Non-aqueous electrolyte and lithium ion battery thereof
By using cycloolefin compound A in the non-aqueous electrolyte as an additive in lithium-ion batteries, the problem of degradation of the stability of the nickel-cobalt-manganese oxide positive electrode material is solved, and the fast charging, cycling and low-temperature discharge performance of lithium-ion batteries is improved. , reduces gas production and improves high-temperature storage performance.
Patent Information
- Application Number
- CN202410855166.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-12-06
AI Technical Summary
When the nickel content of nickel-cobalt-manganese oxide positive electrode material increases in lithium-ion batteries, the body phase structure and surface chemical stability decrease, resulting in increased gas production and poor storage and circulation performance.
A nonaqueous electrolyte solution, including lithium salt, nonaqueous organic solvent and cycloolefin structure compound A, can undergo a ring opening reaction on the negative electrode side, form a sulfur-rich and nitrogen-rich interface, and increase lithium ions. Transfer characteristics and improve interface stability through polymerization at high temperature and high voltage.
Significantly improve the fast charging, circulation, storage and low-temperature discharge characteristics of lithium-ion batteries, reduce gas production, and improve circulation and high-temperature performance.
Smart Images

Figure CN119092822A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a non-aqueous electrolyte and a lithium ion battery thereof. Background Art
[0002] In recent years, lithium-ion batteries have been widely used in energy storage power systems such as hydropower, thermal power, wind power and solar power stations, as well as power tools, electric bicycles, electric motorcycles, electric vehicles, military equipment, aerospace and other fields due to their high energy density, high reversible capacity and environmental friendliness. With the continuous upgrading of market demand for lithium-ion battery performance, people have put forward higher requirements for the energy density, cycle performance and safety performance of lithium-ion batteries. Developing lithium-ion battery cathode materials with high specific capacity is one of the effective ways.
[0003] Among many positive electrode materials, nickel cobalt manganese oxide is considered to be one of the most promising positive electrode materials for high energy density power batteries due to its high discharge specific capacity and low cost. In order to further improve the energy density of nickel cobalt manganese materials, increasing the proportion of active component nickel in the main structure has become the main strategy, but with the increase of nickel content, the bulk structural stability and surface chemical stability of nickel cobalt manganese oxide materials gradually decrease, which is specifically manifested in cation mixing, surface residual alkali and transition metal ion dissolution. These problems will bring adverse effects to lithium-ion batteries, such as increased gas production, poor storage performance and cycle performance.
[0004] Therefore, a non-aqueous electrolyte and a lithium ion battery thereof are urgently needed to solve the above problems. Summary of the invention
[0005] The object of the present invention is to provide a non-aqueous electrolyte and a lithium-ion battery thereof, wherein the non-aqueous electrolyte can reduce the gas production during the circulation and storage process of the lithium-ion battery, thereby improving the storage performance and circulation performance of the lithium-ion battery, and can also effectively improve its fast charging performance and low-temperature discharge performance.
[0006] To achieve the above object, the present invention provides a non-aqueous electrolyte, including a lithium salt, a non-aqueous organic solvent and an additive, wherein the additive includes a compound A shown in Formula 1:
[0007]
[0008] Wherein, R1, R2, and R3 are each independently selected from hydrogen, halogen, cyano, alkyl, alkenyl, or alkynyl.
[0009] Compared with the prior art, the additive of the present invention includes compound A, which is a cycloolefin structure, and the ring contains N elements and sulfonyl groups. The compound A of the structure shown in the present invention can reduce battery impedance, improve battery cycle, and improve battery gas production and storage performance. This may be because compound A can undergo a ring-opening reaction on the negative electrode side to form a sulfur- and nitrogen-rich interface. The interface has excellent lithium ion transmission characteristics, which can support the discharge characteristics of the battery at low temperatures, and can also improve the battery's cycle performance at high voltage and high temperature. In addition, the double bonds after the ring opening will undergo a polymerization reaction at the negative electrode to form an organic polymer, which improves the interfacial stability of the battery at high temperature and high voltage. In summary, the structure shown in the present invention can significantly improve the fast charging, circulation, storage and low-temperature discharge characteristics of lithium-ion batteries.
