High-performance single-component polyurethane sealant and preparation method thereof

By using multiple self-healing polyurethane prepolymer and active hydrogen components in polyurethane sealant, the problem of low self-repair efficiency of polyurethane sealant at low temperature is solved, achieving efficient, rapid self-repair and excellent durability and UV resistance.

CN119081629APending Publication Date: 2024-12-06CHONGQINGSHI ZHIXIANG PAVING TECH ENG CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411444765.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-16
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Existing polyurethane sealants require higher temperatures and longer time when self-repairing, making it difficult to quickly self-repair at lower temperatures.

Method used

Using a combination of multiple self-healing polyurethane prepolymers and active hydrogen components, a high-performance single group is formed through the synergistic action of hyperbranched polyether polyols, polyisocyanate microcapsules, imine bond additives and disulfide bond additives. Part of polyurethane sealant can achieve efficient self-healing at room temperature of 30-40℃.

Benefits of technology

A self-repair rate of more than 98% is achieved at room temperature, with a repair time less than 90 minutes, and the durability and UV resistance of the material are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119081629A_ABST
    Figure CN119081629A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of adhesives of polyurethane, and discloses a high-performance single-component polyurethane sealant which comprises a component A, namely a multi-self-healing polyurethane prepolymer, and a component B, namely reactive hydrogen, the component A is prepared from hyperbranched polyether polyol, polyisocyanate, isocyanate microcapsules, an imine bond auxiliary agent and a disulfide bond auxiliary agent, and the component B is prepared from hyperbranched polyether polyol, polyisocyanate, isocyanate microcapsules, an imine bond auxiliary agent and a disulfide bond auxiliary agent. The mass part ratio of the component A to the component B is 5: (1-2). The material has the advantage of rapid self-repairing at a relatively low temperature.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polyurethane adhesives, and in particular to a high-performance one-component polyurethane sealant. Background Art

[0002] One-component polyurethane specifically refers to polyurethane resin with terminal NCO groups, which means that no curing agent needs to be added when used. The resin can be directly applied to the required position and exposed to the air, where it reacts with trace moisture in the air and solidifies to produce polymers with excellent properties.

[0003] One-component polyurethane sealant is a solvent-free, one-component, room temperature curing sealant. The sealant is in paste form and can be extruded or applied. It has anti-sagging properties and fills vertical joints and top joints without flowing. The cured adhesive layer is rubbery and elastic. It has adhesion to metal, rubber, wood, cement components, ceramics, glass, etc. Sealant is a material used to fill gaps (holes, joints, seams, etc.), and has both bonding and sealing functions.

[0004] Chinese patent document CN105331323B discloses a polyurethane sealant and its preparation method and application, which is prepared by mixing component A and component B in a ratio of 1:1 to 5, wherein component A comprises the following raw materials in parts by weight: 60 to 75 parts of polyether polyol, 20 to 35 parts of toluene-2,4-diisocyanate, and 1 to 20 parts of plasticizer; component B comprises the following raw materials in parts by weight: 25 to 55 parts of liquid filler, 40 to 60 parts of inorganic powder filler, 1 to 10 parts of auxiliary agent, and 1 to 25 parts of curing agent; the curing agent comprises at least one of 4,4′-bis-sec-butylaminodiphenylmethane and 1,4-bis-sec-butylaminobenzene, or a mixture of two of them.

[0005] Chinese patent document CN113817119A discloses a method for preparing a self-healing waterborne polyurethane with synergistic effects of disulfide bonds and multiple hydrogen bonds, a self-healing waterborne polyurethane containing disulfide bonds and multiple hydrogen bonds, the raw materials include by weight: 10-34 parts of isophorone diisocyanate, 30-50 parts of polycarbonate diol, 3-5 parts of dimethylol propionic acid DMPA, 0.08-1 parts of dibutyltin dilaurate, 2.6-3.7 parts of triethylamine, 0-8.2 parts of disulfide bond chain extender, 0-7.6 parts of quadruple hydrogen bond UPy, and the molecular weight Mn of the polycarbonate diol is 1000; the sample is self-healed in a thermostat at 80°C. The surface scratches become significantly lighter after 6 hours of healing, and the surface scratches basically disappear after 12 hours of healing.

[0006] Current polyurethane sealants are widely used in sealing, insulating and filling joints, gaps and cracks, covering civil engineering, construction, transportation and other fields. However, the sealants require higher temperatures and longer times for self-repair. Summary of the invention

[0007] In order to solve the technical problem of how to quickly self-repair self-healing materials at a lower temperature, the present invention provides a high-performance one-component polyurethane sealant, which is characterized by comprising a component A of multiple self-healing polyurethane prepolymers and a component B of active hydrogen, wherein the component A is prepared from a hyperbranched polyether polyol, a polyisocyanate, an isocyanate microcapsule, an imide bond additive and a disulfide bond additive.

