polyacrylonitrile, acrylate polymer, polyacrylic acid, polyvinyl pyrrolidone, polyvinyl ether, polyvinylidene fluoride or poly(vinylidene fluoride-hexafluoropropylene).

[0081] The pore size of the diaphragm in the present application is 0.01 μm to 1 μm, and the thickness is 5 μm to 50 μm. In some embodiments, the thickness of the diaphragm is greater than 1 μm, greater than 5 μm, or greater than 8 μm. In some embodiments, the thickness of the diaphragm is less than 50 μm, less than 40 μm, or less than 30 μm. When the thickness of the diaphragm is within the above range, the insulation and mechanical strength can be ensured, and the rate characteristics and energy density of the secondary battery can be ensured.

[0082] The electrochemical device of the present application also includes a packaging bag for containing a positive electrode sheet, a separator, a negative electrode sheet and an electrolyte, as well as other components known in the art in the electrochemical device, and the present application does not limit the above other components. The present application does not specifically limit the packaging bag, and it can be a packaging bag known in the art, as long as it can achieve the purpose of the present application.

[0083] The present application further provides an electronic device, which includes the electrochemical device of the embodiment of the present application. The electronic device includes but is not limited to a laptop computer, a pen-input computer, a mobile computer, an electronic book player, a portable phone, a portable fax machine, a portable copier, a portable printer, a head-mounted stereo headset, a video recorder, an LCD TV, a portable cleaner, a portable CD player, a mini-disc, a transceiver, an electronic notepad, a calculator, a memory card, a portable recorder, a radio, a backup power supply, a motor, a car, a motorcycle, a power-assisted bicycle, a bicycle, a lighting fixture, a toy, a game console, a clock, an electric tool, a flashlight, a camera, a large household battery and a lithium-ion capacitor, etc.

[0084] Example

[0085] Hereinafter, taking lithium-ion batteries as an example, examples and comparative examples are given to more specifically describe the implementation of the secondary battery of the present application. The preparation method described in the present application is only an example, and any other suitable preparation method is within the scope of the present application. In addition, unless otherwise specified, "parts" and "%" are based on mass.

[0086] Example 1-1

[0087] <Preparation of lithium-ion batteries>

[0088] (1) Preparation of positive electrode:

[0089] <Preparation of positive electrode active material>

[0090] a. Dissolve cobalt nitrate and aluminum nitrate in deionized water in a molar ratio of Co:Al = 0.985:0.015, add a precipitant of sodium carbonate and a complexing agent of ammonia until complete precipitation; then sinter the precipitate at 900°C to 1100°C, grind to obtain (Co 0.985 Al 0.015 )3O4 powder; finally, (Co 0.985 Al 0.015 )3O4 powder reacts with Na2CO3 in a molar ratio of Al:Na=0.015:0.7 in an air atmosphere at 700°C to 900°C to obtain Na 0.7 Co 0.985 Al 0.015 O2;

[0091] b. Using the Na obtained in step a 0.7 Co 0.985 Al 0.015 O2 is used as a precursor, and it is mixed evenly with lithium nitrate in a molar ratio of Na:Li=0.01:0.01, and reacted in an air atmosphere of 200°C to 400°C. After the reaction is completed, the obtained reactant molten salt powder is washed with deionized water for multiple times, and then dried to obtain the positive electrode active material Li 0.73 Na 0.01 Co 0.985 Al 0.015 O2.

[0092] <Preparation of positive electrode sheet>

[0093] The positive electrode active material, conductive carbon black, and polyvinylidene fluoride (PVDF) prepared in the above steps are mixed in a mass ratio of 95:2:3, N-methylpyrrolidone (NMP) is added, and the mixture is stirred evenly under the action of a vacuum mixer to obtain a positive electrode slurry with a solid content of 70wt%. The positive electrode slurry is evenly coated on one surface of a positive electrode current collector aluminum foil with a thickness of 9μm, and dried to obtain a positive electrode sheet coated with a positive electrode mixture layer on one side. Repeat the above steps on the other surface of the positive electrode current collector aluminum foil to obtain a positive electrode sheet coated with a positive electrode mixture layer on both sides. After cold pressing, cutting, slitting, and drying, a positive electrode sheet with a specification of 74mm×867mm is obtained.

[0094] (2) Preparation of non-aqueous electrolyte: In a dry argon atmosphere glove box, diethyl carbonate is used as a base solvent, and then the compound of formula I and lithium hexafluorophosphate (LiPF6) are dissolved in the above base solvent, and vinylene carbonate is added as an additive to obtain an electrolyte. Wherein, based on the total mass of the electrolyte, the mass percentage of LiPF6 is 12.5%, the mass percentage of vinylene carbonate is 2%, the mass percentage of the compound of formula I is 0.1%, and the balance is diethyl carbonate.

