Hard alloy sintering process, hard alloy and hard alloy saw disc thereof
By combining vacuum sintering and differential pressure sintering processes, a uniform high cobalt surface is formed, which solves the problem of black pitting and inert gas partial pressure sintering during vacuum sintering, improves welding fluidity and strength, and extends cemented carbide The service life of the saw disc.
Patent Information
- Application Number
- CN202411133604.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-12-06
AI Technical Summary
In the existing cemented carbide sintering process, vacuum sintering causes black pits and microcracks on the surface of the cobalt-rich layer, affecting the welding fluidity and strength. The cobalt-depleted surface formed by partial pressure sintering of inert gas is not conducive to solder spreading, resulting in welding strength. Difference.
By combining vacuum sintering and differential pressure sintering processes, the differential pressure state is adjusted by continuously vacuuming and introducing inert gas in the sintering furnace, the atmosphere in the furnace is controlled, and a uniform high cobalt surface is formed, impurities are accumulated and capillary resistance is reduced, and black hemp is avoided. generation of points.
The formation of a uniform high cobalt layer on the surface of cemented carbide is achieved, the fluidity and welding strength of solder are improved, the service life of cemented carbide saw disks is extended, and the quality of processing workpieces is improved.
Smart Images

Figure CN119076945A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of cemented carbide, and in particular to a cemented carbide sintering process, cemented carbide and a cemented carbide saw disk thereof. Background Art
[0002] Carbide saw blades are widely used in wood processing, metal cutting and other fields due to their excellent wear resistance and cutting efficiency. Carbide saw discs are formed by welding carbide saw blades and steel substrates. The performance of carbide saw discs depends not only on the quality of carbide, but also on the welding process between the steel body. Among them, welding fluidity and welding strength are important indicators for measuring welding quality, which directly affect the performance and life of carbide saw discs.
[0003] Most of the cemented carbide saw blades in domestic coated cemented carbide saw discs are made of YG tungsten cobalt. At present, the common sintering processes for YG tungsten cobalt are vacuum sintering process and inert gas partial pressure sintering process. During the vacuum sintering process, the carbon atmosphere in the sintering furnace is low, and the decarburization atmosphere promotes the outward migration of the Co phase, so that a cobalt-rich layer is formed on the surface of the prepared cemented carbide. The cobalt-rich layer is conducive to the spreading of the above-mentioned solder on the surface of the cemented carbide, that is, it is conducive to improving the fluidity of the solder, thereby enhancing the welding strength between the cemented carbide and the steel substrate. However, during the sintering process of the vacuum sintering process, it is easy to produce defects such as black pitting, microcracks and metamorphic layers on the surface of the cobalt-rich layer of the cemented carbide, which leads to poor fluidity of the solder on its cemented carbide surface, which is not conducive to its welding strength with the steel substrate. The inert gas partial pressure sintering process reduces the amount of impurity aggregation between the cemented carbide phase interfaces and reduces the capillary resistance in the sintered body, thereby effectively avoiding the problem of black pitting on the cemented carbide surface. However, on the one hand, the cemented carbide surface sintered by the inert gas partial pressure sintering process is a cobalt-poor layer, which is not conducive to the spreading of solder on the cemented carbide surface, that is, the fluidity of the solder on the cemented carbide surface is poor, which is not conducive to the welding strength between it and the steel substrate; on the other hand, the cemented carbide surface sintered by the inert gas partial pressure sintering process is also accompanied by a local cobalt-rich phenomenon, which further makes the solder spread unevenly on the cemented carbide surface and also affects the appearance of the product. Summary of the invention
[0004] In order to solve the above technical problems, the present invention provides a cemented carbide sintering process, by which a cemented carbide with a uniform high-cobalt surface is produced, the solder has strong welding fluidity on the cemented carbide surface, and the welding strength between the cemented carbide and the steel substrate is high.
[0005] The technical solution of the present invention is:
[0006] A cemented carbide sintering process, characterized in that it comprises the following steps:
[0007] S1, blank pressing: placing the cemented carbide mixture in a mold and pressing to obtain a blank;
[0008] S2, vacuum sintering: placing the blank in the furnace of a sintering furnace, evacuating the furnace, controlling the vacuum degree below 30Pa, introducing inert gas, heating from room temperature to 750-850°C, and keeping the temperature for 3-5h;
[0009] Evacuate the sample and control the vacuum degree below 30Pa. Raise the sintering temperature to 800℃-1200℃ and keep it at this temperature for 3-4h.