[0008] Furthermore, the mass ratio of component A to component B is 5:1~2.

[0009] Furthermore, the mass ratio of the hyperbranched polyether polyol, polyisocyanate, isocyanate microcapsule, imide bond auxiliary agent and disulfide bond auxiliary agent in component A is 80-100:150-200:3-5:20-30:10-15.

[0010] Furthermore, the isocyanate microcapsules are wrapped with nano-silicon dioxide / polyethylene wax / polyvinyl alcohol composite wall materials.

[0011] Furthermore, component B is prepared from polyether polyol, inorganic filler, toughening agent, adhesion promoter, defoaming agent and carbon nanomaterial.

[0012] Furthermore, the mass ratio of the polyether polyol, the inorganic filler, the toughening agent, the adhesion promoter, the defoaming agent and the carbon nanomaterial in component B is 20-30:15-20:3-10:1-3:0.5-1:0.05-0.2.

[0013] A method for preparing a high-performance one-component polyurethane sealant comprises the following steps: Step 1: Preparation of component A: Heat the hyperbranched polyether polyol to remove water, add polyisocyanate under the protection of inert gas and mix evenly, then add a non-protonic polar solvent, an imide bond-containing chain extender and a disulfide bond-containing chain extender and mix evenly, and finally, add isocyanate microcapsules to obtain a multiple self-healing polyurethane prepolymer, which is component A; Step 2: Preparation of component B: dehydrate the polyether polyol at high temperature, add inorganic filler, toughening agent, adhesion promoter, defoamer, and carbon nanomaterial, mix well and remove bubbles to obtain active hydrogen component, which is component B; Step 3: Evenly mix component A and component B at a weight ratio of 5:1-2 to obtain a high-performance one-component polyurethane sealant.

[0014] Furthermore, in step 1, component A is prepared by heating the hyperbranched polyether polyol to remove water, adding polyisocyanate under the protection of inert gas, stirring continuously, then adding a non-protonic polar solvent, an imide bond-containing chain extender and a disulfide bond-containing chain extender, heating and stirring continuously, and finally adding isocyanate microcapsules and stirring continuously to obtain a multiple self-healing polyurethane prepolymer, which is component A.

[0015] Further, in step 2, component B is prepared by removing water from the polyether polyol at high temperature, cooling to room temperature, adding inorganic fillers, toughening agents, adhesion promoters, defoaming agents, and carbon nanomaterials, stirring evenly, and removing bubbles under vacuum to obtain active hydrogen components, namely component B. Furthermore, preparation of isocyanate microcapsules: after the polyvinyl alcohol is completely melted, polyethylene wax is added, stirring continuously and keeping the temperature constant, then isocyanate-modified nano titanium dioxide is added, stirring continuously, and then polyisocyanate is added, stirring evenly, heating is stopped, coolant is added, stirring continuously, and a suspension of nano-silica / polyethylene wax / polyvinyl alcohol-encapsulated isocyanate microcapsules is obtained. When the temperature of the mixture drops to room temperature, ultrasonic oscillation is used, filtration and centrifugation are performed, and drying is performed to obtain nano-silica / polyethylene wax / polyvinyl alcohol composite wall material-encapsulated isocyanate microcapsules, i.e., isocyanate microcapsules.

[0016] The present invention has the following beneficial effects: 1. In the self-repairing process of the present invention, the rupture of the microcapsule will promote the exchange reaction of the disulfide bonds in the material, and accelerate the exchange reaction of the imine bonds. Through the synergistic effect of these multiple actions, the present invention can efficiently achieve repeated self-repairing capabilities at room temperature 30-40°C, with a repair rate of more than 98% and the time required being less than 90 minutes.

[0017] 2. Using isocyanate-functionalized titanium dioxide as raw material, nano-silica / polyethylene wax / polyvinyl alcohol composite wall material encapsulated isocyanate microcapsules were successfully prepared. Functionalized nano-titanium dioxide can react with polyether polyols to achieve uniform dispersion in the matrix, thus giving the material excellent durability and UV resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 This is a schematic diagram of the high-performance one-component polyurethane sealant of the present invention before self-repair; Figure 2 It is a schematic diagram of the high-performance one-component polyurethane sealant after self-repair of the present invention. DETAILED DESCRIPTION

[0019] The following is further described in detail through specific implementation methods: 1. Definition Polyether polyol (abbreviated as polyether) is an organic polymer, which is obtained by polyaddition reaction of initiator (compound containing active hydrogen group) with ethylene oxide (EO), propylene oxide (PO), butylene oxide (BO) etc. in the presence of catalyst. The largest polyether production is produced by using glycerol (glycerol) as initiator and epoxide (generally PO and EO are used together). By changing the feeding method of PO and EO (mixed or separate), feeding ratio, feeding order and other conditions, various general-purpose polyether polyols are produced.

