Antibacterial composite fabric and preparation method thereof

By spraying antibacterial nanosol and ordered mesoporous silica materials on textiles to load silver ions, forming an antibacterial layer, the antibacterial rate of antibacterial textiles decreased and the dissolution of nanosilver solution after multiple washings was solved, and good antibacterial Wash-resistant and human safety.

CN119082981AInactive Publication Date: 2024-12-06NINGBO ELITE HLDG GRP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411586587.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-11-08
Publication Date
2024-12-06
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The antibacterial rate of existing antibacterial textiles decreases after multiple washes, and the nano-silver solution causes dissolution problems in the fabric, which may cause harm to the human body.

Method used

Antibacterial nanosol is used to combine with the textile layer, and antibacterial layer is formed through spraying process, and silver ions are loaded with orderly mesoporous silicon oxide materials to reduce dissolution problems and improve antibacterial durability.

Benefits of technology

The antibacterial composite fabric has been achieved to maintain good antibacterial effect after multiple cleanings, which reduces potential damage to the human body and improves the binding fastness and washing resistance of the antibacterial layer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention discloses an antibacterial composite fabric and a preparation method thereof.The antibacterial composite fabric comprises a heat preservation layer and an antibacterial layer, raw materials of the antibacterial layer comprise one or more of cotton fibers and polyester fibers, and the cotton fibers and / or the polyester fibers are woven to form a textile layer; the raw material of the antibacterial layer further comprises antibacterial nano sol; the antibacterial nano sol and one side of the textile layer form an antibacterial layer through a spraying process. The antibacterial and washable fabric has a good antibacterial effect and a good washable effect, and can still keep a certain antibacterial effect after being washed for multiple times; meanwhile, the problem of dissolution of a silver nitrate solution in the use process of the fabric is solved, and harm to a human body in the wearing process is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of antibacterial fabrics, in particular to an antibacterial composite fabric and a preparation method thereof. Background Art

[0002] With the increasing development of the world economy and the advancement of science and technology, people's requirements for textiles are no longer just satisfied with their most basic wearing functions, but want higher and richer use value. Functional textiles came into being, which means that on the basis of satisfying their own basic use value, they also meet other additional functions.

[0003] Bacteria are the most widely distributed type of microorganisms. They are everywhere, have fast reproduction ability, strong adaptability to the environment, and a wide variety of species. Their existence may threaten human health. They may even invade the human body and cause illness. Textiles are functional products that are essential to human life. Due to their own microporous structure, they are very easy to absorb and contaminate microorganisms. In addition, due to the suitable temperature and humidity on the surface of the human body, the secretion of oil, sweat, etc., in some special cases, favorable conditions are created for the reproduction and growth of microorganisms. Therefore, nowadays, more efforts are made to study functional textiles with antibacterial effects, which can quickly and efficiently kill bacteria to prevent their breeding and reproduction, and cause harm to human health. With the deepening of research on antibacterial textiles at home and abroad, the rise and development of nanosilver materials has led many outstanding researchers to gradually explore the research and application of new antibacterial agents in fiber fabrics. At present, the padding method is used to treat polyester and other chemical fiber fabrics with antibacterial finishing, and the antibacterial properties of the fabrics are greatly enhanced. However, after multiple washings, the antibacterial rate drops to 60%. There are also viscose fabrics that are directly immersed in silver nitrate solution to obtain viscose fabrics with high antibacterial properties, but the silver nitrate solution has dissolution problems during the use of the fabric, and excessive silver ions may even cause harm to the human body. There are also in-situ reduction methods that use silver ammonia solutions to finish cotton fabrics. Studies have found that the finished cotton fabrics have a high antibacterial effect, and the antibacterial effect does not decrease significantly after 30 washings.

[0004] In general, the current process of preparing textiles with nano-silver antibacterial agents is limited to padding and chemical reduction. The padding process is simple to operate and easier to industrialize. The chemical reduction method, although it has the advantages of stable performance and strong washability, is still mostly limited to laboratories and difficult to industrialize. Summary of the invention

[0005] The present application provides an antibacterial composite fabric and a preparation method thereof, which has good antibacterial effect and good wash resistance, and can still maintain a certain antibacterial effect after multiple fabric washings; at the same time, it reduces the dissolution problem of silver nitrate solution during the use of the fabric, thereby reducing the harm to the human body during wearing.