[0010] Among them, the sintering stage at 20℃-800℃ is the degreasing sintering stage, the main purpose of which is to remove the forming agent in the blank. The introduction of inert gas is conducive to taking away the wax atmosphere in the furnace and ensuring the cleanliness of the atmosphere in the furnace.
[0011] The sintering stage at 800℃-1200℃ is the solid phase sintering stage. The solid phase reaction in the sintered body is intensified, which is mainly manifested in the diffusion and welding between the elements in the sintered body, and the sintered body shrinks a little;
[0012] S3, micro-pressure sintering: in a continuous vacuum state, inert gas is filled to keep the furnace in a micro-pressure state, and the sintering temperature is raised to 1200°C-1450°C for 3-5h;
[0013] S4, cooling with the furnace, the blank is cooled with the furnace to room temperature, and a cemented carbide with a uniform high-cobalt surface is obtained.
[0014] Furthermore, in the step S1, the pressing pressure is 5.5-6.5 KN.
[0015] Furthermore, in the step S2, the inert gas flow rate is 5-8 SLM.
[0016] Furthermore, in the step S3, the inert gas flow rate is 8-10 SLM, and the differential partial pressure value is less than 5 mbar.
[0017] The above-mentioned sintering stage of 1200° C.-1450° C. is a liquid phase sintering stage, and the Co in the sintered body at this stage is in liquid phase.
[0018] During this stage, if it is in a vacuum state, the carbon atmosphere in the furnace is relatively low, and the decarburization atmosphere promotes the outward migration of the Co phase, thereby forming a cobalt-rich layer on the surface of the sintered body. However, due to the cleanliness and atmosphere in the furnace, the cobalt-rich surface layer is prone to black pitting, which is not conducive to the spreading of the solder on its surface, that is, the fluidity of the solder on its surface is poor, which ultimately affects the welding strength between it and the steel substrate.
[0019] At this stage, if the conventional inert gas partial pressure sintering process is used and the inert gas is directly introduced into the furnace, on the one hand, the inert gas atmosphere in the furnace can effectively control the outward migration of the Co phase and eventually form a cobalt-poor surface on the surface of the sintered body, which is not conducive to the spreading of the solder on the surface, that is, the fluidity of the solder on its surface is poor; on the other hand, if the furnace is kept in a vacuum state while the inert gas is introduced, so that the gas enters and exits at the same time, it is difficult to form the micro-partial pressure state described in the present invention.
[0020] Therefore, the present invention adopts a downward air intake method to introduce inert gas, that is, the inert gas enters from the wax outlet below the sintering furnace, and slowly penetrates into the furnace located in the insulation layer through the insulation layer in the sintering furnace, during which continuous vacuum is maintained, thereby facilitating the adjustment of the differential pressure below 5 mbar.
[0021] The differential pressure sintering described in the present invention, on the one hand, has the advantage of forming a uniform cobalt-rich surface by vacuum sintering, and on the other hand, utilizes the differential pressure atmosphere to reduce the amount of impurity segregation between the interfaces of the sintered bodies, reduces the capillary resistance in the sintered bodies, and thus avoids the problem that the cobalt-rich surface produced by the vacuum sintering process is prone to black pitting.
[0022] Furthermore, the inert gas is argon.
[0023] The present invention produces a hard alloy according to the hard alloy sintering process.
[0024] The invention also provides a hard alloy saw disk, which is made by welding the hard alloy and a metal saw disk.
[0025] Furthermore, the outer circumferential surface of the metal saw disk is provided with a plurality of saw teeth, the cemented carbide is polished and passivated to form a single cemented carbide saw blade, and a cemented carbide saw blade is welded to each saw tooth on the metal saw disk by solder.
[0026] Furthermore, the solder is Ag-Sn solder, and the soldering temperature is 380-420°C.
[0027] The beneficial technical effects of the present invention are:
[0028] Firstly, the present invention adopts vacuum sintering combined with differential pressure sintering process in the liquid phase sintering stage of cemented carbide, thereby producing a cemented carbide with a high cobalt surface and a surface cobalt content of up to 99.5%. This preparation process obtains a uniform high cobalt surface while effectively solving the problem of black pitting impurities produced by conventional vacuum sintering process.