[0020] Isocyanate is a general term for various esters of isocyanic acid, which are used in household appliances, automobiles, construction, footwear, furniture, adhesives and other industries. If classified by the number of -NCO groups, it includes monoisocyanate R-N=C=O, diisocyanate O=C=N-R-N=C=O and polyisocyanate.

[0021] Polyisocyanate molecules contain two or more active sites, so when polymerization occurs, they can be extended to two or three ends to form linear or cross-linked (stereotype) polymers. The industrial preparation of polyisocyanates is achieved by the reaction of primary amines with phosgene. Among polyisocyanates, the most commonly used are TDI, MDI and PAPI. TDI has 2,4-TDI and 2,6-TDI, which are isomers of each other, and the commonly used TDI is a mixture of them. TDI has the advantages of high activity and low price, but it is relatively volatile, irritating and toxic. At low temperatures, the isocyanate group on the para position of the methyl group is much more active than the one on the ortho position.

[0022] A high-performance one-component polyurethane sealant, comprising component A, a multiple self-healing polyurethane prepolymer and component B, active hydrogen, wherein: Component A is prepared from hyperbranched polyether polyol, polyisocyanate, isocyanate microcapsule, aprotic polar solvent, imine bond auxiliary agent and disulfide bond auxiliary agent, and the mass ratio of hyperbranched polyether polyol, polyisocyanate, isocyanate microcapsule, aprotic polar solvent, imine bond auxiliary agent and disulfide bond auxiliary agent is 80-100:150-200:3-5:10-20:20-30:10-15, and the mass ratio in component A is only for the raw materials of component A and does not affect other ratios; Component B is prepared from polyether polyol, inorganic filler, toughening agent, adhesion promoter, defoaming agent and carbon nanomaterial. The mass ratio of polyether polyol, inorganic filler, toughening agent, adhesion promoter, defoaming agent and carbon nanomaterial is 20-30:15-20:3-10:1-3:0.5-1:0.05-0.2. The mass ratio in component B is only for the raw materials of component B and does not affect other ratios.

[0023] Polyisocyanate: at least one of hexamethylene diisocyanate, toluene-2,4-diisocyanate, and 4,4'-diphenylmethane diisocyanate; Polyether polyol: at least one of polyether polyol LE-220A, polyether polyol LEP-330N and polyether polyol 5603; Aprotic polar solvent: at least one of N,N-dimethylformamide, dimethyl sulfoxide, and acetonitrile; Adhesion promoter: at least one of oligomer siloxane, aminosiloxane, and vinyl oligomer siloxane; Inorganic filler: at least one of aerosil, nano calcium carbonate, kaolin, etc.; Defoamer: silicone defoamer; Toughening agent: at least one of dioctyl phthalate, tricresyl phosphate, and dibutyl phthalate; Carbon nanomaterial: at least one of graphene, carbon nanotubes, graphene oxide, etc.

[0024] Example 1 A method for preparing a high-performance one-component polyurethane sealant comprises the following steps: Step 1, preparation of isocyanate-modified nano titanium dioxide: weigh 15 grams of nano titanium dioxide particles and pre-dry them in an oven at 120°C for 1 hour, dissolve them in 100 grams of aprotic polar solvent by ultrasound, drip 30 grams of isocyanate into the reaction solution drop by drop, and continue stirring at room temperature for 2 hours. The isocyanate group has been successfully connected to the surface of the nano titanium dioxide, and centrifugal drying is performed to obtain isocyanate-modified nano titanium dioxide particles (TiO2-NCO), and 2 grams of isocyanate-modified nano titanium dioxide particles are taken for standby use; Step 2, preparation of isocyanate microcapsules: weigh 15 grams of polyvinyl alcohol and put it into a flask, heat it to 200°C, and after the polyvinyl alcohol is completely melted, add 15 grams of polyethylene wax, continue stirring for 30 minutes and keep the temperature unchanged, then add 2 grams of isocyanate-modified nano titanium dioxide, continue stirring for 1 hour, then weigh 80 grams of polyisocyanate, stir evenly for 3 hours, finally, turn off the heating device, add 800 grams of coolant to the flask, continue stirring for 30 minutes, and obtain a suspension of nano-silica / polyethylene wax / polyvinyl alcohol-encapsulated isocyanate microcapsules. When the temperature of the mixture drops to room temperature, use ultrasonic oscillation for 30 minutes, filter and centrifuge, and dry in a vacuum drying oven at 40 degrees for 24 hours to obtain nano-silica / polyethylene wax / polyvinyl alcohol composite wall material-encapsulated isocyanate microcapsules, i.e., isocyanate microcapsules. Take 3 grams of isocyanate microcapsules for standby use; Step 3, preparation of component A: weigh 80 grams of hyperbranched polyether polyol and heat at 120°C to remove water for 2 hours, then reduce the temperature to 80°C, add 150 grams of polyisocyanate under nitrogen protection, continue stirring for 1 hour, then reduce the temperature to 60°C, add 10 grams of aprotic polar solvent, 20 grams of imide bond-containing chain extender and 10 grams of disulfide bond-containing chain extender, heat to 75°C, continue stirring and react for 4 hours, finally, add 3 grams of isocyanate microcapsules, continue stirring for 1 hour, and obtain a multiple self-healing polyurethane prepolymer, which is component A; Step 4, preparation of component B: weigh 20 grams of polyether polyol and add it to a flask, remove water at high temperature for 2 hours, cool to room temperature, then add 15 grams of inorganic filler, 3 grams of toughening agent, 1 gram of adhesion promoter, 0.5 grams of defoaming agent, and 0.05 grams of carbon nanomaterial, stir evenly, remove bubbles under vacuum to obtain active hydrogen component, which is component B; Step 5: Evenly mix component A and component B at a weight ratio of 5:1 at room temperature to obtain a single-component high-performance multiple self-healing polyurethane sealant.

