Foam silk protein film and preparation method thereof, and pressure sensor and preparation method thereof

Through the preparation method of foam silk protein membrane, the problem of the in vivo pressure sensor requiring secondary surgery is solved, and the in vivo degradable and flexible pressure sensor without removal is achieved, with good biocompatibility and no biotoxicity.

CN119078235AActive Publication Date: 2024-12-06SHANGHAI INST OF MICROSYSTEM & INFORMATION TECH CHINESE ACAD OF SCI
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411185600.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-12-06
Estimated Expiration
2044-08-27

AI Technical Summary

Technical Problem

Existing in vivo pressure sensors require secondary surgery after the monitoring task is completed, which increases the burden on the patient and the material does not have good biocompatibility and degradability.

Method used

Using foam silk protein film as material, the preparation method includes providing a preset number of layers of auxiliary films, preparing silk protein solution, foaming treatment, drying and cross-linking treatment to form a foam layer with gas-containing products for building a pressure sensor.

Benefits of technology

It realizes a pressure sensor with in vivo degradable, flexible and mechanical properties that are adjustable in vivo, with good biocompatibility and no biotoxicity, and is suitable for in vivo monitoring.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119078235A_ABST
    Figure CN119078235A_ABST
Patent Text Reader

Abstract

The invention provides a foam silk protein film and a preparation method thereof, and a pressure sensor based on the foam silk protein film and a preparation method thereof. The preparation method of the foam silk protein film comprises the following steps: providing a preset number of layers of auxiliary films; preparing a silk protein solution with a second preset concentration; carrying out foaming treatment on the silk protein solution with the second preset concentration to obtain a foamed silk protein solution; injecting the foam silk protein solution between adjacent auxiliary membranes in a preset number of layers of auxiliary membranes to obtain a preset foam silk protein membrane; and drying and cross-linking the preset foam silk protein film to obtain the foam silk protein film with a preset number of layers. The foam layer in the foam silk protein membrane is composed of the silk protein foam containing gas and can correspondingly expand and contract when external pressure changes, and when the material is applied to a pressure sensor, the pressure sensor can have the advantages that the material can be degraded in vivo and does not need to be taken out through a secondary operation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of biomedical engineering, and specifically to a foam silk protein membrane and a preparation method thereof, and a pressure sensor based on the foam silk protein membrane and a preparation method thereof. Background Art

[0002] In clinical applications, in vivo pressure sensors are used to monitor and record pressure changes in the body or human body. In vivo pressure sensors can be implanted or inserted into the body to monitor blood pressure, intracranial pressure, intraocular pressure, bladder pressure, etc. Current in vivo pressure detection is often based on silicon materials or flexible materials such as polydimethylsiloxane (PDMS), polyurethane (PU), polyimide (PI), polyethylene terephthalate (PET), etc., but the pressure sensors made of these materials need to be removed by a secondary operation after their monitoring task is completed, which brings a bad experience to patients. Therefore, it is necessary to develop a material with good biocompatibility, degradable in vivo, no need for secondary surgery to remove, flexible and with adjustable mechanical properties for use in pressure sensors. Summary of the invention

[0003] In order to solve the above technical problems, the present application proposes a foam silk protein membrane and a preparation method, a pressure sensor based on the foam silk protein membrane and a preparation method.

[0004] On the one hand, the present application provides a method for preparing a foamed silk protein film, the method comprising:

[0005] Providing a preset number of layers of auxiliary film;

[0006] Preparing a silk fibroin solution of a first preset concentration, and concentrating the silk fibroin solution of the first preset concentration to obtain a silk fibroin solution of a second preset concentration;

[0007] Performing foaming treatment on the silk fibroin solution of the second preset concentration to obtain a foamed silk fibroin solution;

[0008] Injecting a foamed silk protein solution between adjacent auxiliary films in a preset number of layers of auxiliary films, and maintaining a preset distance between adjacent auxiliary films, to obtain a preset foamed silk protein film;

[0009] The preset foamed silk protein membrane is dried and cross-linked to obtain a foamed silk protein membrane with a preset number of layers.

[0010] Furthermore, the auxiliary film comprises a dry and water-insoluble silk protein film, and the above-mentioned provision of a preset number of layers of the auxiliary film comprises:

[0011] Providing a preset number of layers of dry and water-insoluble silk protein membrane, wherein the dry and water-insoluble silk protein membrane is pre-cross-linked;

[0012] The method of injecting the foamed silk protein solution between adjacent auxiliary films in a preset number of layers of auxiliary films and maintaining a preset distance between adjacent auxiliary films to obtain a preset foamed silk protein film comprises:

[0013] The foamed silk protein solution is injected between adjacent dry and water-insoluble silk protein membranes in a preset number of layers of dry and water-insoluble silk protein membranes, and a preset distance is maintained between adjacent dry and water-insoluble silk protein membranes to obtain a preset foamed silk protein membrane.