[0029] Secondly, the cemented carbide prepared by the cemented carbide sintering process of the present invention has a uniform high-cobalt surface, so that the solder has better welding fluidity thereon, which is beneficial to the welding of the cemented carbide with the metal matrix, so that the cemented carbide saw disc made therefrom has stronger welding strength, effectively prolonging the service life of the cemented carbide saw disc and improving the quality of the workpiece processed therefrom. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 is a schematic cross-sectional view of a sintering furnace of the present invention;
[0031] Figure 2 This is a surface morphology image of cemented carbide A1 obtained in Example 1 of the present invention (resolution is 50X);
[0032] Figure 3 This is a surface morphology image of cemented carbide A1 prepared in Comparative Example 1 of the present invention (resolution is 100X);
[0033] Figure 4 This is a surface morphology image of cemented carbide B1 obtained in Comparative Example 1 of the present invention (resolution is 100X);
[0034] Figure 5 This is a surface morphology image of cemented carbide B1 obtained in Comparative Example 1 of the present invention (resolution is 550X);
[0035] Figure 6 This is a surface morphology image of cemented carbide C1 obtained in Comparative Example 2 of the present invention (resolution is 100X);
[0036] Figure 7 This is a surface morphology image of cemented carbide C1 obtained in Comparative Example 2 of the present invention (resolution is 3000X);
[0037] Figure 8 This is a surface morphology image of cemented carbide D1 obtained in Comparative Example 3 of the present invention (resolution is 100X);
[0038] Fig. 9 This is a surface morphology image of cemented carbide D1 obtained in Comparative Example 3 of the present invention (resolution is 3000X);
[0039] Fig.10 This is a schematic diagram of a hard alloy saw disc A2 product made by the present invention;
[0040] Fig.11 yes Fig.10 A partial enlarged view of
[0041] Fig.12 This is the spreading distribution state diagram of the solder on the surface of cemented carbide A1 after being heated;
[0042] Fig.13This is the spreading distribution state diagram of the solder on the surface of cemented carbide B1 after being heated;
[0043] Fig.14 This is the spreading distribution state diagram of the solder on the surface of cemented carbide C1 after being heated;
[0044] Fig.15 This is the spreading distribution state diagram of the solder on the surface of cemented carbide D1 after being heated;
[0045] in:
[0046] 1-furnace, 2-vacuum pump, 3-insulation layer, 4-wax outlet, 5-blank, 6-heater, 7-partial pressure air inlet. DETAILED DESCRIPTION
[0047] In order to more clearly understand the technical means of the present invention and implement it according to the contents of the specification, the specific implementation methods of the present invention are further described in detail below in conjunction with the drawings and examples. The following examples are used to illustrate the present invention but are not used to limit the scope of the present invention.
[0048] Example 1
[0049] The present invention provides a cemented carbide process, comprising the following steps:
[0050] S1, compaction molding:
[0051] The cemented carbide mixture is placed in a cemented carbide mold and pressed using a press (Oswald) at a pressure of 5.8 KN to obtain a blank 5;
[0052] The cemented carbide mixture is a commercially available YG6 alloy powder, which includes 93% WC, 6% Co, and 1% additives;
[0053] S2, vacuum sintering:
[0054] The blank is placed in the furnace 1 of the sintering furnace, and the vacuum is evacuated to 20 Pa. Argon gas is introduced from the partial pressure inlet 7, and the argon gas flow rate is 8 SLM. The temperature is raised from room temperature to 800°C within 5 hours to complete debinding sintering.
[0055] After the debinding and sintering steps are completed, the vacuum is evacuated to 20 Pa, and the temperature is raised from 800°C to 1200°C within 4 hours to complete the solid phase sintering;
[0056] S3, micro-pressure sintering, under continuous vacuum state, argon gas is filled in, the argon gas flow rate is 10SLM, and the furnace 1 is controlled to be in a micro-pressure state, the micro-pressure is 3mbar, and the sintering temperature is increased from 1200℃ to 1400℃ within 5h to complete liquid phase sintering;
[0057] The argon gas enters the furnace 1 in the following manner. That is, the argon gas enters from the wax outlet 4 below the sintering furnace, and slowly penetrates into the furnace 1 located in the insulation layer 3 through the insulation layer 3;
[0058] S4, cooling with the furnace. After the blank 5 is cooled with the furnace to room temperature, a cemented carbide with a uniform high-cobalt surface is obtained.
[0059] By the cemented carbide process described in Example 1 above, a cemented carbide A1 having a uniform high-cobalt surface was obtained.
[0060] In addition, the present invention also produces cemented carbide B1, cemented carbide C1 and cemented carbide D1, and cemented carbide B1-D1 are respectively produced by the cemented carbide processes described in comparative examples 1-3. Among them, the cemented carbide process described in comparative example 1 is a conventional vacuum sintering process. The cemented carbide processes described in comparative examples 2-3 are existing inert gas partial pressure sintering processes, and the difference between the two is that the partial pressure values are different.