[0025] Example 2 A method for preparing a high-performance one-component polyurethane sealant comprises the following steps: Step 1, preparation of isocyanate-modified nano titanium dioxide: weigh 15 grams of nano titanium dioxide particles and pre-dry them in an oven at 120°C for 1 hour, dissolve them in 100 grams of aprotic polar solvent by ultrasound, drip 30 grams of isocyanate into the reaction solution drop by drop, and continue stirring at room temperature for 2 hours. The isocyanate group has been successfully connected to the surface of the nano titanium dioxide, and centrifugal drying is performed to obtain isocyanate-modified nano titanium dioxide particles (TiO2-NCO), and 2 grams of isocyanate-modified nano titanium dioxide particles are taken for standby use; Step 2, preparation of isocyanate microcapsules: weigh 15 grams of polyvinyl alcohol and put it into a flask, heat it to 200°C, and after the polyvinyl alcohol is completely melted, add 15 grams of polyethylene wax, continue stirring for 30 minutes and keep the temperature unchanged, then add 2 grams of isocyanate-modified nano titanium dioxide, continue stirring for 1 hour, then weigh 80 grams of polyisocyanate, stir evenly for 3 hours, finally, turn off the heating device, add 800 grams of coolant to the flask, continue stirring for 30 minutes, and obtain a suspension of nano-silica / polyethylene wax / polyvinyl alcohol-encapsulated isocyanate microcapsules. When the temperature of the mixture drops to room temperature, use ultrasonic oscillation for 30 minutes, filter and centrifuge, and dry in a vacuum drying oven at 40 degrees for 24 hours to obtain nano-silica / polyethylene wax / polyvinyl alcohol composite wall material-encapsulated isocyanate microcapsules, i.e., isocyanate microcapsules, and take 5 grams of isocyanate microcapsules for standby use; Step 3, preparation of component A: weigh 100 grams of hyperbranched polyether polyol and heat it at 120°C to remove water for 2 hours, then reduce the temperature to 80°C, add 200 grams of polyisocyanate under nitrogen protection, continue stirring for 1 hour, then reduce the temperature to 60°C, add 20 grams of aprotic polar solvent, 30 grams of imide bond-containing chain extender and 15 grams of disulfide bond-containing chain extender, heat to 75°C, continue stirring and react for 4 hours, finally, add 5 grams of isocyanate microcapsules, continue stirring for 1 hour, and obtain a multiple self-healing polyurethane prepolymer, which is component A; Step 4, preparation of component B: weigh 30 grams of polyether polyol and add it to a flask, remove water at high temperature for 2 hours, cool to room temperature, then add 20 grams of inorganic filler, 10 grams of toughening agent, 3 grams of adhesion promoter, 1 gram of defoaming agent, 0.2 grams of carbon nanomaterial, stir evenly, remove bubbles under vacuum to obtain active hydrogen component, which is component B; Step 5: Evenly mix component A and component B at a weight ratio of 5:2 at room temperature to obtain a single-component high-performance multiple self-healing polyurethane sealant.