[0095] (3) Preparation of negative electrode: artificial graphite is used as the negative electrode active material, and the negative electrode active material, styrene-butadiene rubber (SBR), polyacrylic acid (PAA), carbon nanotubes (CNT), and carboxymethyl cellulose (CMC) are mixed in a mass ratio of 95.8:2.4:0.5:0.5:0.8, and then deionized water is added as a solvent and stirred evenly to prepare a negative electrode slurry with a solid content of 45wt%. The negative electrode slurry is evenly coated on one surface of a negative electrode current collector copper foil with a thickness of 6μm, and dried to obtain a negative electrode sheet coated with a negative electrode mixture layer on one side. The above steps are repeated on the other surface of the negative electrode current collector copper foil to obtain a negative electrode sheet coated with a negative electrode mixture layer on both sides. After cold pressing, cutting, slitting, and drying, a negative electrode sheet with a specification of 76.6mm×875mm is obtained.

[0096] (4) Preparation of diaphragm: A porous polyethylene film with a thickness of 15 μm was used as the diaphragm.

[0097] (5) Preparation of lithium-ion batteries: stack the positive electrode sheet, separator, and negative electrode sheet in order, place the separator between the positive electrode sheet and the negative electrode sheet to play an isolating role, and wind them to obtain a bare cell. Place the bare cell in a packaging bag, inject electrolyte, and package. After the process of formation, degassing, trimming, and capacity testing, a lithium-ion battery is obtained.

[0098] <Test Method>

[0099] (1) Test of the atomic ratio of lithium-containing transition metal composite oxides in the positive electrode material layer

[0100] Disassemble the lithium-ion battery to obtain the positive electrode plate, clean the positive electrode plate with dimethyl carbonate (DMC), scrape off the positive electrode material layer of the cleaned positive electrode plate with a scraper, take 0.4g of the positive electrode material layer and dissolve it in a mixed solvent of 10mL (nitric acid and hydrochloric acid mixed in a ratio of 1:1) aqua regia and 2mL HF, make the volume to 100mL, and then use an ICP (Inductively coupled plasma) analyzer to test the mass percentage of lithium, sodium, cobalt and M elements, and the remainder is the percentage of oxygen. According to the atomic mass of each element, it is converted into its molar percentage, and the molar percentage ratio of each element is normalized to calculate the corresponding x value, y value and z value. The z value is the number of sodium atoms in the lithium-containing transition metal composite oxide in the positive electrode material layer. Li 0.73 Na 0.01 Co 0.985 Al 0.015 Taking O2 as an example, 0.4g of the positive electrode material layer was dissolved in a mixed solvent of 10mL (nitric acid and hydrochloric acid were mixed in a ratio of 1:1) aqua regia and 2mL of HF, and the volume was fixed to 100mL. Then, the ICP analyzer was used to test and the mass percentages of lithium, sodium, cobalt and aluminum were 52919ppm, 2401ppm, 606266ppm and 4227ppm respectively. The remaining mass was recorded as the mass of the oxygen element, and its mass proportion was 1000000ppm-(52919+2401+606266+4277)ppm=334187ppm. The mass percentage was then divided by the atomic mass of each element to obtain the molar ratio of the above elements Li:Na:Co:Al:O=0.762:0.0104:1.029:0.0157:2.089. The value of oxygen is set to 2, and the above ratio is normalized to obtain Li:Na:Co:Al:O=0.73:0.01:0.985:0.015:2, that is, x=0.73; y=0.015; z=0.01.

[0101] (2) High temperature storage performance test:

[0102] Place the lithium-ion battery in a constant temperature environment at 25°C and let it stand for 30 minutes to allow the lithium-ion battery to reach a constant temperature. Charge it to 4.5V at a constant current of 0.5C, and then charge it to a current of 0.025C at a constant voltage of 4.5V. Use a PPG soft-pack battery thickness gauge to test the battery thickness at a pressure of 700g. Select 5 different points at the non-ear position to measure the thickness. Record the thickness of the lithium-ion battery measured 5 times, and record the average of the 5 test values ​​as the initial thickness. Transfer the lithium-ion battery to a 60°C constant temperature box for storage for 30 days. Take out the battery and cool it to room temperature. Select 5 different points at the non-ear position, use a PPG soft-pack battery thickness gauge to test and record the battery thickness after storage at a pressure of 700g, and record the average of the 5 test values ​​as the storage thickness. Calculate the thickness expansion rate of the lithium-ion battery and use it as an indicator to evaluate the high-temperature storage performance of the lithium-ion battery.