[0061] Comparative Example 1
[0062] Compared with the cemented carbide process of Example 1, the cemented carbide process of Comparative Example 1 has the same S1 step and S4 step. The difference is that the cemented carbide process of Comparative Example 1 replaces the S2 and S3 steps in the cemented carbide process of Example 1 with:
[0063] Place the blank 5 in the furnace 1 of the sintering furnace, evacuate the furnace to a vacuum degree of 20 Pa, raise the temperature from room temperature to 800°C within 5 hours to complete degreasing sintering; raise the temperature from 800°C to 1200°C within 4 hours to complete solid phase sintering; raise the sintering temperature from 1200°C to 1400°C within 5 hours to complete liquid phase sintering.
[0064] Comparative Example 2
[0065] Compared with the cemented carbide process of Example 1, the cemented carbide process of Comparative Example 2 has the same S1 step and S4 step, and the only difference is that the cemented carbide process of Comparative Example 2 adjusts the S2 and S3 steps in the cemented carbide process of Example 1 to:
[0066] The blank 5 is placed in the furnace 1 of the sintering furnace. After evacuation, the vacuum degree is 20Pa, and argon is directly introduced into the furnace 1 from the partial pressure inlet 7. The argon flow rate is 10SLM, and the partial pressure value is maintained at 40mbar. The temperature is raised from room temperature to 800℃ within 5 hours to complete degreasing sintering; the temperature is raised from 800℃ to 1200℃ within 4 hours to complete solid phase sintering; the sintering temperature is raised from 1200℃ to 1400℃ within 5 hours to complete liquid phase sintering.
[0067] Comparative Example 3
[0068] Compared with Comparative Example 2, Comparative Example 3 differs only in the argon flow rate and partial pressure value, and the other process steps are the same. The argon flow rate of Comparative Example 3 is 20 SLM, and the partial pressure value is 200 mbar.
[0069] The surface morphology and surface cobalt content test results of cemented carbide A1-D1 are as follows Figure 2-Figure 9 As shown, the surface morphology of the cemented carbide was measured by an electron microscope (JSM-I T500A), and the cobalt content on the cemented carbide surface was measured by an electron scanning electron microscope (JSM-IT500A).
[0070] Depend on Figure 2-3 It can be seen that the surface layer of cemented carbide A1 is a uniform cobalt-rich layer with a cobalt content of 99.5%. Figure 4-5 It can be seen that the surface layer of cemented carbide B1 is a cobalt-rich layer with a cobalt content of 98%, and the cobalt-rich layer is uniformly dotted with black pits.
[0071] Depend on Figure 6-7 It can be seen that the surface layer of cemented carbide C1 is a cobalt-poor layer with a cobalt content of 52.5%, and the cobalt-poor layer is accompanied by a dot-shaped local cobalt-rich layer. Figure 8-9 It can be seen that the surface layer of cemented carbide D1 is a cobalt-poor layer with a cobalt content of 42%, and the cobalt-poor layer is accompanied by a flaky local cobalt-rich layer. Moreover, by comparing the test results of cemented carbide C1-D1, it can be seen that with the increase of the partial pressure value, the cobalt content on the surface of cemented carbide D1 is lower than that on the surface of cemented carbide C1.
[0072] Preparation of carbide saw blade
[0073] The preparation steps of the cemented carbide saw disc of the present invention are as follows:
[0074] 1. Raw materials: hard alloy, metal saw disc and solder. The metal saw disc is in the shape of a disc, and its outer circumference is composed of a plurality of saw teeth. The metal saw disc of the present invention is an alloy steel matrix. The solder used in the present invention includes: Ag-Sn solder.
[0075] 2. The cemented carbide is polished and passivated to form a single cemented carbide saw blade, each cemented carbide saw blade is dipped in solder and placed on each saw tooth on a metal saw disk, and then heated to 400°C by a high-frequency brazing gun for welding, thereby obtaining a cemented carbide saw disk.
[0076] According to the above-mentioned preparation steps of the cemented carbide saw disc, cemented carbide A1-D1 are used to prepare cemented carbide saw discs A2-D2, wherein Figure 10-11 It is carbide saw disc A2.
[0077] Carbide A1-D1 welding fluidity and carbide saw blade A2-D2 welding strength test
[0078] Welding fluidity and welding strength are important indicators to measure welding quality. If the welding fluidity and welding strength are poor, the carbide saw blade of the carbide saw disk will easily fall off or break teeth, which will seriously affect the service life of the carbide saw disk and reduce the quality of the processed workpiece.
[0079] Welding fluidity test
[0080] 0.1g of solder was placed on the surface of cemented carbide A1-D1 respectively, and after being heated to 400°C using a high-frequency brazing gun, the distribution state of the solder on the surface of cemented carbide A1-D1 was observed. Among them, the surface size of cemented carbide A1-D1 is about 8mm×3mm.