[0026] Example 3 A method for preparing a high-performance one-component polyurethane sealant comprises the following steps: Step 1, preparation of isocyanate-modified nano titanium dioxide: weigh 15 grams of nano titanium dioxide particles and pre-dry them in an oven at 120°C for 1 hour, dissolve them in 100 grams of aprotic polar solvent by ultrasound, drip 30 grams of isocyanate into the reaction solution drop by drop, and continue stirring at room temperature for 2 hours. The isocyanate group has been successfully connected to the surface of the nano titanium dioxide, and centrifugal drying is performed to obtain isocyanate-modified nano titanium dioxide particles (TiO2-NCO), and 2 grams of isocyanate-modified nano titanium dioxide particles are taken for standby use; Step 2, preparation of isocyanate microcapsules: weigh 15 grams of polyvinyl alcohol and put it into a flask, heat it to 200°C, and after the polyvinyl alcohol is completely melted, add 15 grams of polyethylene wax, continue stirring for 30 minutes and keep the temperature unchanged, then add 2 grams of isocyanate-modified nano titanium dioxide, continue stirring for 1 hour, then weigh 80 grams of polyisocyanate, stir evenly for 3 hours, finally, turn off the heating device, add 800 grams of coolant to the flask, continue stirring for 30 minutes, and obtain a suspension of nano-silica / polyethylene wax / polyvinyl alcohol-encapsulated isocyanate microcapsules. When the temperature of the mixture drops to room temperature, use ultrasonic oscillation for 30 minutes, filter and centrifuge, and dry in a vacuum drying oven at 40 degrees for 24 hours to obtain nano-silica / polyethylene wax / polyvinyl alcohol composite wall material-encapsulated isocyanate microcapsules, i.e., isocyanate microcapsules, and take 4 grams of isocyanate microcapsules for standby use; Step 3, preparation of component A: weigh 90 grams of hyperbranched polyether polyol and heat at 120° C. to remove water for 2 hours, then reduce the temperature to 80° C., add 170 grams of polyisocyanate under nitrogen protection, continue stirring for 1 hour, then reduce the temperature to 60° C., add 15 grams of aprotic polar solvent, 25 grams of imide bond-containing chain extender and 13 grams of disulfide bond-containing chain extender, heat to 75° C., continue stirring and react for 4 hours, finally, add 4 grams of isocyanate microcapsules, continue stirring for 1 hour, and obtain a multiple self-healing polyurethane prepolymer, which is component A; Step 4, preparation of component B: weigh 25 grams of polyether polyol and add it to a flask, remove water at high temperature for 2 hours, cool to room temperature, then add 17 grams of inorganic filler, 6 grams of toughening agent, 2 grams of adhesion promoter, 0.7 grams of defoaming agent, and 0.1 grams of carbon nanomaterial, stir evenly, remove bubbles under vacuum to obtain active hydrogen component, which is component B; Step 5: Evenly mix component A and component B at a weight ratio of 5:1.5 at room temperature to obtain a single-component high-performance multiple self-healing polyurethane sealant.

[0027] Comparative Example 1 A method for preparing a one-component polyurethane sealant comprises the following steps: Step 1, preparation of isocyanate-modified nano titanium dioxide: weigh 15 grams of nano titanium dioxide particles and pre-dry them in an oven at 120°C for 1 hour, dissolve them in 100 grams of aprotic polar solvent by ultrasound, drip 30 grams of isocyanate into the reaction solution drop by drop, and continue stirring at room temperature for 2 hours. The isocyanate group has been successfully connected to the surface of the nano titanium dioxide, and centrifugal drying is performed to obtain isocyanate-modified nano titanium dioxide particles (TiO2-NCO), and 2 grams of isocyanate-modified nano titanium dioxide particles are taken for standby use; Step 2, preparation of isocyanate microcapsules: weigh 15 grams of polyvinyl alcohol and put it into a flask, heat it to 200°C, and after the polyvinyl alcohol is completely melted, add 15 grams of polyethylene wax, continue stirring for 30 minutes and keep the temperature unchanged, then add 2 grams of isocyanate-modified nano titanium dioxide, continue stirring for 1 hour, then weigh 80 grams of polyisocyanate, stir evenly for 3 hours, finally, turn off the heating device, add 800 grams of coolant to the flask, continue stirring for 30 minutes, and obtain a suspension of nano-silica / polyethylene wax / polyvinyl alcohol-encapsulated isocyanate microcapsules. When the temperature of the mixture drops to room temperature, use ultrasonic oscillation for 30 minutes, filter and centrifuge, and dry in a vacuum drying oven at 40 degrees for 24 hours to obtain nano-silica / polyethylene wax / polyvinyl alcohol composite wall material-encapsulated isocyanate microcapsules, i.e., isocyanate microcapsules, and take 4 grams of isocyanate microcapsules for standby use; Step 3, preparation of component A: weigh 90 grams of hyperbranched polyether polyol and heat at 120°C to remove water for 2 hours, then reduce the temperature to 80°C, add 170 grams of polyisocyanate under nitrogen protection, continue stirring for 1 hour, then reduce the temperature to 60°C, add 15 grams of aprotic polar solvent, raise the temperature to 75°C, continue stirring and react for 4 hours, finally, add 4 grams of isocyanate microcapsules, continue stirring for 1 hour, and obtain component A; Step 4, preparation of component B: weigh 25 grams of polyether polyol and add it to a flask, remove water at high temperature for 2 hours, cool to room temperature, then add 17 grams of inorganic filler, 6 grams of toughening agent, 2 grams of adhesion promoter, 0.7 grams of defoaming agent, and 0.1 grams of carbon nanomaterial, stir evenly, remove bubbles under vacuum to obtain active hydrogen component, which is component B; Step 5: Evenly mix component A and component B at a weight ratio of 5:1.5 at room temperature to obtain a one-component polyurethane sealant.