[0103] High temperature storage thickness expansion ratio = (storage thickness - initial thickness) / initial thickness × 100%.

[0104] (3) Low temperature discharge performance test:

[0105] Place the lithium-ion battery in a high and low temperature box, adjust the temperature to 25°C, and let it stand for 30 minutes to allow the lithium-ion battery to reach a constant temperature. The lithium-ion battery that has reached a constant temperature is discharged to 3.0V at a current constant current of 0.5C, then charged to 4.5V at a current constant current of 0.5C, and then charged to a current of 0.05C at the 4.5V voltage constant voltage. Also at a temperature of 25°C, discharge to 3.0V at a current constant current of 0.5C, and record the discharge capacity as the initial discharge capacity. At a temperature of 25°C, charge to 4.5V at a constant current of 0.5C, and then charge to a current of 0.05C at the 4.5V voltage constant voltage. Afterwards, place the lithium-ion battery at a temperature of 0°C and let it stand for 30 minutes to keep the temperature of the lithium-ion battery consistent with the outside temperature. At 0°C, discharge to 3.0V at a current constant current of 0.5C, and record the discharge capacity as the low-temperature discharge capacity.

[0106] Low-temperature discharge capacity retention rate = (low-temperature discharge capacity / initial discharge capacity) × 100%.

[0107] (4) Cyclic performance test:

[0108] Place the lithium-ion battery in a 45°C constant temperature test box and let it stand for 30 minutes to allow the lithium-ion battery to reach a constant temperature. Charge to 4.5V at a constant current of 0.5C, then charge to a current of 0.025C at a constant voltage of 4.5V, let it stand for 5 minutes, and discharge to 3.0V at a constant current of 0.5C, and record it as the initial discharge capacity C0. Repeat this step for 100 cycles, record the discharge capacity C1 after 100 cycles, and calculate the cycle capacity retention rate of the lithium-ion battery. Cycle capacity retention rate = C1 / C0×100%.

[0109] The lithium ion batteries of the following embodiments or comparative examples differ from those of embodiment 1-1 only in that the type of the compound of formula I in the non-aqueous electrolyte and the value of the mass percentage A, the type of the M element in the lithium-containing transition metal composite oxide, and the z value are adjusted according to Table 1, wherein when adjusting the z value, lithium-containing transition metal composite oxides with different numbers of sodium atoms are used as raw materials, and x and y are controlled to satisfy 0.6<x<0.95 and 0≤y<0.15, respectively. The performance test results of the lithium ion batteries of the embodiments and comparative examples are shown in Table 1 below.

[0110] Table 1

[0111]

[0112] In the above table, " / " indicates that the substance is not contained. M is the type of M element, based on the mass of the electrolyte, A is the mass percentage of the compound of formula I, and z is the z value in the lithium-containing transition metal composite oxide.

[0113] As can be seen from Table 1, the lithium-containing transition metal composite oxide Li x Na z Co 1-y M y In O2, the z value satisfies 0<z≤0.03, and the mass percentage of the compound of formula I, A%, satisfies 1≤A / z≤200, which can improve the low-temperature discharge performance of the lithium-ion battery, and is also beneficial to improve the stability of the positive electrode material layer under high temperature conditions, so that the lithium-ion battery has excellent high-temperature storage performance. Among them, when the above conditions meet at least one of the following situations: (1) 5≤A / z≤100; (2) 0.1≤A≤5; (3) 0.005≤z≤0.02, the low-temperature discharge capacity retention rate of the lithium-ion battery can be further improved, while taking into account the high-temperature storage expansion rate of the lithium-ion battery.

[0114] The lithium ion batteries of the following Examples 2-1 to 2-28 differ from those of Example 1-5 only in that a specific type and content of dinitrile compounds and trinitrile compounds are added during the preparation of the electrolyte. The lithium ion batteries of Examples 2-29 to 2-34 differ from those of Example 1-5 only in that a specific type and content of dinitrile compounds and trinitrile compounds are added during the preparation of the electrolyte, and the value of the mass percentage A% of the compound of formula I is adjusted. The mass percentages of the above-mentioned compounds of formula I, dinitrile compounds and trinitrile compounds in the electrolyte are shown in Table 2, and the performance test results of the lithium ion batteries of each example are shown in Table 2 below.

[0115] Table 2

[0116]

[0117]

[0118] In the above table, " / " indicates that the substance is not contained. Based on the mass of the electrolyte, A is the mass percentage of the compound of formula I, B is the mass percentage of the compound of formula II, and C is the mass percentage of the compound of formula III.

