Method for improving structure uniformity of high-strength titanium alloy large component
Through the multi-fire forging and heating forging process, the alpha grains in titanium alloy forging are transformed and uniformly grown, which solves the problem of tissue inhomogeneity caused by traditional heat treatment, and significantly improves the mechanical properties and tissue uniformity of the forging.
Patent Information
- Application Number
- CN202411207694.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-08-30
AI Technical Summary
In the production process of large components of high-strength titanium alloys, traditional heat treatment processes lead to uneven tissue structure of forgings, uneven distribution of α grain size and volume fraction, and large differences in contrast, affecting product performance.
By using multi-fire forging and heating forging processes, the forging parts are heated to a specific temperature in a heating furnace for insulation treatment, the α grains are completely transformed into β grains, and the small-angle grain boundary is converted into large-angle grain boundary. Weak the contrast difference and perform aging insulation treatment to uniformly grow β grains.
It effectively eliminates the contrast difference in the forging tissue, improves the uniformity and mechanical properties of the forging, and ensures the overall performance of the forging.
Smart Images

Figure CN119082639A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metal hot processing, in particular to a method for improving the uniformity of the structure of a large high-strength titanium alloy component. Background Art
[0002] With the demand for lightweight aviation equipment, key load-bearing components are gradually developing in the direction of large-scale and integrated, which further increases the size of raw material bars. In the production process of large-sized raw material bars (diameter ≥ 400mm), large-sized ingots (diameter ≥ 700mm) are often used to produce raw materials. Due to the small forging ratio, the number of fires from ingots to large-sized raw materials is small, and the degree of deformation is insufficient, which will produce a large amount of incomplete recrystallization in the core. There will be a large number of small-angle grain boundaries in the incompletely recrystallized grains, resulting in a significant contrast difference between the incompletely recrystallized grains and the completely recrystallized grains ( Figure 1 ), resulting in uneven overall structure of forgings produced after traditional heat treatment, which will eventually be inherited by the forging structure. In addition, it is also easy to have uneven overall structure, such as uneven distribution of the size and volume fraction of α grains in various parts of the bar ( Figure 2 If the traditional heat treatment process is used, the core of the forging still has the primary α phase ( Figure 3 ), resulting in poor product performance.
[0003] When producing small-sized raw materials (diameter < 350mm), large-sized ingots (diameter ≥ 700mm) are also used to produce raw materials. However, during the forging process, the forging ratio is large, and multiple forgings will be performed in the middle. During the multiple forgings, the size of the large-sized ingots gradually decreases, and the deformation of the forgings is more uniform during the forging process, so that the α grains in the core of the forgings can also be uniformly deformed. The temperature can also be guaranteed to be uniform during the heat treatment process, and the overall structural unevenness in the large-sized ingots can be eliminated to obtain raw materials with uniform overall structural morphology. The overall structural morphology of the final forgings is also very uniform. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide a method for improving the uniformity of the structure of a large high-strength titanium alloy component, which is used to eliminate the contrast difference in the forging structure.
[0005] The technical solution adopted by the present invention to solve the technical problem is a method for improving the uniformity of the structure of a large high-strength titanium alloy component, comprising the following steps:
[0006] S1: placing the ingot in a heating furnace, heating the ingot to the forging temperature, and warming the core of the ingot to the temperature;
[0007] S2: forging the ingot for multiple times to form raw materials;
[0008] S3: The raw materials are heated and forged for multiple times to form forgings;
[0009] S4: placing the forging in a heating furnace, heating the forging to Tβ+Δt, Δt is -30 to -20°C, and keeping the temperature for 90 to 120 minutes;
[0010] S5: After the insulation is completed, the forging is heated to Tβ+Δn, Δn is 15-30°C, and the temperature is kept for 60-90 minutes; then the forging is subjected to aging insulation treatment.
[0011] S6: Turn off the heating furnace and allow the forging to air cool to room temperature.
[0012] Further, in step S5, the aging and heat preservation treatment process is to adjust the temperature of the heating furnace to the aging temperature, the aging temperature is 540-590°, and put the forging into the heating furnace for aging and heat preservation for 6-8 hours.