[0028] Comparative Example 2 A method for preparing a one-component polyurethane sealant comprises the following steps: Step 1, preparation of isocyanate-modified nano titanium dioxide: weigh 15 grams of nano titanium dioxide particles, pre-dry them in an oven at 120° C. for 1 hour, dissolve them in 100 grams of aprotic polar solvent by ultrasonication, drip 30 grams of isocyanate into the reaction solution drop by drop, and after continuous stirring at room temperature for 2 hours, the isocyanate group has been successfully connected to the surface of the nano titanium dioxide, centrifuge and dry to obtain isocyanate-modified nano titanium dioxide particles (TiO2-NCO), and take 2 grams of isocyanate-modified nano titanium dioxide particles for standby use; Step 2, preparation of isocyanate microcapsules: weigh 15 grams of polyvinyl alcohol and put it into a flask, heat it to 200°C, and after the polyvinyl alcohol is completely melted, add 15 grams of polyethylene wax, continue stirring for 30 minutes and keep the temperature unchanged, then add 2 grams of isocyanate-modified nano titanium dioxide, continue stirring for 1 hour, then weigh 80 grams of polyisocyanate, stir evenly for 3 hours, finally, turn off the heating device, add 800 grams of coolant to the flask, continue stirring for 30 minutes, and obtain a suspension of nano-silica / polyethylene wax / polyvinyl alcohol-encapsulated isocyanate microcapsules. When the temperature of the mixture drops to room temperature, use ultrasonic oscillation for 30 minutes, filter and centrifuge, and dry in a vacuum drying oven at 40 degrees for 24 hours to obtain nano-silica / polyethylene wax / polyvinyl alcohol composite wall material-encapsulated isocyanate microcapsules, i.e., isocyanate microcapsules, and take 4 grams of isocyanate microcapsules for standby use; Step 3, preparation of component A: weigh 90 grams of hyperbranched polyether polyol and heat at 120° C. to remove water for 2 hours, then reduce the temperature to 80° C., add 170 grams of polyisocyanate under nitrogen protection, continue stirring for 1 hour, then reduce the temperature to 60° C., add 15 grams of aprotic polar solvent and 13 grams of disulfide bond-containing chain extender, raise the temperature to 75° C., continue stirring and react for 4 hours, finally, add 4 grams of isocyanate microcapsules, continue stirring for 1 hour, and obtain a multiple self-healing polyurethane prepolymer, which is component A; Step 4, preparation of component B: weigh 25 grams of polyether polyol and add it to a flask, remove water at high temperature for 2 hours, cool to room temperature, then add 17 grams of inorganic filler, 6 grams of toughening agent, 2 grams of adhesion promoter, 0.7 grams of defoaming agent, and 0.1 grams of carbon nanomaterial, stir evenly, remove bubbles under vacuum to obtain active hydrogen component, which is component B; Step 5: Evenly mix component A and component B at a weight ratio of 5:1.5 at room temperature to obtain a polyurethane sealant.