[0119] As can be seen from Table 2, when the non-aqueous electrolyte of the lithium ion battery prepared in the embodiment of the present application further includes the compound of formula II and the compound of formula III, and satisfies 0.05≤A / (B+C)≤50, the high temperature storage expansion rate and low temperature discharge capacity retention rate of the lithium ion battery can be further improved. In particular, when the content relationship of the compound of formula I, the compound of formula II and the compound of formula III in the electrolyte is regulated to meet any of the following conditions: (1) 0.5≤B+C≤8; (2) 0.1≤A / (B+C)≤2; (3) 0.1≤B≤6; (4) 0.1≤C≤6, the effect of improving the high temperature storage expansion rate and low temperature discharge capacity retention rate of the lithium ion battery is more significant.

[0120] The lithium ion batteries of the following Examples 3-1 to 3-40 are adjusted based on the parameters of Examples 1-5; the lithium ion batteries of Example 3-41 are adjusted based on the parameters of Examples 2-30. The specific adjustment is: adding specific types and contents of cyclic carbonates, fluorinated linear esters, non-fluorinated linear esters, compounds of Formula IV and compounds of Formula V during the preparation of the electrolyte, and the mass percentages of these substances in the electrolyte are shown in Table 3. The performance test results of the lithium ion batteries of each example are shown in Table 3 below.

[0121] Table 3

[0122]

[0123]

[0124] In the above table, “ / ” means that the substance is not contained. The contents of each item are based on the mass of the electrolyte, and the corresponding compounds of each item code are as follows:

[0125] EC: ethylene carbonate, PC: propylene carbonate, FEC: fluoroethylene carbonate.

[0126] As can be seen from Table 3, when the non-aqueous electrolyte of the lithium ion battery prepared by the embodiment of the present application further includes cyclic carbonate, linear ester or inner salt material, the cycle capacity retention rate of the lithium ion battery can be further improved, while taking into account the improvement of high temperature storage expansion rate and low temperature discharge capacity retention rate. In particular, when the mass percentage of cyclic carbonate is 2% to 15%, the cycle capacity retention rate of the lithium ion battery can be significantly improved, while taking into account the improvement of high temperature storage expansion rate and low temperature discharge capacity retention rate. In particular, when the mass percentage of linear ester is 15% to 50%, the cycle capacity retention rate of the lithium ion battery can be significantly improved, while taking into account the improvement of high temperature storage expansion rate and low temperature discharge capacity retention rate. In particular, when the sum of the mass percentage of the inner salt material IV compound and the formula V compound is 0.1% to 1%, the cycle capacity retention rate of the lithium ion battery can be significantly improved, while taking into account the improvement of high temperature storage expansion rate and low temperature discharge capacity retention rate.

[0127] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the principles of the present application should be included in the protection scope of the present application.

Claims

1. An electrochemical device, characterized in that The invention comprises a positive electrode and a non-aqueous electrolyte, wherein the positive electrode comprises a positive electrode material layer provided on at least one surface of a positive electrode current collector, wherein the positive electrode material layer comprises a lithium-containing transition metal composite oxide, wherein the lithium-containing transition metal composite oxide comprises Li x Na z Co 1-y M y O2, wherein 0.6<x<0.95, 0≤y<0.15, 0<z≤0.03, M is at least one selected from the group consisting of Al, Mg, Ti, Mn, Fe, Ni, Zn, Cu, Nb, Cr and Zr; the non-aqueous electrolyte comprises a compound of formula I: wherein R is selected from C2 to C6 alkyl which is unsubstituted or substituted by Ra, C2 to C6 alkenyl which is unsubstituted or substituted by Ra, C2 to C6 alkynyl which is unsubstituted or substituted by Ra, C5 to C6 alkyl which is unsubstituted or substituted by Ra, 12 nitrogen-containing heteroaryl, unsubstituted or substituted C6 to C 12 The aryl group, the substituents Ra of each group are independently selected from fluorine or C1 to C6 fluoroalkyl; Based on the total mass of the non-aqueous electrolyte, the mass percentage of the compound of formula I is A%, and 1≤A / z≤200.