[0006] The present application provides an antibacterial composite fabric, which includes a thermal insulation layer and an antibacterial layer. The raw material of the antibacterial layer includes one or more of cotton fiber and polyester fiber. The cotton fiber and / or the polyester fiber are woven into a textile layer. The raw material of the antibacterial layer also includes antibacterial nanosol. The antibacterial nanosol forms an antibacterial layer with one side of the textile layer through a spraying process.

[0007] By adopting the above technical solution, the present application reduces the dissolution problem of silver nitrate solution during the use of fabrics by adopting the method of antibacterial nanosol. Due to the small size effect of nanoparticles, they themselves have high surface activity and are very easy to combine with other atoms. At the same time, the bending of the fibers on the textile layer creates gaps on the fiber surface, which helps the adsorption and diffusion of nanosol particles. In addition, an antibacterial layer is formed on one side of the textile layer through the spraying process, and then quickly crystallizes on the fiber surface, producing good bonding fastness, thereby reducing the damage to the human body during wearing, and having good antibacterial and washable effects.

[0008] Preferably, the raw materials of the antibacterial nano-sol include urea, butyl titanate, silver nitrate and modified molecular sieve, and the modified molecular sieve is an ordered mesoporous silicon oxide material.

[0009] By adopting the above technical solution, the molecular sieve used in this application is an ordered mesoporous silicon oxide material, wherein the molecular sieve has a "honeycomb" porous structure, a large specific surface area, a narrow pore size distribution range, and is widely used in the fields of biomedicine, catalytic adsorption, environmental engineering, etc. By loading silver ions in the molecular sieve, the dissolution problem of silver nitrate solution during the use of the fabric is further reduced.

[0010] On the other hand, the present application discloses a method for preparing an antibacterial composite fabric, comprising the following steps: S1, dissolving a certain amount of urea in anhydrous ethanol, stirring evenly for a certain period of time, slowly adding a certain amount of butyl titanate, and adjusting the pH to a certain range with a certain concentration of dilute nitric acid, and continuing to stir for a certain period of time to obtain liquid A; S2, slowly dropping a certain concentration of silver nitrate aqueous solution into the liquid A, and continuously stirring until the solution system shows a Tyndall effect, immediately stopping to obtain liquid B and storing it in the dark; S3, dissolving a certain amount of molecular sieve in anhydrous ethanol, and adding a certain amount of silane coupling agent, stirring and reflux for a certain period of time, and washing with a mixed solution of ethanol and water Remove excess silane coupling agent, pour in the B liquid, seal and stir for a certain period of time in a light-proof manner to obtain a modified antibacterial agent; S4, immerse the fabric of the textile layer in deionized water for a certain period of time to wash away the oil and impurities on the surface of the fabric, add a certain amount of isopropanol solution to the antibacterial agent to obtain a pretreated antibacterial agent; S5, put the washed fabric into the rolling roller in the spraying equipment, and adjust the parameters of the rolling roller, nozzle and air pump, spray the pretreated antibacterial agent on the surface of the fabric to absorb and combine with the fiber, pass the fabric sprayed with the pretreated antibacterial agent into the shaping equipment through the rolling roller, and adjust the shaping equipment parameters to obtain a fabric with antibacterial properties.

[0011] Preferably, in step S1, the mass ratio of the urea to the butyl titanate is 1-2:10-20.

[0012] Preferably, in step S1, a certain amount of urea is dissolved in anhydrous ethanol, stirred evenly for 1-2 hours, a certain amount of butyl titanate is slowly added, and the pH is adjusted to 3-4 with 5wt%-10wt% of dilute nitric acid, and stirring is continued for 1-2 hours to obtain liquid A.

[0013] Preferably, in step S3, the molecular sieve comprises one of ZSM-5, MCM-41 and MCM-48.

[0014] Preferably, in step S3, after dissolving the molecular sieve in anhydrous ethanol, a silane coupling agent is added, stirred and refluxed for 12-24 hours, and washed 2-5 times with a mixed solution of ethanol and water until the excess silane coupling agent is washed away, and then the B liquid is poured into the mixture and stirred for 4-12 hours in a light-proof sealed state to obtain a modified antibacterial agent.