[0014] Furthermore, the auxiliary film comprises a water-insoluble polyvinyl alcohol film, and the above-mentioned provision of a preset number of layers of the auxiliary film comprises:

[0015] providing two layers of water-insoluble polyvinyl alcohol films;

[0016] Injecting a foamed silk protein solution between adjacent auxiliary films in a preset number of layers of auxiliary films, and maintaining a preset spacing between adjacent auxiliary films, to obtain a preset foamed silk protein film, comprising:

[0017] Injecting a foamed silk protein solution between two layers of water-insoluble polyvinyl alcohol films, and maintaining a preset distance between the two layers of water-insoluble polyvinyl alcohol films, to obtain a preset foamed silk protein film;

[0018] The above-mentioned drying treatment and cross-linking treatment of the preset foamed silk protein membrane to obtain a foamed silk protein membrane with a preset number of layers includes:

[0019] The preset foamed silk protein membrane is dried and cross-linked to obtain a three-layer foamed silk protein membrane. The three-layered foamed silk protein membrane comprises a polyvinyl alcohol film layer, a foam layer and a polyvinyl alcohol film layer from top to bottom.

[0020] Furthermore, after obtaining the three-layer foamed silk protein membrane, the method further comprises:

[0021] The polyvinyl alcohol film in the three-layer foam silk protein film is peeled off to obtain a single-layer foam silk protein film.

[0022] Furthermore, the above-mentioned processing of the silk fibroin solution of the second preset concentration to obtain the foamed silk fibroin solution comprises:

[0023] Stirring the silk fibroin solution of the second preset concentration and controlling the stirring conditions to obtain a foam silk fibroin solution of a preset foam size comprises: and / or,

[0024] Microbubbles are introduced into the silk protein solution of the second preset concentration, and the conditions for introducing the microbubbles are controlled to obtain a foam silk protein solution of a preset foam size.

[0025] Furthermore, the first preset concentration is 5-7% by mass, and the second preset concentration is 15-25% by mass.

[0026] Furthermore, the preset spacing is 30 μm-300 μm.

[0027] On the other hand, an embodiment of the present application further provides a foam silk protein membrane, which is prepared by the above method.

[0028] On the other hand, an embodiment of the present application also provides a pressure sensor based on a foam silk protein membrane, characterized in that the pressure sensor includes the above-mentioned foam silk protein membrane and a conductive structure; the conductive structure is used for impedance testing.

[0029] On the other hand, the embodiment of the present application also provides a method for preparing a pressure sensor based on a foamed silk protein film, characterized in that the method comprises:

[0030] Prepare a conductive structure on the surface of a preset number of layers of foam silk protein film; and / or

[0031] Conductive materials are doped into a preset number of layers of foam silk protein membrane to obtain a pressure sensor based on the foam silk protein membrane.

[0032] The embodiment of the present application provides a foam silk protein membrane and a preparation method, a pressure sensor based on the foam silk protein membrane and a preparation method. The preparation method of the foam silk protein membrane includes providing a preset number of layers of auxiliary membranes; preparing a silk protein solution of a second preset concentration; foaming the silk protein solution of the second preset concentration to obtain a foam silk protein solution; injecting the foam silk protein solution between adjacent auxiliary membranes in the preset number of layers of auxiliary membranes to obtain a preset foam silk protein membrane; drying and cross-linking the preset foam silk protein membrane to obtain a foam silk protein membrane with a preset number of layers. The foam layer in the foam silk protein membrane disclosed in the present application is composed of silk protein foam containing gas, and can expand and contract accordingly when the external pressure changes. The material is applied to the pressure sensor, which can make the pressure sensor have the advantages of no biological toxicity, no rejection reaction, in vivo degradability, flexibility, adjustable mechanical properties, in vivo degradability and no need for secondary surgery to remove. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] In order to more clearly illustrate the technical solutions and advantages in the embodiments of the present application or the prior art, the drawings required for use in the embodiments or the prior art descriptions are briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0034] Figure 1 It is a schematic diagram of a process for preparing a foamed silk protein film provided in an embodiment of the present application;

[0035] Figure 2 This is a schematic structural diagram of a three-layer foam silk protein membrane provided in an embodiment of the present application;

[0036] Figure 3 It is a schematic diagram of the structure of a single-layer foam silk protein membrane provided in an embodiment of the present application;

[0037] Figure 4 This is a schematic diagram of the structure of a pressure sensor based on a foam silk protein membrane provided in an embodiment of the present application;

[0038] Figure 5 This is a schematic diagram of the structure of a pressure sensor based on a foam silk protein membrane provided in an embodiment of the present application;

[0039] Figure 6 This is a schematic diagram of the structure of a pressure sensor based on a foam silk protein membrane provided in an embodiment of the present application;

[0040] Figure 7 This is a schematic diagram of the structure of a pressure sensor based on foam silk protein membrane provided in an embodiment of the present application. DETAILED DESCRIPTION

[0041] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.