[0029] Comparative Example 3 A method for preparing a one-component polyurethane sealant comprises the following steps: Step 1, preparation of isocyanate-modified nano titanium dioxide: weigh 15 grams of nano titanium dioxide particles, pre-dry them in an oven at 120° C. for 1 hour, dissolve them in 100 grams of aprotic polar solvent by ultrasonication, drip 30 grams of isocyanate into the reaction solution drop by drop, and after continuous stirring at room temperature for 2 hours, the isocyanate group has been successfully connected to the surface of the nano titanium dioxide, centrifuge and dry to obtain isocyanate-modified nano titanium dioxide particles (TiO2-NCO), and take 2 grams of isocyanate-modified nano titanium dioxide particles for standby use; Step 2, preparation of isocyanate microcapsules: weigh 15 grams of polyvinyl alcohol and put it into a flask, heat it to 200°C, and after the polyvinyl alcohol is completely melted, add 15 grams of polyethylene wax, continue stirring for 30 minutes and keep the temperature unchanged, then add 2 grams of isocyanate-modified nano titanium dioxide, continue stirring for 1 hour, then weigh 80 grams of polyisocyanate, stir evenly for 3 hours, finally, turn off the heating device, add 800 grams of coolant to the flask, continue stirring for 30 minutes, and obtain a suspension of nano-silica / polyethylene wax / polyvinyl alcohol-encapsulated isocyanate microcapsules. When the temperature of the mixture drops to room temperature, use ultrasonic oscillation for 30 minutes, filter and centrifuge, and dry in a vacuum drying oven at 40 degrees for 24 hours to obtain nano-silica / polyethylene wax / polyvinyl alcohol composite wall material-encapsulated isocyanate microcapsules, i.e., isocyanate microcapsules, and take 4 grams of isocyanate microcapsules for standby use; Step 3, preparation of component A: weigh 90 grams of hyperbranched polyether polyol and heat at 120°C to remove water for 2 hours, then reduce the temperature to 80°C, add 170 grams of polyisocyanate under nitrogen protection, continue stirring for 1 hour, then reduce the temperature to 60°C, add 15 grams of aprotic polar solvent and 25 grams of imide bond-containing chain extender, raise the temperature to 75°C, continue stirring and react for 4 hours, finally, add 4 grams of isocyanate microcapsules, continue stirring for 1 hour, and obtain a multiple self-healing polyurethane prepolymer, which is component A; Step 4, preparation of component B: weigh 25 grams of polyether polyol and add it to a flask, remove water at high temperature for 2 hours, cool to room temperature, then add 17 grams of inorganic filler, 6 grams of toughening agent, 2 grams of adhesion promoter, 0.7 grams of defoaming agent, and 0.1 grams of carbon nanomaterial, stir evenly, remove bubbles under vacuum to obtain active hydrogen component, which is component B; Step 5: Evenly mix component A and component B at a weight ratio of 5:1.5 at room temperature to obtain a polyurethane sealant.

[0030] Comparative Example 4 A method for preparing a one-component polyurethane sealant comprises the following steps: Step 1, preparation of component A: weighing 90 grams of hyperbranched polyether polyol, heating at 120° C. to remove water for 2 hours, then reducing the temperature to 80° C., adding 170 grams of polyisocyanate under nitrogen protection, continuously stirring for 1 hour, then reducing the temperature to 60° C., adding 15 grams of aprotic polar solvent, 25 grams of an imide bond-containing chain extender and 13 grams of a disulfide bond-containing chain extender, heating to 75° C., continuously stirring for 4 hours, and obtaining component A; Step 2, preparation of component B: weigh 25 grams of polyether polyol and add it to a flask, remove water at high temperature for 2 hours, cool to room temperature, then add 17 grams of inorganic filler, 6 grams of toughening agent, 2 grams of adhesion promoter, 0.7 grams of defoaming agent, and 0.1 grams of carbon nanomaterial, stir evenly, remove bubbles under vacuum to obtain active hydrogen component, which is component B; Step 3: Mix component A and component B at a weight ratio of 5:1.5 at room temperature to obtain a polyurethane sealant. Table 1 Test results Microcapsules Imine bond Disulfide bond Temperature, °C Time, min Repair rate, % Tensile strength, MPa Tensile strength after repair, MPa Durability, % Example 1 3 g 20g 10g 36 85 98.5 3.8 3.7 99.3 Example 2 2 g 30g 15g 38 90 98.1 3.7 3.6 99.2 Example 3 4 g 25g 13g 33 75 98.3 4.2 4.1 99.4 Comparative Example 1 4 g - - 65 180 82.7 3.6 2.8 99.4 Comparative Example 2 4 g - 13g 75 160 87.5 3.8 3.3 99.4 Comparative Example 3 4 g 25g - 70 170 90.2 3.5 3.2 99.4 Comparative Example 4 - 25g 13g 85 200 85.6 3.6 3.1 97.3 The above data parameters show that the self-healing temperature of the material of the present invention is 30-40°C, the repair rate is more than 98%, the repair time is less than 90 minutes, the mechanical properties of the repaired material are not much different from the original, and the durability of the material containing microcapsules is more than 99%. However, the self-healing environment temperature required for materials containing only microcapsules or microcapsules and imine bonds is as high as 65°C, the repair time is longer, and the repair rate is lower.