[0015] By adopting the above technical solution, the present application adopts the modification of molecular sieves, and uses the currently available molecular sieves to modify ZSM-5, MCM-41 and MCM-48 for the adaptability of antibacterial nanosols, thereby achieving the fixation of silver ions on the carrier. +It can be evenly distributed on the carrier, which helps to improve the antibacterial performance and antibacterial durability of the modified antibacterial agent in the antibacterial layer.

[0016] The silane coupling agent includes one or more of γ-aminopropyltriethoxysilane, γ-ureapropyltriethoxysilane, γ-aminopropyltrimethoxysilane, and γ-(β-aminoethyl)aminopropyltrimethoxysilane.

[0017] By adopting the above technical solution, the present invention uses a silane coupling agent to modify the surface amino functionalization of the molecular sieve to make Ag + It can be evenly distributed on the carrier; the silane coupling agent used is γ-aminopropyltriethoxysilane, γ-ureapropyltriethoxysilane, γ-aminopropyltrimethoxysilane, and γ-(β-aminoethyl)aminopropyltrimethoxysilane, which can grow silver nitrate in situ at the loading site, thereby improving the antibacterial performance and antibacterial durability of the modified antibacterial agent in the antibacterial layer.

[0018] Preferably, in step S5, the washed fabric is placed in a rolling roller in a spray device, and the flow rate of the nozzle is adjusted to 5-10 ml / min, the speed of the rolling roller is 10-20 m / min, and the air pump is started to control the fabric to roll evenly over the nozzle position, and the pretreated antibacterial agent is sprayed on the surface of the fabric to be adsorbed and combined with the fiber, and the fabric sprayed with the pretreated antibacterial agent enters a shaping device through a rolling roller, and the shaping temperature is set at 80-120°C for 40-50 min, thereby obtaining a fabric with antibacterial properties.

[0019] One or more technical solutions provided in this application have at least the following technical effects or advantages: 1. The present application adopts the method of antibacterial nano-sol to reduce the dissolution problem of silver nitrate solution during the use of fabrics, and forms an antibacterial layer with one side of the textile layer through a spraying process, so that the fiber surface crystallization produces good bonding strength, reducing the harm to the human body during wearing, so that the composite fabric has good antibacterial and washable effects.

[0020] 2. The molecular sieve used in the present application is an ordered mesoporous silicon oxide material. By loading silver ions in the molecular sieve, the dissolution problem of silver nitrate solution during the use of the fabric is further reduced.

[0021] 3. This application aims at fixing silver ions on a carrier through process and retrograde modification of molecular sieves, eliminating the currently commercially available molecular sieves and targeting the adaptability of antibacterial nanosols, thereby improving the antibacterial performance and antibacterial durability of the modified antibacterial agent in the antibacterial layer. DETAILED DESCRIPTION

[0022] The present application provides an antibacterial composite fabric and a preparation method thereof, which has good antibacterial effect and good wash resistance, and can still maintain a certain antibacterial effect after multiple fabric washings; at the same time, it reduces the dissolution problem of silver nitrate solution during the use of the fabric, thereby reducing the harm to the human body during wearing.

[0023] The following will be a clear and complete description of the technical solutions of the embodiments of the present application. Obviously, the described embodiments are only a part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.

[0024] It should be noted that the terms "first", "second", etc. in the specification and claims of the present application are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchangeable where appropriate, so that the embodiments of the present application described herein can be implemented in an order other than those described herein. In addition, the terms "including" and "having" and any of their variations are intended to cover non-exclusive inclusions, for example, a process, method, system, product or server comprising a series of steps or units is not necessarily limited to those steps or units clearly listed, but may include other steps or modules that are not clearly listed or inherent to these processes, methods, products or devices.

[0025] raw material: Cotton fiber: The cotton fiber is common fine-staple cotton, and the variety is selected from upland cotton. The fiber has medium fineness and length, is white or milky white in color, has mercerization, and can be spun into 11~100tex fine yarn.

[0026] Polyester fiber: Polyester fiber is polyester twisted filament (DTY) used for clothing to weave imitation silk fabrics, or interwoven with natural fibers and chemical staple yarns. The elastic modulus can reach 5.6 to 8.0 cN / dtex.