[0042] It should be noted that the terms "first", "second", etc. in the specification and claims of the embodiment of the present application and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchanged where appropriate, so that the embodiments of the embodiment of the present application described here can be implemented in an order other than those illustrated or described here. Thus, the features defined as "first" and "second" can expressly or implicitly include one or more of the features. In the description of the present embodiment, unless otherwise specified, the meaning of "multiple" is two or more. In addition, the terms "including" and "having" and any of their variations are intended to cover non-exclusive inclusions, for example, a process, method, system, product or server comprising a series of steps or units is not necessarily limited to those steps or units clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.

[0043] In clinical applications, in vivo pressure sensors are used to monitor and record pressure changes in the body or human body. In vivo pressure sensors can be implanted or inserted into the body to monitor blood pressure, intracranial pressure, intraocular pressure, bladder pressure, etc. Current in vivo pressure detection is often based on silicon materials or flexible materials such as polydimethylsiloxane (PDMS), polyurethane (PU), polyimide (PI), polyethylene terephthalate (PET), etc. However, pressure sensors made of these materials require secondary surgery to remove after completing their monitoring tasks, which increases the burden on patients. Therefore, it is necessary to develop a material that can be degraded in vivo, does not require secondary surgery to remove, is flexible, and has adjustable mechanical properties for use in pressure sensors.

[0044] Silk protein materials are highly biocompatible and have been clinically applied. They have excellent properties such as non-biotoxicity, no rejection, in vivo degradability, flexibility, adjustable mechanical properties, and functionalization. With the help of micro-electromechanical systems (MEMS) technology and other methods, some functional structures can be integrated on silk protein membranes and applied to specific purposes, including bioelectrodes, controllable drug delivery, and biological indicator monitoring.

[0045] Based on this, Figure 1 As shown, the present application proposes a method for preparing a foamed silk protein film, the method comprising:

[0046] S10: providing a preset number of layers of auxiliary films.

[0047] Exemplarily, a preset number of layers of auxiliary films are provided first, and the function of the auxiliary films is to assist in the formation of the foamed silk protein film.

[0048] Optionally, the preset number of layers is greater than or equal to two layers and is an even number of layers.

[0049] S30: preparing a silk fibroin solution of a first preset concentration, and concentrating the silk fibroin solution of the first preset concentration to obtain a silk fibroin solution of a second preset concentration.

[0050] Exemplarily, a silk protein solution of a first preset concentration is prepared, and the method for preparing the silk protein solution is not limited herein, and the silk protein solution of the first preset concentration is concentrated to increase the concentration of the silk protein solution to obtain a silk protein solution of a second preset concentration. The second preset concentration is greater than the first preset concentration.

[0051] Optionally, the concentration treatment method includes but is not limited to dialysis.

[0052] S50: foaming the silk fibroin solution of the second preset concentration to obtain a foamed silk fibroin solution.

[0053] Exemplarily, the silk fibroin solution of the second preset concentration is foamed to obtain a silk fibroin solution containing gas, namely, a foamed silk fibroin solution.

[0054] It should be noted that, during the foaming process, the size of the foam can be controlled by controlling the conditions of the foaming process.

[0055] S70: injecting the foamed silk protein solution between adjacent auxiliary films in a preset number of layers of the auxiliary film, and maintaining a preset distance between adjacent auxiliary films, to obtain a preset foamed silk protein film.

[0056] Exemplarily, the foam silk protein solution is injected between adjacent auxiliary membranes in a preset number of layers of auxiliary membranes, that is, the foam silk protein solution is injected into every two layers of auxiliary membranes, and the distance between every two layers of auxiliary membranes is controlled to be a preset distance, thereby obtaining a preset foam silk protein membrane.

[0057] It should be noted that the preset distance between each two layers of auxiliary films can be different distances, that is, the preset distance can include a first preset distance, a second preset distance, a third preset distance and other preset distances, and it is not limited that the preset distance between each two layers of auxiliary films is the same. The preset distance corresponds to the thickness of a single layer of foam silk protein film.

[0058] S90: drying and cross-linking the preset foamed silk protein membrane to obtain a foamed silk protein membrane with a preset number of layers.

[0059] Exemplarily, the preset foamed silk protein membrane is dried as a whole, and then cross-linked to obtain a foamed silk protein membrane with a preset number of layers, wherein the preset number of layers is an odd number of layers.

[0060] Optionally, the cross-linking method includes but is not limited to water annealing and methanol cross-linking.

[0061] Optionally, the conditions for the drying process are not limited in this application, and the process may be carried out at room temperature and a relative humidity of 40%, or may be carried out under other conditions.