[0031] The above is only an embodiment of the present invention. The common sense such as the known specific structure and characteristics in the scheme is not described in detail here. The ordinary technicians in the relevant field know all the common technical knowledge in the technical field of the invention before the application date or priority date, can obtain all the existing technologies in the field, and have the ability to apply the conventional experimental means before that date. The ordinary technicians in the relevant field can improve and implement this scheme in combination with their own abilities under the enlightenment given by this application. Some typical known structures or known methods should not become obstacles for ordinary technicians in the relevant field to implement this application. It should be pointed out that for those skilled in the art, without departing from the structure of the present invention, several deformations and improvements can be made, which should also be regarded as the protection scope of the present invention, which will not affect the effect of the implementation of the present invention and the practicality of the patent. The protection scope required by this application shall be based on the content of its claims, and the specific implementation methods and other records in the specification can be used to interpret the content of the claims.

Claims

1. A high performance one-component polyurethane sealant, It is characterized in that The invention comprises a component A of multiple self-healing polyurethane prepolymer and a component B of active hydrogen, wherein the component A is prepared from hyperbranched polyether polyol, polyisocyanate, isocyanate microcapsule, imine bond auxiliary agent and disulfide bond auxiliary agent.

2. The high performance one-component polyurethane sealant according to claim 1, Features: The mass ratio of component A to component B is 5:1~2.

3. The high performance one-component polyurethane sealant according to claim 1 or 2, Features: The mass ratio of the hyperbranched polyether polyol, polyisocyanate, isocyanate microcapsule, imide bond auxiliary agent and disulfide bond auxiliary agent in component A is 80-100:150-200:3-5:20-30:10-15.

4. The high performance one-component polyurethane sealant according to claim 3, Features: The isocyanate microcapsules are wrapped with nano-silicon dioxide / polyethylene wax / polyvinyl alcohol composite wall materials.

5. The high performance one-component polyurethane sealant according to claim 4, Features: The B component is prepared from polyether polyol, inorganic filler, toughening agent, adhesion promoter, defoaming agent and carbon nanomaterial.

6. The high performance one-component polyurethane sealant according to claim 5, Features: The mass ratio of polyether polyol, inorganic filler, toughening agent, adhesion promoter, defoaming agent and carbon nanomaterial in component B is 20-30:15-20:3-10:1-3:0.5-1:0.05-0.

2.

7. A method for preparing the high-performance one-component polyurethane sealant according to claims 1 to 6, It is characterized in that The following steps are involved: Step 1: Preparation of component A: Heat the hyperbranched polyether polyol to remove water, add polyisocyanate under the protection of inert gas and mix evenly, then add a non-protonic polar solvent, an imide bond-containing chain extender and a disulfide bond-containing chain extender and mix evenly, and finally, add isocyanate microcapsules to obtain a multiple self-healing polyurethane prepolymer, which is component A; Step 2: Preparation of component B: dehydrate the polyether polyol at high temperature, add inorganic filler, toughening agent, adhesion promoter, defoamer, and carbon nanomaterial, mix well and remove bubbles to obtain active hydrogen component, which is component B; Step 3: Evenly mix component A and component B at a weight ratio of 5:1-2 to obtain a high-performance one-component polyurethane sealant.

8. The method for preparing the high-performance one-component polyurethane sealant according to claim 7, Features: In step 1, component A is prepared by heating the hyperbranched polyether polyol to remove water, adding polyisocyanate under the protection of inert gas, stirring continuously, then adding a non-protonic polar solvent, an imide bond-containing chain extender and a disulfide bond-containing chain extender, heating and stirring continuously, and finally adding isocyanate microcapsules and stirring continuously to obtain a multiple self-healing polyurethane prepolymer, which is component A.

9. The method for preparing the high-performance one-component polyurethane sealant according to claim 8, Features: In step 2, component B is prepared by removing water from the polyether polyol at high temperature and cooling to room temperature, then adding inorganic fillers, toughening agents, adhesion promoters, defoaming agents, and carbon nanomaterials, stirring evenly, and removing bubbles under vacuum to obtain an active hydrogen component, which is component B.

10. The method for preparing the high-performance one-component polyurethane sealant according to claim 9, Features: Preparation of isocyanate microcapsules: After the polyvinyl alcohol is completely melted, polyethylene wax is added, stirring continuously and keeping the temperature constant, then isocyanate-modified nano titanium dioxide is added, stirring continuously, and then polyisocyanate is added, stirring evenly, heating is stopped, coolant is added, stirring continuously, and a suspension of nano-silica / polyethylene wax / polyvinyl alcohol-encapsulated isocyanate microcapsules is obtained. When the temperature of the mixture drops to room temperature, ultrasonic oscillation is used, filtration and centrifugation are performed, and drying is performed to obtain nano-silica / polyethylene wax / polyvinyl alcohol composite wall material-encapsulated isocyanate microcapsules, i.e., isocyanate microcapsules.