[0027] ZSM-5 molecular sieve: This application uses a zeolite molecular sieve containing organic amine cations synthesized by Mobil Corporation of the United States, with relative crystallinity: Na type>85%, H type>95%; pore size: 5A; skeleton density: 1.81.

[0028] The MCM-41 molecular sieve in this application is synthesized by Mobil Oil Company using ethyl silicate as the silicon source through a micelle-based soft template method. MCM-41 has a one-dimensional pore structure formed by regular cylindrical mesopores. The mesopore diameter can be adjusted between 2-6.5nm.

[0029] The MCM-48 molecular sieve in this application is synthesized by Mobil Oil Company using ethyl silicate as the silicon source through a micelle-based soft template method. The MCM-48 molecular sieve belongs to the M41S series of mesoporous molecular sieves, with a uniform pore size of about 2.6nm and two sets of independent three-dimensional spiral pore network structures.

[0030] Urea CAS: 58069-82-2 Molecular weight: 61.048 Purity: 99.5% Titanate butyl ester CAS: 5593-70-4 Molecular weight: 388.189 Purity: 98.0% Silver nitrate CAS: 7761-88-8 Molecular weight: 169.873 Purity: 99.5% γ-Aminopropyltriethoxysilane CAS: 919-30-2 Molecular weight: 221.369 Purity: 98.0% Example 1

[0031] S1. Dissolve 1.0 kg of urea in an appropriate amount of anhydrous ethanol, stir evenly for a certain period of time, slowly add 10 kg of butyl titanate, adjust the pH to 3-4 with 5 wt % dilute nitric acid, continue stirring for a certain period of time, and obtain liquid A; S2, slowly drop 3 kg of 10 wt% silver nitrate aqueous solution into liquid A, continue stirring until the solution system shows Tyndall effect, then stop stirring immediately to obtain liquid B and store it in dark; S3, dissolving 0.3 kg of ZSM-5 molecular sieve in anhydrous ethanol, adding 100 mL of γ-aminopropyltriethoxysilane, stirring and reflux for 12 h, and washing 3 times with a mixed solution of ethanol and water until the excess γ-aminopropyltriethoxysilane is washed away, and pouring the B liquid into the light-proof sealed stirring for 6 h to obtain a modified antibacterial agent; S4, immersing 1.0 kg of the textile layer fabric obtained by weaving cotton fibers in deionized water for 1 hour at a temperature of 40° C. and a 0.5% soap solution as a detergent to wash away the oil and impurities on the surface of the fabric, adding a certain amount of isopropanol solution to 0.1 kg of the antibacterial agent, and ultrasonically treating the mixed solution for 1 hour to prepare a pre-treated antibacterial agent; S5. Put the washed fabric into the rolling roller in the spray equipment, adjust the flow rate of the nozzle to 10 ml / min, the speed of the rolling roller to 20 m / min, start the air pump to control the fabric to roll evenly over the nozzle position, spray the pretreated antibacterial agent on the surface of the fabric to adsorb and combine with the fiber, pass the fabric sprayed with the pretreated antibacterial agent into the shaping equipment through the rolling roller, set the shaping temperature at 100 ° C, and the time is 40-50 minutes, so as to obtain the fabric with antibacterial properties.

[0032] Example 2

[0033] The difference between Example 2 and Example 1 is that in step S3, after the MCM-41 molecular sieve is dissolved in anhydrous ethanol, γ-aminopropyltriethoxysilane is added for modification.

[0034] Example 3

[0035] The difference between Example 3 and Example 1 is that in step S3, after the MCM-48 molecular sieve is dissolved in anhydrous ethanol, γ-aminopropyltriethoxysilane is added for modification.

[0036] Comparative Example The difference between Comparative Example 1 and Example 1 is that, in steps S1 and S2, a certain amount of urea is dissolved in anhydrous ethanol, and butyl titanate is added, and the pH is adjusted to 40 ℃ with dilute nitric acid to obtain liquid A, and a silver nitrate aqueous solution is added to liquid A to prepare liquid B with antibacterial effect; in step S5, liquid B is directly sprayed on the surface of the fabric to be adsorbed and combined with the fiber, and the sprayed fabric is passed through a rolling roller into a shaping device to obtain a fabric with antibacterial properties. Comparative Example 2 The difference between Comparative Example 2 and Example 1 is that, in step S3, the ZSM-5 molecular sieve is not modified by γ-aminopropyltriethoxysilane to obtain the modified antibacterial agent.