[0062] It should be noted that the auxiliary membrane can be a biodegradable membrane or a non-degradable membrane. When a non-degradable auxiliary membrane is used, the auxiliary membrane is stripped after cross-linking to obtain a foamed silk protein membrane. If a biodegradable membrane is used, no stripping treatment is required.

[0063] It should be noted that the preset number of layers is greater than the preset number of layers, and the preset number of layers is determined according to actual application needs.

[0064] The embodiment of the present application provides a method for preparing a foamed silk protein membrane, including providing a preset number of layers of auxiliary membranes; preparing a silk protein solution of a second preset concentration; foaming the silk protein solution of the second preset concentration to obtain a foamed silk protein solution; injecting the foamed silk protein solution between adjacent auxiliary membranes in the preset number of layers of auxiliary membranes to obtain a preset foamed silk protein membrane; drying and cross-linking the preset foamed silk protein membrane to obtain a foamed silk protein membrane of a preset number of layers. The foam layer in the foamed silk protein membrane disclosed in the present application is composed of silk protein foam containing gas, and can expand and contract accordingly when the external pressure changes. The application of this material to a pressure sensor can make the pressure sensor have the advantages of good biocompatibility, no biological toxicity, no rejection reaction, in vivo degradability, flexibility, adjustable mechanical properties, in vivo degradability, and no need for secondary surgery to remove.

[0065] As an optional implementation manner, the above-mentioned processing of the silk fibroin solution of the second preset concentration to obtain the foamed silk fibroin solution comprises:

[0066] Stirring the silk fibroin solution of the second preset concentration and controlling the stirring conditions to obtain a foam silk fibroin solution of a preset foam size comprises: and / or,

[0067] Microbubbles are introduced into the silk protein solution of the second preset concentration, and the conditions for introducing the microbubbles are controlled to obtain a foam silk protein solution of a preset foam size.

[0068] Exemplarily, the method of treating the silk protein solution includes stirring the silk protein solution and passing microbubbles into the silk protein solution, and both methods can control the size of the foam in the obtained foam silk protein solution, and the two methods can be used alone or together.

[0069] The stirring process can also be called the whipping process. The preparation of the foamed silk protein solution by this method means mixing air into the silk protein solution during the whipping process. The longer the whipping time, the finer the foam obtained. At the same time, the whipping amplitude can be controlled. The larger the whipping amplitude, the more air is mixed in, and the foam can be formed faster. In addition, the size of the foam formed can be changed by controlling the temperature of the silk protein solution, the type of agitator, etc.

[0070] The method of introducing microbubbles to prepare a foamed silk protein solution is achieved by directly introducing air into the silk protein solution. This method can change the size of the foam formed by controlling the size of the introduced bubbles. The smaller the introduced bubbles, the finer the foam.

[0071] The embodiment of the present application prepares a foamed silk protein solution by stirring or introducing microbubbles into the silk protein solution, laying a foundation for preparing a foamed silk protein membrane. The foam layer in the foamed silk protein membrane prepared by using the foamed silk protein solution is composed of silk protein containing gas, and can expand and contract accordingly when the external pressure changes. The application of this material to the pressure sensor can make the pressure sensor have the advantages of good biocompatibility, no biological toxicity, no rejection reaction, in vivo degradability, flexibility, adjustable mechanical properties, in vivo degradability, and no need for secondary surgery to remove.

[0072] As an optional implementation, the auxiliary film includes a dry and water-insoluble silk protein film. In the above step S10, providing a preset number of layers of auxiliary films includes:

[0073] A preset number of layers of dry and water-insoluble silk protein membranes are provided, wherein the dry and water-insoluble silk protein membranes are pre-cross-linked.

[0074] Exemplarily, the auxiliary membrane can be a dry and water-insoluble silk protein membrane, which has biocompatibility, biodegradability, good mechanical strength and flexibility, water permeability (although insoluble in water, the silk protein membrane has a certain water permeability, allowing water vapor and some small molecules to pass through), antibacterial properties and thermal stability.

[0075] The dry and water-insoluble silk protein membrane is pre-crosslinked, and the crosslinking method includes but is not limited to water annealing and methanol crosslinking.

[0076] In the above step S70, the foamed silk protein solution is injected between adjacent auxiliary films in a preset number of layers of auxiliary films, and a preset spacing is maintained between adjacent auxiliary films to obtain a preset foamed silk protein film, including:

[0077] The foamed silk protein solution is injected between adjacent dry and water-insoluble silk protein membranes in a preset number of layers of dry and water-insoluble silk protein membranes, and a preset distance is maintained between adjacent dry and water-insoluble silk protein membranes to obtain a preset foamed silk protein membrane.

[0078] It should be noted that the preset number of layers can be selected according to actual needs, so that the degradation speed and degradation time of the overall structure in the organism can be controlled.