[0010] Further, R1, R2, and R3 are each independently selected from hydrogen or C1-C6 alkyl. Specifically, the C1-C6 alkyl of the present invention refers to an alkyl group containing 1 to 6 carbon atoms, and the alkyl group can be linear, branched, or cyclic, such as methyl, ethyl, propyl, isopropyl, butyl, sec-butyl, tert-butyl, pentyl, and cyclohexyl. It is understood that R1, R2, and R3 can be the same or different, and are not limited here.
[0011] Furthermore, the compound A of the present invention is at least one selected from compounds 1 to 8:
[0012]
[0013]
[0014] Further, the mass percentage of the compound A of the present invention in the non-aqueous electrolyte is 0.1% to 5.0%. As an example, the mass percentage of the compound A of the present invention in the non-aqueous electrolyte is specifically but not limited to 0.1%, 0.5%, 0.8%, 1.0%, 1.2%, 1.5%, 1.8%, 2.0%, 2.2%, 2.5%, 2.8%, 3.0%, 3.2%, 3.5%, 3.8%, 4.0%, 4.3%, 4.5%, 5.0%.
[0015] Furthermore, the lithium salt of the present invention is selected from at least one of lithium hexafluorophosphate (LiPF6), lithium perchlorate (LiClO4), lithium tetrafluoroborate (LiBF4), lithium trifluoromethanesulfonate (LiCF3SO3), lithium bistrifluoromethylsulfonyl imide (LiTFSI), lithium bis(oxalatoborate) (LiBOB), lithium difluorophosphate (LiPO2F2), lithium fluorosulfonate (LiSO2F), lithium dioxalatoborate (LiBC4O8), lithium difluorooxalatoborate (LiODFB), lithium difluorobis(oxalatophosphate) (LiDODFP) and lithium bis(fluorosulfonyl imide) (LiFSI).
[0016] Furthermore, the mass percentage of the lithium salt of the present invention in the non-aqueous electrolyte is 5% to 25%. As an example, the mass percentage of the lithium salt of the present invention in the non-aqueous electrolyte is specifically but not limited to 5%, 6%, 7%, 8%, 9%, 10%, 12%, 14%, 15%, 16%, 18%, 20%, 22%, 25%.
[0017] Furthermore, the non-aqueous organic solvent of the present invention is at least one of carbonate, carboxylate and ether compounds.
[0018] Specifically, carbonates include, but are not limited to, ethylene carbonate (EC), propylene carbonate, butylene carbonate (BC), pentylene carbonate, dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), propylene carbonate (PC). Carboxylates include, but are not limited to, γ-butyrolactone (GBL), γ-valerolactone (GVL), δ-valerolactone, methyl acetate (MA), ethyl acetate (EA), ethyl propionate (EP), butyl acetate (n-Ba), propyl propionate (n-PP), butyl propionate. Ether compounds include, but are not limited to, 1,3-dioxolane (DOL), 1,4-dioxolane (DX), crown ether, tetrahydrofuran (THF), 2-methyltetrahydrofuran (2-CH3-THF), 2-trifluoromethyltetrahydrofuran (2-CF3-THF), dimethoxymethane, diethoxymethane, ethoxymethoxymethane, ethylene glycol di-n-propyl ether, ethylene glycol di-n-butyl ether (EDB), and diethylene glycol dimethyl ether (DEGME).
[0019] Furthermore, the non-aqueous electrolyte of the present invention also includes an auxiliary agent, and the auxiliary agent is selected from vinylene carbonate (VC), vinylene carbonate (VEC), fluoroethylene carbonate (FEC), vinyl sulfite (ES), 1,3-propane sultone (PS), 1,3-propene sultone (PST), 1,4-butane sultone (1,4-BS), vinyl sulfate (DTD), succinic anhydride (SA), maleic anhydride (MA), 2-methylmaleic anhydride, tetravinylsilane (TVSI), triallyl isocyanurate (TAIC), hexamethylene diisocyanate (HDI), o-phenanthroline, p-phenylene diisocyanate, At least one of 2,4-butane sultone (2,4-BS), isocyanoethyl methacrylate (IEM), methylene disulfonate (MMDS), tris(trimethylsilyl) borate (TMSB), tris(trimethylsilyl) phosphate (TMSP), and tris(vinyldimethylsilyl) phosphate. As an example, the auxiliary agent is fluoroethylene carbonate (FEC), and for example, the auxiliary agent is a mixture of vinylene carbonate (VC) and vinyl sulfite (ES).