[0037] Comparative Example 3 The difference between Comparative Example 3 and Example 1 is that, in step S3, the ZSM-5 molecular sieve is modified with γ-aminopropyltriethoxysilane to obtain a modified molecular sieve; however, the modified molecular sieve is not loaded with liquid A and liquid B.

[0038] Comparative Example 4 The difference between Comparative Example 4 and Example 1 is that, in step S5, the pretreatment antibacterial agent is used to perform antibacterial finishing on chemical fiber fabrics such as polyester by padding method.

[0039] Performance testing

[0040] In order to further study the effects of various components and preparation parameters on the antibacterial composite fabric, the present application further carries out the following examples for verification.

[0041] According to Examples 1-3 and Comparative Examples 1-4, the antibacterial composite fabrics prepared in each Example and each Comparative Example were tested for their antibacterial properties and the lasting effect of the antibacterial properties after multiple washings, and the dissolution of silver ions after multiple washings was also tested.

[0042] Among them, the antibacterial composite fabric was washed according to the method in GB / T8629-2017 "Household Washing and Drying Procedure for Textile Testing", the washing degree was 5N, and it was washed 0, 20, 50, and 100 times respectively. The washed composite fiber core was dried and placed in an environment of 20°C and 60% relative humidity for 48 hours to test its antibacterial properties.

[0043] 1. Antibacterial performance test: The test was carried out in accordance with GB / T20944.3-2008 "Evaluation of antibacterial properties of textiles Part 3: Oscillation method", with Escherichia coli, Candida albicans and Staphylococcus aureus as the test bacteria. The antibacterial rate in this embodiment is the average of the antibacterial rates of the three bacteria.

[0044] 2. Silver ion dissolution test: 20g of fabric is immersed in 1L of deionized water at 25℃ for 48h. The OEKO-TEX standard is used as the test procedure. The test instrument adopts plasma atomic emission spectrometry to detect the silver ion content dissolved in deionized water.

[0045] The test results are integrated into the following table.

[0046] Table 1, Performance test table of Examples 1-3 and Comparative Examples 1-4

[0047] Antibacterial performance test: Unit: % (average antibacterial rate of Escherichia coli ATCC 8099, Candida albicans ATCC 10231 and Staphylococcus aureus ATCC 6538) Silver ion dissolution test results: Unit: mmol / L Conclusion Analysis

[0048] Through the antibacterial performance test analysis of Examples 1-3, the antibacterial composite fabric without washing has a high antibacterial rate, and can show a high antibacterial effect on Escherichia coli, Candida albicans and Staphylococcus aureus. In addition, compared with the analysis of Comparative Example 1, in which the mixed liquid is not loaded with molecular sieves, Comparative Example 1 has a certain antibacterial effect, but it is significantly lower than the effect of Examples 1-3. In addition, since the silver ions in Comparative Example 1 are not loaded with molecular sieves, the silver ions are easily dissolved in the fabric, and their dissolution concentration will gradually increase with the increase in the number of washing times.

[0049] In addition, for the analysis of Comparative Example 2, the molecular sieve was not modified by a silane coupling agent, so its antibacterial effect was improved compared with Comparative Example 1, but after multiple washings, its antibacterial effect gradually decreased, and after 100 washings, the antibacterial effect was almost the same as that of Comparative Example 1. In addition, for the silver ion dissolution test, the silver ion dissolution was almost zero during the soaking process of the fabric that had not been washed; but after multiple washings, since there was no silane coupling agent to modify the molecular sieve, the probability of silver ion dissolution would increase.

[0050] In addition, in Comparative Example 3, the molecular sieve was modified with a silane coupling agent, but the modified molecular sieve was not loaded with liquid A and liquid B, so the antibacterial effect was not obvious; and since the modified molecular sieve was not loaded with liquid A and liquid B, no silver ion dissolution was found in the silver ion dissolution result test of the antibacterial composite membrane fabric.