[0079] The embodiment of the present application prepares a foam silk protein membrane with a preset number of layers through a degradable, dry and water-insoluble silk protein membrane, and controls its degradation rate and time in the organism by selecting the preset number of layers. The foam layer of the foam silk protein membrane with the preset number of layers is composed of silk protein containing gas, and can expand and contract accordingly when the external pressure changes. Applying this material to a pressure sensor can make the pressure sensor have the advantages of good biocompatibility, non-biological toxicity, no rejection reaction, in vivo degradability, flexibility, adjustable mechanical properties, in vivo degradability and no need for secondary surgery to remove.

[0080] As an optional implementation, the auxiliary film includes a water-insoluble polyvinyl alcohol film. In the above step S10, providing a preset number of layers of auxiliary films includes:

[0081] Two layers of water-insoluble polyvinyl alcohol film are provided.

[0082] In the above step S70, the foamed silk protein solution is injected between adjacent auxiliary films in a preset number of layers of auxiliary films, and a preset spacing is maintained between adjacent auxiliary films to obtain a preset foamed silk protein film, including:

[0083] The foamed silk protein solution is injected between two layers of water-insoluble polyvinyl alcohol films, and a preset distance is maintained between the two layers of water-insoluble polyvinyl alcohol films to obtain a preset foamed silk protein film.

[0084] In the above step S90, the above-mentioned drying treatment and cross-linking treatment are performed on the preset foam silk protein film to obtain a foam silk protein film with a preset number of layers, including:

[0085] The preset foamed silk protein membrane is dried and cross-linked to obtain a three-layer foamed silk protein membrane. The three-layered foamed silk protein membrane comprises a polyvinyl alcohol film layer, a foam layer and a polyvinyl alcohol film layer from top to bottom.

[0086] As an optional implementation manner, after obtaining the three-layer foam silk protein film, the method further comprises:

[0087] The polyvinyl alcohol film in the three-layer foam silk protein film is peeled off to obtain a single-layer foam silk protein film.

[0088] For example, polyvinyl alcohol film (PVA film) is selected as the auxiliary film because it has the characteristic of being able to absorb water and can dehydrate and dry the inner protein solution while maintaining the distance between the two layers.

[0089] When a single-layer foam silk protein membrane is synthesized according to actual application requirements, a PVA membrane is selected as an auxiliary membrane. The specific synthesis steps are slightly different from the above process, specifically:

[0090] In the above step S10, the preset number of layers is two layers, specifically providing two layers of water-insoluble polyvinyl alcohol films;

[0091] The above steps S30-S50 remain unchanged to prepare a foamed silk protein solution;

[0092] Then, the foamed silk protein solution is injected between two layers of water-insoluble polyvinyl alcohol films, and a preset distance is maintained between the two layers of water-insoluble polyvinyl alcohol films to obtain a preset foamed silk protein film;

[0093] The preset foamed silk protein membrane is dried and cross-linked to obtain a three-layer foamed silk protein membrane. The three-layered foamed silk protein membrane comprises a polyvinyl alcohol film layer, a foam layer and a polyvinyl alcohol film layer from top to bottom.

[0094] However, since the polyvinyl alcohol film is not degradable in the body and the purpose is to prepare a foamed silk protein film having only a foam layer, after obtaining the three-layer foamed silk protein film, the polyvinyl alcohol film in the three-layer foamed silk protein film is peeled off to obtain Figure 3 The single-layer foam silk protein film shown.

[0095] The embodiment of the present application prepares a foam silk protein membrane containing only a foam layer through a polyvinyl alcohol film. The foam layer of the foam silk protein membrane is composed of silk protein containing gas, and can expand and contract accordingly when the external pressure changes. Applying this material to a pressure sensor can make the pressure sensor have the advantages of good biocompatibility, no biological toxicity, no rejection reaction, biodegradability, flexibility, adjustable mechanical properties, biodegradability in the body, and no need for secondary surgery to remove.

[0096] As an optional implementation manner, the first preset concentration is 5-7% by mass, and the second preset concentration is 15-25% by mass.

[0097] Exemplarily, in order to control the quality of the prepared foam silk protein film, the stability of the foam, the density of the foam, the volume of the foam, etc., the first preset concentration is 5-7% by mass, and the second preset concentration is 15-25% by mass.

[0098] The embodiment of the present application can control the concentration of the silk protein solution to control the quality and characteristics of the formed foamed silk protein solution, thereby ensuring the quality of the prepared foamed silk protein membrane. It not only does not affect its advantages of good biocompatibility, non-biotoxicity, no rejection reaction, in vivo degradability, flexibility, adjustable mechanical properties, in vivo degradability and no need for secondary surgery to remove, but is also more conducive to ensuring its ability to expand and contract accordingly when the external pressure changes, thereby ensuring the performance of devices such as pressure sensors made using it.