2. The electrochemical device according to claim 1, wherein The electrochemical device satisfies at least one of the following conditions: (1)5≤A / z≤100; (2)0.1≤A≤5; (3)0.005≤z≤0.02。 3. The electrochemical device according to claim 1, wherein The compound of formula I includes at least one of the following compounds:

4. The electrochemical device according to claim 1, wherein The non-aqueous electrolyte further comprises a compound of formula II and a compound of formula III: Wherein, R0 is selected from C2 to C 10 Chain alkylene, C2 to C 10 Alkenylene or -R a -(OR b ) n -R c -, R a 、R b and R c Each is independently selected from C1 to C3 alkylene or C2 to C3 alkenylene, and n is an integer from 1 to 3; Among them, R 11 、R 12 and R 13 Each independently selected from C1 to C3 alkylene or -R A -(OR B ) n -R C -, R A 、R B and R C Each is independently selected from a single bond, a C1 to C2 alkylene group, n is an integer from 1 to 3, R 21 a hydrogen atom, a C1 to C3 alkylene group; Based on the total mass of the non-aqueous electrolyte, the mass percentage of the compound of formula II is B%, the mass percentage of the compound of formula III is C%, and 0.05≤A / (B+C)≤50.

5. The electrochemical device according to claim 4, characterized in that The non-aqueous electrolyte satisfies at least one of the following conditions: (1) 0.5≤B+C≤8; (2) 0.1≤A / (B+C)≤2; (3)0.1≤B≤6; (4)0.1≤C≤6。 6. The electrochemical device according to claim 4, characterized in that The compound of formula II is selected from at least one of succinonitrile, glutaronitrile, methylglutaronitrile, adiponitrile, pimelonitrile, suberonitrile, fumaronitrile or 1,2-bis(cyanoethoxy)ethane; and / or, The compound of formula III is selected from at least one of 1,3,5-pentanetrinitrile, 1,3,6-hexanetrinitrile or 1,2,3-tris(2-cyanoethoxy)propane.

7. The electrochemical device according to any one of claims 1 to 6, characterized in that The non-aqueous electrolyte further comprises a cyclic carbonate, which is selected from at least two of ethylene carbonate, propylene carbonate, and fluoroethylene carbonate; based on the total mass of the non-aqueous electrolyte, the mass percentage of the cyclic carbonate is 1% to 30%.

8. The electrochemical device according to claim 7, characterized in that Based on the total mass of the non-aqueous electrolyte, the mass percentage of the cyclic carbonate is 2% to 15%.

9. The electrochemical device according to any one of claims 1 to 6, characterized in that The non-aqueous electrolyte further includes a linear ester, wherein the linear ester includes a fluorinated linear ester and a non-fluorinated linear ester; and the linear ester satisfies at least one of the following conditions: (1) The fluorinated linear ester is at least one selected from methyl difluoroethyl carbonate, methyl trifluoroethyl carbonate, ethyl trifluoroethyl carbonate, methyl hexafluoroisopropyl carbonate, bis(2,2,2-trifluoroethyl) carbonate, 2,2-difluoroethyl acetate, 2,2,2-trifluoroethyl acetate, hexafluoroisopropyl acetate, 2,2-difluoroethyl propionate, 2,2,2-trifluoroethyl propionate or hexafluoroisopropyl propionate; (2) the non-fluorinated linear ester is selected from at least one of dimethyl carbonate, ethyl methyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, or propyl propionate; (3) Based on the total mass of the non-aqueous electrolyte, the mass percentage of the linear ester is X0%, 10≤X0≤70.

10. The electrochemical device according to claim 9, characterized in that Based on the total mass of the non-aqueous electrolyte, the non-aqueous electrolyte satisfies at least one of the following conditions: (1) The mass percentage of the fluorinated linear ester is X1%, 10≤X1≤50; (2) The mass percentage of the non-fluorinated linear ester is X2%, 5≤X2≤50; (3)15≤X0≤50。 11. The electrochemical device according to any one of claims 1 to 6, characterized in that: The non-aqueous electrolyte further comprises a compound of formula IV and / or a compound of formula V; wherein R1 to R5 are each independently selected from a hydrogen atom, a fluorine atom, a vinyl group, an acetylene group or an anhydride group; Based on the total mass of the non-aqueous electrolyte, the sum of the mass percentages of the compound of formula IV and the compound of formula V is 0.1% to 1%; Any two adjacent groups among R1 to R5 exist independently, or are linked to the parent ring through a covalent bond to form a ring.

12. The electrochemical device according to claim 11, characterized in that The compound of formula IV comprises at least one of the following compounds: And / or, the compound of formula V comprises at least one of the following compounds:

13. An electronic device comprising the electrochemical device according to any one of claims 1 to 12.

Citation Information

Patent Citations

  • Electrolyte containing -S-F group compound and electrochemical device thereof

    CN111370766A

  • Electrolyte, electrochemical device and electronic device

    CN116960454A

  • Electrochemical apparatus and electronic apparatus

    WO2024168480A1