[0020] Furthermore, the mass percentage of the auxiliary agent of the present invention in the non-aqueous electrolyte is 0.1% to 5.0%. As an example, the mass percentage of the auxiliary agent of the present invention in the non-aqueous electrolyte is specifically but not limited to 0.1%, 0.5%, 0.8%, 1.0%, 1.2%, 1.5%, 1.8%, 2.0%, 2.2%, 2.5%, 2.8%, 3.0%, 3.2%, 3.5%, 3.8%, 4.0%, 4.3%, 4.5%, 5.0%.
[0021] Another aspect of the present invention provides a lithium-ion battery, comprising a positive electrode material and a negative electrode material, and also comprising the above-mentioned non-aqueous electrolyte.
[0022] Furthermore, the positive electrode material of the present invention is selected from nickel cobalt manganese oxide, and the chemical formula of the nickel cobalt manganese oxide is LiNi x Co y Mn (1-x-y) M z O2, wherein 0.6≤x<0.9, x+y<1, 0≤z<0.08, M is at least one of Al, Mg, Zr and Ti. As an example, x=0.8, y=0.1, M is Zr, and z=0.03.
[0023] Furthermore, the negative electrode material of the present invention is selected from at least one of a carbon-based negative electrode, a silicon-based negative electrode, a tin-based negative electrode, and a lithium negative electrode. The carbon-based negative electrode may include graphite, hard carbon, soft carbon, graphene, mesophase carbon microspheres, etc.; the silicon-based negative electrode may include silicon materials, silicon oxides, silicon-carbon composite materials, and silicon alloy materials, etc.; the tin-based negative electrode may include tin, tin carbon, tin oxygen, and tin metal compounds; the lithium negative electrode may include metallic lithium or a lithium alloy. The lithium alloy may specifically be at least one of a lithium silicon alloy, a lithium sodium alloy, a lithium potassium alloy, a lithium aluminum alloy, a lithium tin alloy, and a lithium indium alloy. DETAILED DESCRIPTION
[0024] In order to better illustrate the purpose, technical scheme and beneficial effects of the present invention, the present invention will be further described below in conjunction with specific embodiments. It should be noted that the following implementation method is a further explanation of the present invention and should not be used as a limitation of the present invention.
[0025] If no specific conditions are specified in the examples and comparative examples of the present invention, the experiments may be carried out under conventional conditions or conditions recommended by the manufacturer. If no manufacturer is specified for the reagents or instruments used, they are all conventional products available on the market.
[0026] Example 1
[0027] (1) Preparation of non-aqueous electrolyte
[0028] In a glove box filled with argon (O2 <1ppm, H2O <1ppm), ethylene carbonate (EC), ethyl methyl carbonate (EMC) and diethyl carbonate (DEC) were mixed in a weight ratio of EC:EMC:DEC=1:1:3 to prepare 85.0g of a non-aqueous organic solvent, and then 1.0g of compound 1 was added as an additive, dissolved and fully stirred to obtain a mixed solution, the mixed solution was sealed and packaged, placed in a quick freezer (-4°C) and frozen for 2h, and then taken out, and in a glove box filled with nitrogen (O2 <1ppm, H2O <1ppm), 14g of lithium hexafluorophosphate was slowly added to the mixed solution, and the electrolyte was prepared after mixing evenly.
[0029] (2) Preparation of positive electrode
[0030] The high nickel ternary material LiNi 0.8 Co 0.1 Mn 0.1 Zr 0.03 O2, conductive agent SuperP, adhesive PVDF and carbon nanotubes (CNT) are mixed evenly in a mass ratio of 96.5:1.5:1:1 to form a lithium-ion battery positive electrode slurry with a certain viscosity, which is coated on the aluminum foil for current collector. The coating amount is 324g / m 2, dried at 85°C and then cold pressed; then trimmed, cut into pieces, and slit, and after slitting, dried at 85°C for 4 hours under vacuum conditions, and the tabs were welded to make lithium-ion battery positive electrodes that meet the requirements.
[0031] (3) Preparation of negative electrode sheet
[0032] Artificial graphite and silicon are mixed in a mass ratio of 90:10, and then mixed with conductive agent SuperP, thickener CMC, and adhesive SBR (styrene-butadiene rubber latex) in a mass ratio of 95:1.5:1.0:2.5 to make a slurry, mix evenly, apply the mixed slurry on both sides of the copper foil, dry and roll to obtain a negative electrode sheet, and make a lithium-ion battery negative electrode sheet that meets the requirements.