[0099] As an optional implementation, the preset spacing is 30 μm-300 μm.

[0100] Exemplarily, the preset distance is controlled in order to control the thickness of a single foam layer in the prepared foam silk protein membrane with a preset number of layers. In practical applications, the thickness is selected according to the degradation time or rate in the actual application, and can be between 30 μm and 300 μm.

[0101] The embodiment of the present application controls the thickness of a single foam layer by controlling the spacing between adjacent auxiliary films, thereby controlling the overall thickness of the foam protein layer, ensuring that the corresponding thickness can be selected according to actual degradation needs or other needs, thereby making the foam silk protein membrane flexible in application and being more conducive to integrating a pressure sensor on the foam silk protein membrane.

[0102] Specific examples are listed below to illustrate the preparation method of this scheme.

[0103] Example 1: When the auxiliary film is a dry and water-insoluble silk protein film, taking the auxiliary film as two layers as an example, a specific example is provided to illustrate the above scheme.

[0104] Step 1: providing two layers of dry and water-insoluble silk protein membranes, and the silk protein membranes are subjected to water annealing treatment;

[0105] Step 2: preparing a silk protein solution with a mass fraction of about 6%, and concentrating the silk protein solution by dialysis to make its mass fraction reach 20%;

[0106] Step 3: using a whipping method to prepare the 20% by mass fraction silk protein solution into a foamed silk protein solution;

[0107] Step 4: injecting the foamed silk protein solution into between two layers of dry and water-insoluble silk protein membranes, and maintaining a distance of 300 μm between the two layers of dry and water-insoluble silk protein membranes, to obtain a preset foamed silk protein membrane;

[0108] Step 5: Dry the preset foam silk protein membrane as a whole, and perform methanol cross-linking treatment on the dried preset foam silk protein membrane to obtain Figure 2 The three-layer structure of the foamed silk protein membrane shown comprises, from top to bottom, a dry and water-insoluble silk protein membrane layer, a foam layer, and a dry and water-insoluble silk protein membrane layer.

[0109] Embodiment 2: When the auxiliary film is a polyvinyl alcohol film, taking the auxiliary film as two layers as an example, a specific embodiment is provided to illustrate the above scheme.

[0110] Step 1: providing two layers of polyvinyl alcohol films;

[0111] Step 2: preparing a silk protein solution with a mass fraction of about 5%, and concentrating the silk protein solution by dialysis to make its mass fraction reach 18%;

[0112] Step 3: introducing microbubbles into the above-mentioned silk protein solution with a mass fraction of 18% to obtain a foamed silk protein solution;

[0113] Step 4: injecting the foamed silk protein solution into between two layers of polyvinyl alcohol films, and maintaining a distance of 300 m between the two layers of dry and water-insoluble silk protein films, to obtain a preset foamed silk protein film;

[0114] Step 5: Dry the preset foam silk protein membrane as a whole, and perform methanol cross-linking treatment on the dried preset foam silk protein membrane to obtain Figure 3 The three-layer structure of the foamed silk protein membrane shown in the figure comprises, from top to bottom, a polyvinyl alcohol film layer, a foam layer, and a polyvinyl alcohol film layer;

[0115] Step 6: Peel off the polyvinyl alcohol film layers on the upper and lower surfaces of the foam layer to obtain a single-layer foam silk protein film.

[0116] On the other hand, an embodiment of the present application further provides a foam silk protein membrane, which is prepared by the above method.

[0117] In the embodiment of the present application, the foam layer in the foam silk protein membrane obtained by the above method is composed of silk protein foam containing gas, and can expand and contract accordingly when the external pressure changes. Applying this material to a pressure sensor can make the pressure sensor have the advantages of good biocompatibility, non-biological toxicity, no rejection reaction, biodegradability, flexibility, adjustable mechanical properties, biodegradability in the body, and no need for secondary surgery to remove.

[0118] On the other hand, an embodiment of the present application also provides a pressure sensor based on a foam silk protein membrane, characterized in that the pressure sensor includes the above-mentioned foam silk protein membrane and a conductive structure; the conductive structure is used for impedance testing.

[0119] In an embodiment of the present application, the foam silk protein membrane can be used for a pressure sensor, which also includes a conductive structure. The conductive structure is used for impedance testing, that is, for obtaining transmembrane impedance. The conductive structure can be arranged on the surface of the foam silk protein membrane, or in the middle of the foam silk protein membrane, and on this basis, the external pressure corresponding to the monitored impedance value can be confirmed by a calibration method. The pressure sensor based on the foam silk protein membrane can sense the external pressure by preparing structures such as capacitors and resistors on the surface of the foam silk protein membrane or by adding conductive components inside the foam silk protein membrane, by detecting its electrical properties. And due to the high biocompatibility of silk protein materials, the pressure sensor can be implanted in the body for use. Figure 4-Figure 7 As shown, the pressure sensor based on foam silk protein film can monitor not only the surface impedance but also the transmembrane impedance.