[0081] The welding fluidity test results of the solder on the surface of cemented carbide A1-D1 are as follows Figure 12-Figure 15 shown.
[0082] like Fig.12 As shown in the figure, after the solder is heated, it covers the surface of cemented carbide A1, indicating that the solder has good welding fluidity on the surface of cemented carbide A1; Fig.13 As shown in the figure, after the solder is heated, its spreading area on the surface of cemented carbide B1 is larger, but smaller than the spreading rate on cemented carbide A1, that is, its welding fluidity on the surface of cemented carbide B1 is worse than that of cemented carbide A1; Figure 14-15 As shown, after the solder is heated, the spreading area on the surface of cemented carbide C1-D1 is small, which indicates that the welding fluidity of the solder on the cobalt-poor surface is poor.
[0083] Carbide saw blade A2-D2 welding strength test
[0084] This test uses a welding strength tester (JQD-800B) to test the welding strength. It applies longitudinal shear force to the carbide saw blade on the carbide saw disk, and calculates the welding strength value by calculating the force per unit area. When the calculated welding strength value is greater than 120Mpa, the welding strength of the carbide saw disk is a qualified value.
[0085] In this test, in order to ensure the reliability of the test results, 10 pieces of carbide saw discs A2-D2 were prepared, that is, each carbide saw disc was subjected to 10 strength tests, and the final test result was taken as the average value. The test results of each carbide saw disc are shown in Table 1.
[0086] Table 1
[0087]
[0088] From the test results in Table 1, it can be seen that the welding strength between carbide saw disc A2 and metal saw disc is the largest, which is 146.6Mpa, far greater than the qualified value of carbide saw disc welding strength. The welding strength between carbide saw disc B2, carbide saw disc C2 and carbide saw disc D2 and metal saw disc are all less than 120Mpa, which do not reach the qualified value of carbide saw disc welding strength.
[0089] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. It should be pointed out that a person skilled in the art can make several improvements and modifications without departing from the technical principles of the present invention, and these improvements and modifications should also be regarded as within the scope of protection of the present invention.
Claims
1. A cemented carbide sintering process, characterized in that: The following steps are involved: S1, blank pressing: placing the cemented carbide mixture in a mold and pressing to obtain a blank; S2, vacuum sintering: placing the blank in the furnace of a sintering furnace, evacuating the furnace, controlling the vacuum degree below 30Pa, introducing inert gas, heating from room temperature to 750-850°C, and keeping the temperature for 3-5h; Evacuate the sample and control the vacuum degree below 30Pa. Raise the sintering temperature to 800℃-1200℃ and keep it at this temperature for 3-4h. S3, micro-pressure sintering: under continuous vacuum state, inert gas is introduced in the following air intake method to keep the furnace in micro-pressure state, and the sintering temperature is raised to 1200°C-1450°C for 3-5h; S4, cooling with the furnace, the blank is cooled with the furnace to room temperature, and a cemented carbide with a uniform high-cobalt surface is obtained.
2. The cemented carbide sintering process according to claim 1, characterized in that: In the step S1, the pressing pressure is 5.5-6.5 KN.
3. The cemented carbide sintering process according to claim 1, characterized in that: In the step S2, the inert gas flow rate is 5-8 SLM.
4. The cemented carbide sintering process according to claim 1, characterized in that: In the step S3, the inert gas flow rate is 8-10 SLM, and the differential partial pressure value is less than 5 mbar.
5. The cemented carbide sintering process according to claim 4, characterized in that: The inert gas enters the furnace of the sintering furnace in a downward air intake manner, that is, it enters from the wax outlet below the sintering furnace, passes through the insulation layer in the sintering furnace, and slowly penetrates into the furnace located in the insulation layer.
6. The cemented carbide sintering process according to claim 1, characterized in that: The inert gas is argon.
7. A cemented carbide, characterized in that: It is obtained by the cemented carbide sintering process according to any one of claims 1 to 6.
8. A cemented carbide saw disc, characterized in that: It is made by welding the hard alloy described in claim 7 and a metal saw disk.
9. A cemented carbide saw disc according to claim 8, characterized in that: The outer circumferential surface of the metal saw disk is provided with a plurality of saw teeth. The hard alloy is polished and passivated to form a single hard alloy saw blade. Each saw tooth on the metal saw disk is welded with a hard alloy saw blade by solder.
10. A cemented carbide saw disc according to claim 9, characterized in that: The solder is Ag-Sn solder, and the soldering temperature is 380-420°C.