[0051] In Comparative Example 4, the pre-treated antibacterial agent was used to perform antibacterial finishing on polyester and other chemical fiber fabrics by padding method. The modified antibacterial agent was not prepared by two-step method, nor was the modified molecular sieve used to fix silver ions, so the antibacterial performance and silver ion dissolution test were slightly weaker than those of Examples 1-3.

[0052] The experimental data analysis in Examples 1-3 shows that the use of modified molecular sieves can effectively improve the antibacterial properties of antibacterial composite fabrics and reduce the dissolution of silver ions in antibacterial composite fabrics. In addition, when ZSM-5 molecular sieves, a zeolite molecular sieve containing organic amine cations, are used, more excellent data are obtained. Therefore, Example 1 is the best example.

[0053] Example 4

[0054] The difference between Example 4 and Example 1 is that in step S3, the silane coupling agent used is γ-ureapropyltriethoxysilane.

[0055] Example 5

[0056] The difference between Example 5 and Example 1 is that in step S3, the silane coupling agent used is γ-aminopropyltrimethoxysilane.

[0057] Example 6

[0058] The difference between Example 6 and Example 1 is that in step S3, the silane coupling agent used is γ-(β-aminoethyl)aminopropyltrimethoxysilane.

[0059] Performance testing

[0060] In order to further study the influence of each component and preparation parameter on the antibacterial composite fabric, the present application further carries out the following examples for verification. According to Examples 1, 4-6, the antibacterial composite fabric prepared in each example is used to detect its antibacterial performance and the lasting effect of the antibacterial performance after multiple washings according to the above-mentioned testing standards; and the dissolution of silver ions after multiple washings is also detected. The obtained data is sorted into the following table.

[0061] Table 2. Performance test table of Examples 1, 4-6

[0062] Conclusion Analysis Through the antibacterial performance test analysis of Examples 1, 4-6, improvements are made in the modification of molecular sieves by silane coupling agents in the examples, in which different silane coupling agents are tried for modification. Among the selections of γ-aminopropyltriethoxysilane, γ-ureapropyltriethoxysilane, γ-aminopropyltrimethoxysilane, and γ-(β-aminoethyl)aminopropyltrimethoxysilane, it can be obtained through experimental data that when the silane coupling agent is γ-(β-aminoethyl)aminopropyltrimethoxysilane, the amino group on the silane coupling agent can modify the disease to make Ag + It can be evenly distributed on the molecular sieve carrier, thereby improving the antibacterial performance and antibacterial durability of the modified antibacterial agent in the antibacterial layer. And from the silver ion dissolution experiment, it is detected that the antibacterial composite fabric can reduce the harm to the human body during wearing. Therefore, Example 6 is the best embodiment of the embodiments of this application.

[0063] It should be noted that the above-mentioned sequence of the embodiments of the present application is only for description and does not represent the advantages and disadvantages of the embodiments. And the above-mentioned specific embodiments of this specification are described. Other embodiments are within the scope of the attached claims. In some cases, the actions or steps recorded in the claims can be performed in an order different from that in the embodiments and still achieve the desired results. In some embodiments, multitasking and parallel processing are also possible or may be advantageous.

[0064] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present application should be included in the protection scope of the present application.

[0065] This specification is merely an exemplary description of the present application and is deemed to cover any and all modifications, variations, combinations or equivalents within the scope of the present application. Obviously, a person skilled in the art may make various modifications and variations to the present application without departing from the scope of the present application. Thus, if these modifications and variations of the present application fall within the scope of the present application and its equivalents, the present application is intended to include these modifications and variations.

Claims

1. An antibacterial composite fabric, characterized in that: The antibacterial composite fabric includes a thermal insulation layer and an antibacterial layer, the raw materials of the antibacterial layer include one or more of cotton fibers and polyester fibers, and the cotton fibers and / or the polyester fibers are woven into a textile layer; the raw materials of the antibacterial layer also include antibacterial nanosol; the antibacterial nanosol forms an antibacterial layer with one side of the textile layer through a spraying process; the raw materials of the antibacterial nanosol include urea, butyl titanate, silver nitrate and modified molecular sieve, and the modified molecular sieve is an ordered mesoporous silicon oxide material.