[0120] Optionally, the conductive structure includes but is not limited to conductive components or structures such as capacitors and resistors.

[0121] Optionally, the conductive component includes but is not limited to graphene, carbon nanotubes, a composite of poly(3,4-ethylenedioxythiophene) and poly(styrene sulfonate) (PEDOT:PSS), and the like.

[0122] The pressure sensor based on foam silk protein membrane disclosed in the embodiment of the present application utilizes the property that the foam layer in the foam silk protein membrane can expand and contract accordingly when the external pressure changes to perform pressure testing, and has the advantages of good biocompatibility, no biological toxicity, no rejection reaction, biodegradability in vivo, flexibility, adjustable mechanical properties, biodegradability in vivo and no need for secondary surgery to remove.

[0123] On the other hand, the embodiment of the present application also provides a method for preparing a pressure sensor based on a foamed silk protein film, characterized in that the method comprises:

[0124] Prepare a conductive structure on the surface of a preset number of layers of foam silk protein film; and / or

[0125] Conductive materials are doped into a preset number of layers of foam silk protein membrane to obtain a pressure sensor based on the foam silk protein membrane.

[0126] For example, a schematic diagram of a typical pressure sensor based on foam silk protein membrane prepared according to an embodiment of the present application is as follows: Figure 4-Figure 7 Doping conductive substances inside the foamed silk protein membrane with a preset number of layers refers to doping conductive structures in the foam layer, and the specific doping concentration and doping method are not limited in the embodiments of the present application.

[0127] Optionally, at least one of an upper surface and a lower surface is prepared on the surface of the foamed silk protein membrane with a preset number of layers.

[0128] Optionally, the conductive component includes but is not limited to graphene, carbon nanotubes, a composite of poly(3,4-ethylenedioxythiophene) and poly(styrene sulfonate) (PEDOT:PSS), and the like.

[0129] Specifically, Figure 4 A pressure sensor obtained by preparing a conductive structure on the surface of the three-layer foam silk protein film prepared in Example 1; Figure 5 A pressure sensor obtained by preparing a conductive structure on the surface of the single-layer foam silk protein film prepared in Example 2; Figure 6 A pressure sensor is obtained by doping a conductive substance inside the three-layer foam silk protein membrane prepared in Example 1; Figure 7 A pressure sensor is obtained by doping a conductive substance inside the single-layer foam silk protein membrane prepared in Example 2. The pressure sensor based on the foam silk protein membrane can monitor not only the surface impedance but also the transmembrane impedance.

[0130] The pressure sensor based on the foam silk protein membrane provided in the embodiment of the present application can be used to record the pressure in the intracranial, blood vessels, bladder and other locations.

[0131] The present application also provides a specific embodiment for illustrating the specific application of the above-mentioned pressure sensor based on foam silk protein membrane:

[0132] Embodiment 3:

[0133] Step 1: preparing a patterned metal conductive structure on the upper and lower surfaces of the foam silk protein film with a preset number of layers by electron beam metal evaporation to obtain a pressure sensor based on the foam silk protein film;

[0134] Step 2: Pull out the patterned metal conductive structure to monitor the electrical properties such as impedance at both ends of the foam silk protein film;

[0135] Step 3: After immersing the sensor in water or phosphate buffer solution (PBS solution) and absorbing the solution and wetting it, the sensor is placed in a pressure-controlled environment for calibration to obtain a table of electrical parameters corresponding to different pressures;

[0136] Step 4: Implant the sensor into the skull and lead out the wires at both ends. After the skull is sealed, the intracranial pressure can still be monitored and recorded through the wires.

[0137] The embodiment of the present application prepares a pressure sensor based on a foam silk protein membrane through the above method. The pressure sensor utilizes the property that the foam layer in the foam silk protein membrane can expand and contract accordingly when the external pressure changes to perform pressure testing. The pressure sensor has the advantages of good biocompatibility, no biological toxicity, no rejection reaction, biodegradability, flexibility, adjustable mechanical properties, biodegradability in the body, and no need for secondary surgery to remove.

[0138] It should be noted that the above-mentioned sequence of the embodiments of the present application is for description only and does not represent the advantages and disadvantages of the embodiments. The above-mentioned specific embodiments of this specification are described. Other embodiments are within the scope of the attached claims. In some cases, the actions or steps recorded in the claims can be performed in an order different from that in the embodiments and still achieve the desired results. In addition, the processes depicted in the drawings do not necessarily require the specific order or continuous order shown to achieve the desired results. In some embodiments, multitasking and parallel processing are also possible or may be advantageous.