[0033] (4) Preparation of lithium-ion batteries
[0034] The positive electrode sheet, negative electrode sheet and separator prepared according to the above process are laminated to form a lithium-ion battery with a thickness of 4.7mm, a width of 55mm and a length of 60mm. The battery is vacuum-baked at 75°C for 10 hours and the above non-aqueous electrolyte is injected. After standing for 24 hours, the battery is charged to 4.45V with a constant current of 0.1C (180mA), and then charged at a constant voltage of 4.45V until the current drops to 0.05C (90mA); then discharged to 3.0V with 0.2C (180mA), and the charge and discharge are repeated twice. Finally, the battery is charged to 3.8V with 0.2C (180mA) to complete the production of the lithium-ion battery.
[0035] The components and contents of the electrolytes of Examples 1 to 19 and Comparative Examples 1 to 3 are shown in Table 1, wherein the preparation processes of the non-aqueous electrolytes, positive electrodes, negative electrodes and lithium-ion batteries of Examples 2 to 19 and Comparative Examples 1 to 3 are the same as those of Example 1.
[0036] Table 1 Compositions of the non-aqueous electrolytes of the embodiments and comparative examples
[0037]
[0038]
[0039] The lithium ion batteries prepared in Examples 1 to 19 and Comparative Examples 1 to 3 were subjected to high temperature storage performance test, high temperature cycle performance test, room temperature cycle performance test, and fast charging performance test under the following conditions. The results are shown in Table 2.
[0040] High temperature storage performance test :
[0041] At room temperature (25°C), the lithium-ion battery was charged and discharged at 0.5C / 0.5C (the battery discharge capacity was recorded as C0), with an upper limit voltage of 4.4V, and then the battery was charged to 4.4V under 0.5C constant current and constant voltage conditions, and the battery thickness was measured (the thickness was recorded as D0); the battery was placed in a 60°C oven for 30 days, taken out and the battery thickness was measured (the thickness was recorded as D1); the battery was placed in a 25°C environment and discharged at 0.5C (the discharge capacity was recorded as C1); the lithium-ion battery was continued to be charged and discharged at room temperature (25°C) at 0.5C / 0.5C (the battery discharge capacity was recorded as C2), with an upper limit voltage of 4.4V and a lower limit voltage of 3.0V, and the capacity retention rate, capacity recovery rate and thickness expansion rate were calculated.
[0042] Capacity retention rate = (C1 / C0)*100%
[0043] Capacity recovery rate = (C2 / C0)*100%
[0044] Thickness expansion rate = (D1-D0) / D0*100%
[0045] Normal temperature cycle performance test :
[0046] At room temperature (25°C), the lithium-ion battery is charged and discharged at 1.0C / 1.0C once (the battery discharge capacity is C0), with an upper voltage of 4.4V and a lower voltage of 3.0V. Then, it is charged and discharged at 1.0C / 1.0C for 500 cycles at room temperature (the battery discharge capacity is C1), and the capacity retention rate is calculated.
[0047] Capacity retention rate = (C1 / C0)*100%
[0048] High temperature cycle test :
[0049] Under high temperature (45°C) conditions, the lithium-ion battery was charged and discharged at 1.0C / 1.0C (the battery discharge capacity is C0), the upper limit voltage was 4.4V, the lower limit voltage was 3.0V, the battery thickness was measured (the thickness was recorded as D0), then charged and discharged at 1.0C / 1.0C for 400 weeks at 45°C (the battery discharge capacity is C1), the battery thickness was measured (the thickness was recorded as D1), and the capacity retention rate and battery thickness expansion rate were calculated.
[0050] Capacity retention rate = (C1 / C0)*100%
[0051] Thickness expansion rate = (D1-D0) / D0*100%
[0052] Fast charging performance test :
[0053] At room temperature (25°C), the lithium-ion battery is charged and discharged at 1.0C / 1.0C once (the battery discharge capacity is C0), with an upper voltage of 4.4V and a lower voltage of 3.0V. Then, it is charged and discharged at 4.0C / 1.0C for 400 cycles at room temperature (the battery discharge capacity is C1), and the capacity retention rate is calculated.