[0013] Further, in step S4, the forging is heated to Tβ+Δt, Δt is -30 to -20°C, and kept warm for 90 to 120 minutes to ensure that all α grains are completely dissolved and completely transformed into β grains. While promoting the dissolution of α grains, the low-angle grain boundaries are transformed into high-angle grain boundaries, weakening the contrast.
[0014] The beneficial effects of the present invention are as follows: by placing a forging in a heating furnace, heating the forging to Tβ+Δt, and keeping the temperature for a first time; making α grains in the forging completely transform into β grains and promoting the transformation of small-angle grain boundaries into large-angle grain boundaries, thereby weakening the contrast; and then heating the forging to Tβ+Δn, where n is greater than t, and keeping the temperature for a second time; making the β grains grow uniformly, ensuring uniform internal structure of the forging, avoiding excessive growth of the β grains, and eliminating the contrast difference in the forging structure. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 It is a physical picture of the ingot with contrast difference in the prior art;
[0016] Figure 2 yes Figure 1 Schematic diagram of the crystal phase in;
[0017] Figure 3 yes Figure 1 Schematic diagram of the crystal phase of the formed forging;
[0018] Figure 4 It is a flow chart of the present invention. DETAILED DESCRIPTION
[0019] Embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present invention, and cannot be understood as limiting the present invention.
[0020] like Figure 1 As shown, the present invention provides a method for improving the uniformity of the structure of a large high-strength titanium alloy component, comprising the following steps:
[0021] S1: placing the ingot in a heating furnace, heating the ingot to the forging temperature, and warming the core of the ingot to the temperature;
[0022] S2: forging the ingot for multiple times to form raw materials;
[0023] S3: The raw materials are heated and forged for multiple times to form forgings;
[0024] S4: placing the forging in a heating furnace, heating the forging to Tβ+Δt, Δt is -30 to -20°C, and keeping the temperature for 90 to 120 minutes;
[0025] S5: After the insulation is completed, the forging is heated to Tβ+Δn, Δn is 15-30°C, and the temperature is kept for 60-90 minutes; then the forging is subjected to aging insulation treatment.
[0026] S6: Turn off the heating furnace and allow the forging to air cool to room temperature.
[0027] Among them, the ingot is a titanium alloy steel ingot with contrast difference, and the diameter of the ingot is more than 700mm; the diameter of the raw material formed by forging the ingot is more than 400mm. In the process from ingot to raw material, due to the small forging ratio, there is also a contrast difference in the formed raw material, and this contrast difference will eventually be inherited to the forging structure, and the typical structure in the forging still has a contrast difference; the contrast difference is the abnormality of the central structure and the uneven distribution of the size and volume fraction of the grains; by placing the forging in a heating furnace, the forging is heated to Tβ+Δt, Δt is -30~-20℃, and kept warm for 90~120 minutes; while promoting the dissolution of α grains, the small angle grain boundaries are promoted to large angle grain boundaries, weakening the contrast. The forging is then heated to Δn of 15~30℃ and kept warm for 60~90 minutes; the β grains grow evenly, ensuring the uniformity of the internal structure of the forging and eliminating the contrast difference in the forging structure.
[0028] In step S5, the aging and heat preservation treatment process is to adjust the temperature of the heating furnace to the aging temperature, the aging temperature is 540-590°, and put the forging into the heating furnace for aging and heat preservation for 6-8 hours.
[0029] Further, in step S4, the forging is heated to Tβ+Δt, Δt is -30 to -20°C, and kept warm for 90 to 120 minutes to ensure that all α grains are completely dissolved and completely transformed into β grains, promoting the dissolution of the α phase while promoting the transformation of small-angle grain boundaries into large-angle grain boundaries, thereby weakening the contrast.