[0139] Each embodiment in this specification is described in a progressive manner, and the same or similar parts between the embodiments can be referred to each other, and each embodiment focuses on the differences from other embodiments. In particular, for the device embodiment, since it is basically similar to the method embodiment, the description is relatively simple, and the relevant parts can be referred to the partial description of the method embodiment.

[0140] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present application should be included in the protection scope of the present application.

Claims

1. A method for preparing a foamed silk protein film, characterized in that: The method comprises: Providing a preset number of layers of auxiliary film; Preparing a silk fibroin solution of a first preset concentration, and concentrating the first silk fibroin solution of a first preset concentration to obtain a silk fibroin solution of a second preset concentration; performing foaming treatment on the silk fibroin solution of the second preset concentration to obtain a foamed silk fibroin solution; Injecting the foamed silk protein solution between adjacent auxiliary films in the preset number of layers of auxiliary films, and maintaining a preset distance between the adjacent auxiliary films, to obtain a preset foamed silk protein film; The preset foamed silk protein membrane is dried and cross-linked to obtain a foamed silk protein membrane with a preset number of layers.

2. The method according to claim 1, characterized in that The auxiliary film comprises a dry and water-insoluble silk protein film, and the method of providing a preset number of layers of the auxiliary film comprises: Providing a preset number of layers of the dry and water-insoluble silk protein membrane, wherein the dry and water-insoluble silk protein membrane has been cross-linked in advance; The step of injecting the foamed silk protein solution between adjacent auxiliary films in the preset number of layers of auxiliary films and maintaining a preset distance between the adjacent auxiliary films to obtain a preset foamed silk protein film comprises: The foamed silk protein solution is injected between adjacent dry and water-insoluble silk protein membranes in the preset number of layers of dry and water-insoluble silk protein membranes, and a preset distance is maintained between the adjacent dry and water-insoluble silk protein membranes to obtain a preset foamed silk protein membrane.

3. The method according to claim 1, characterized in that The auxiliary film comprises a water-insoluble polyvinyl alcohol film, and the method of providing a preset number of layers of the auxiliary film comprises: providing two layers of water-insoluble polyvinyl alcohol films; The step of injecting the foamed silk protein solution between adjacent auxiliary films in the preset number of layers of auxiliary films and maintaining a preset distance between the adjacent auxiliary films to obtain a preset foamed silk protein film comprises: Injecting the foamed silk protein solution between the two layers of water-insoluble polyvinyl alcohol films, and maintaining a preset distance between the two layers of water-insoluble polyvinyl alcohol films, to obtain a preset foamed silk protein film; The step of drying and cross-linking the preset foamed silk protein membrane to obtain a foamed silk protein membrane with a preset number of layers comprises: The preset foamed silk protein membrane is dried and cross-linked to obtain a three-layer foamed silk protein membrane, wherein the three-layered foamed silk protein membrane comprises a polyvinyl alcohol film layer, a foam layer and the polyvinyl alcohol film layer in order from top to bottom.

4. The method according to claim 3, characterized in that After obtaining the foamed silk fibroin film with a three-layer structure, the method further comprises: The polyvinyl alcohol film in the three-layer foamed silk fibroin film is peeled off to obtain a single-layer foamed silk fibroin film.

5. The method according to claim 1, characterized in that The step of processing the second silk protein solution of the preset concentration to obtain a foamed silk protein solution comprises: Stirring the second silk protein solution of the preset concentration and controlling the stirring conditions to obtain a foam silk protein solution of a preset foam size comprises: and / or, Microbubbles are introduced into the second silk protein solution of the preset concentration, and the conditions for introducing the microbubbles are controlled to obtain the foam silk protein solution of the preset foam size.

6. The method according to claim 1, characterized in that The first preset concentration is 5-7% by mass, and the second preset concentration is 15-25% by mass.

7. The method according to claim 1, characterized in that The preset spacing is 30 μm-300 μm.

8. A foamed silk protein membrane, characterized in that: The foamed silk protein membrane is prepared by the method according to any one of claims 1 to 7.

9. A pressure sensor based on foamed silk protein membrane, characterized in that: The pressure sensor comprises the foam silk protein membrane as claimed in claim 8 and a conductive structure; the conductive structure is used for impedance testing.

10. A method for preparing a pressure sensor based on foamed silk protein membrane according to claim 9, characterized in that: The method comprises: Prepare a conductive structure on the surface of a preset number of layers of foam silk protein film; and / or Conductive materials are doped inside the foam silk protein membrane with a preset number of layers to obtain the foam silk protein membrane-based pressure sensor.

Citation Information

Patent Citations

  • Preparation method of silk fibroin aerogel

    CN106178131A

  • Protein-based biomaterial having viscoelastic behavior, method for obtaining same and use thereof

    CN114599407A

  • High-stability alcohol-resistant silk-I structure fibroin material and preparation method thereof

    CN118027443A