2. A method for preparing the antibacterial composite fabric according to claim 1, characterized in that: The following steps are involved: S1. Dissolve a certain amount of urea in anhydrous ethanol, stir evenly for a certain period of time, slowly add a certain amount of butyl titanate, adjust the pH to a certain range with a certain concentration of dilute nitric acid, continue stirring for a certain period of time, and obtain liquid A; S2, slowly adding a certain concentration of silver nitrate aqueous solution to the liquid A, and stirring continuously until the solution system shows a Tyndall effect, then stopping immediately to obtain liquid B and storing it in the dark; S3, dissolving a certain amount of modified molecular sieve in anhydrous ethanol, adding a certain amount of silane coupling agent, stirring and refluxing for a certain time, washing away excess silane coupling agent with a mixed solution of ethanol and water, pouring the B liquid into the mixture, sealing and stirring for a certain time in a light-proof manner, to obtain a modified antibacterial agent; S4, immersing the fabric of the textile layer in deionized water for a certain period of time to wash away the oil and impurities on the surface of the fabric, and adding a certain amount of isopropanol solution to the antibacterial agent to obtain a pretreated antibacterial agent; S5. Place the washed fabric into the rolling roller in the spraying equipment, and adjust the parameters of the rolling roller, nozzle and air pump, spray the pretreated antibacterial agent on the surface of the fabric to adsorb and combine with the fiber, pass the fabric sprayed with the pretreated antibacterial agent into the shaping equipment through the rolling roller, and adjust the shaping equipment parameters to obtain fabric with antibacterial properties.

3. The method for preparing the antibacterial composite fabric according to claim 2, characterized in that: In step S1, the mass ratio of the urea to the butyl titanate is 1-2:10-20.

4. The method for preparing the antibacterial composite fabric according to claim 3, characterized in that: In step S1, a certain amount of urea is dissolved in anhydrous ethanol, and the mixture is stirred evenly for 1-2 hours. A certain amount of butyl titanate is slowly added, and the pH is adjusted to 3-4 with 5wt%-10wt% of dilute nitric acid. The mixture is stirred for 1-2 hours to obtain liquid A.

5. The method for preparing the antibacterial composite fabric according to claim 2, characterized in that: In the step S3, the modified molecular sieve includes one of ZSM-5, MCM-41 and MCM-48.

6. The method for preparing the antibacterial composite fabric according to claim 5, characterized in that: In the step S3, after the molecular sieve is dissolved in anhydrous ethanol, a silane coupling agent is added, stirred and refluxed for 12-24 hours, and washed 2-5 times with a mixed solution of ethanol and water until the excess silane coupling agent is washed away, and the B liquid is poured into the light-proof sealed and stirred for 4-12 hours to obtain a modified antibacterial agent.

7. The method for preparing the antibacterial composite fabric according to claim 6, characterized in that: The silane coupling agent includes one or more of γ-aminopropyltriethoxysilane, γ-ureapropyltriethoxysilane, γ-aminopropyltrimethoxysilane, and γ-(β-aminoethyl)aminopropyltrimethoxysilane.

8. The method for preparing the antibacterial composite fabric according to claim 2, characterized in that: In the step S5, the washed fabric is placed in the rolling roller of the spraying equipment, and the flow rate of the nozzle is adjusted to 5-10 ml / min, the speed of the rolling roller is 10-20 m / min, and the air pump is started to control the fabric to roll evenly over the nozzle position, and the pretreated antibacterial agent is sprayed on the surface of the fabric to be adsorbed and combined with the fiber, and the fabric sprayed with the pretreated antibacterial agent enters the shaping equipment through the rolling roller, and the shaping temperature is set at 80-120° C. for 40-50 min, thereby obtaining a fabric with antibacterial properties.

Citation Information

Patent Citations

  • Functional mesoporous silicon oxide, method for preparing same and method for applying functional mesoporous silicon oxide to wound repair

    CN108721635A

  • Nano-silver antibacterial fabric with good wear resistance and preparation process thereof

    CN114619723A

  • Zinc ion-based antibacterial and heating fabric and weaving method thereof

    CN114734689A

  • Washable antibacterial fabric and preparation method thereof

    CN115216964A

  • Silver ion antibacterial fabric and production method thereof

    CN115652613A