[0030] Example 1
[0031] S1: placing the ingot in a heating furnace, heating the ingot to the forging temperature, and warming the core of the ingot to the temperature;
[0032] S2: forging the ingot for multiple times to form raw materials;
[0033] S3: The raw materials are heated and forged for multiple times to form forgings;
[0034] S4: Place the forging in a heating furnace, heat the forging to (Tβ-30)°, and keep it warm for 90 minutes;
[0035] S5: After the insulation is completed, the forging is heated to Tβ+15° and kept warm for 60 minutes; then the heating furnace temperature is adjusted to 540° and the aging insulation is carried out for 6 hours;
[0036] S6: Turn off the heating furnace and allow the forging to air cool to room temperature.
[0037] Example 2
[0038] S1: placing the ingot in a heating furnace, heating the ingot to the forging temperature, and warming the core of the ingot to the temperature;
[0039] S2: forging the ingot for multiple times to form raw materials;
[0040] S3: The raw materials are heated and forged for multiple times to form forgings;
[0041] S4: Place the forging in a heating furnace, heat the forging to (Tβ-20)°, and keep it warm for 120 minutes;
[0042] S5: After the heat preservation is completed, the forging is heated to Tβ+30° and kept warm for 90 minutes; then the heating furnace temperature is adjusted to 590° and the aging heat preservation is carried out for 8 hours;
[0043] S6: Turn off the heating furnace and allow the forging to air cool to room temperature.
[0044] Comparative Example 1
[0045] S1: placing the ingot in a heating furnace, heating the ingot to the forging temperature, and warming the core of the ingot to the temperature;
[0046] S2: forging the ingot for multiple times to form raw materials;
[0047] S3: The raw materials are heated and forged for multiple times to form forgings;
[0048] S4: Turn off the heating furnace and allow the forging to air cool to room temperature.
[0049] The mechanical properties of the forgings formed in Example 1, Example 2 and Comparative Example 1 were tested respectively, as shown in the following table.
[0050] serial number tensile strength Yield Strength Elongation Sectional shrinkage Example 1 1170 1050 12 24 Example 2 1178 1058 11 22 Comparative Example 1 1120 1039 16 37
[0051] The mechanical properties test results show that the mechanical properties of the forgings treated by this method are significantly higher than those of the untreated forgings.
[0052] The embodiments of this specific implementation method are all preferred embodiments of the present invention, and are not intended to limit the protection scope of the present invention. Therefore, all equivalent changes made based on the structure, shape, and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for improving the uniformity of the structure of a large high-strength titanium alloy component, characterized in that: The following steps are included: S1: placing the ingot in a heating furnace, heating the ingot to the forging temperature, and warming the core of the ingot to the temperature; S2: forging the ingot for multiple times to form raw materials; S3: The raw materials are heated and forged for multiple times to form forgings; S4: placing the forging in a heating furnace, heating the forging to Tβ+Δt, Δt is -30 to -20°C, and keeping the temperature for 90 to 120 minutes; S5: After the heat preservation is completed, the forging is heated to Tβ+Δn, Δn is 15-30°C, and the heat preservation is carried out for 60-90 minutes; then the forging is subjected to aging heat preservation treatment; S6: Turn off the heating furnace and allow the forging to air cool to room temperature.
2. A method for improving the uniformity of the structure of a large high-strength titanium alloy component as claimed in claim 1, characterized in that: In step S5, the aging and heat preservation treatment process is to adjust the temperature of the heating furnace to the aging temperature, the aging temperature is 540-590°, and put the forging into the heating furnace for aging and heat preservation for 6-8 hours.
3. A method for improving the uniformity of the structure of a large high-strength titanium alloy component as claimed in claim 1, characterized in that: In step S4, the forging is heated to Tβ+Δt, where Δt is -30 to -20°C, and kept warm for 90 to 120 minutes to ensure that all α grains are completely dissolved and completely transformed into β grains.
Citation Information
Patent Citations
Forging technology for abnormal structure of TC18 titanium alloy raw material
CN105441845A
Free forging method for Ti662 titanium alloy large-size bars
CN110586828A
Heat treatment method of TC21 alloy forging
CN112662974A
High-efficiency and low-cost TC19 titanium alloy beta-forged blisk forging preparation method
CN115041616A
Short-process Ti-55531 titanium alloy bar preparation method
CN117821870A