[0054] Capacity retention rate = (C1 / C0)*100%
[0055] Low temperature discharge performance test :
[0056] At room temperature (25°C), the lithium-ion battery is charged and discharged at 0.5C / 0.5C (the discharge capacity is recorded as C0), the upper limit voltage is 4.4V, and then the battery is charged to 4.4V under 0.5C constant current and constant voltage conditions; the lithium-ion battery is placed in a -20°C low temperature box for 4 hours and discharged at 0.5C at -20°C (the discharge capacity is recorded as C1); the low temperature discharge rate of the lithium-ion battery is calculated using the following formula;
[0057] Low temperature discharge rate = C1 / C0*100%
[0058] Table 2 Lithium-ion battery performance test results
[0059]
[0060]
[0061] As can be seen from Table 2, compared with Comparative Examples 1 to 3, Examples 1 to 19 use the additive compound A of the present invention in their non-aqueous electrolytes, so the lithium-ion batteries have better high-temperature storage performance, cycle performance and fast charging performance, and can effectively reduce the gas production of lithium-ion batteries. This may be because the additive compound A of the present invention can undergo a ring-opening reaction on the negative electrode side to form an interface rich in sulfur and nitrogen. The interface has excellent lithium ion transmission characteristics, which can support the discharge characteristics of the battery at low temperatures, and can also improve the cycle performance of the battery at high voltage and high temperature. In addition, the double bonds after the ring opening will undergo a polymerization reaction here to form an organic polymer, which improves the interfacial stability of the battery at high temperature and high voltage. In summary, the additive compound of the structure shown in the present invention can significantly improve the fast charging, cycling and storage characteristics of lithium-ion batteries.
[0062] From the comparison between Example 1 and Examples 15 to 19, it can be seen that adding a film-forming aid on the basis of the additive of the present invention can further improve the high-temperature storage performance, cycle performance, fast charging performance and low-temperature discharge performance of the lithium-ion battery.
[0063] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention is described in detail with reference to the preferred embodiments, it is not limited to those listed in the embodiments. Those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A non-aqueous electrolyte comprising a lithium salt, a non-aqueous organic solvent and an additive, characterized in that: The additive includes a compound A shown in Formula 1: Wherein, R1, R2, and R3 are each independently selected from hydrogen, halogen, cyano, alkyl, alkenyl, or alkynyl.
2. The non-aqueous electrolyte according to claim 1, characterized in that R1, R2, and R3 are each independently selected from hydrogen or C1-C6 alkyl.
3. The non-aqueous electrolyte according to claim 1, characterized in that The compound A is selected from at least one of compounds 1 to 8:
4. The non-aqueous electrolyte according to claim 1, characterized in that The mass percentage of the compound A in the non-aqueous electrolyte is 0.1% to 5.0%.
5. The non-aqueous electrolyte according to claim 1, characterized in that The lithium salt is selected from at least one of lithium hexafluorophosphate, lithium perchlorate, lithium tetrafluoroborate, lithium trifluoromethanesulfonate, lithium bistrifluoromethanesulfonyl imide, lithium bisoxalatoborate, lithium difluorophosphate, lithium fluorosulfonate, lithium bisoxalatoborate, lithium difluorooxalatoborate, lithium difluorobisoxalatophosphate and lithium bisfluorosulfonyl imide.
6. The non-aqueous electrolyte according to claim 1, characterized in that The mass percentage of the lithium salt in the non-aqueous electrolyte is 5% to 25%.
7. The non-aqueous electrolyte according to claim 1, characterized in that The non-aqueous organic solvent is at least one of carbonate, carboxylate and ether compounds.
8. The non-aqueous electrolyte according to claim 1, characterized in that The invention also includes an auxiliary agent, which is selected from at least one of vinylene carbonate, vinylene carbonate, fluoroethylene carbonate, vinyl sulfite, 1,3-propane sultone, 1,3-propylene sultone, 1,4-butane sultone, vinyl sulfate, succinic anhydride, maleic anhydride, 2-methylmaleic anhydride, tetravinylsilane, triallyl isocyanurate, hexamethylene diisocyanate, o-phenanthroline, p-phenylene diisocyanate, 2,4-toluene diisocyanate, N-phenylbis(trifluoromethanesulfonyl)imide, phenyl methanesulfonate, vinyl disulfate, hydroquinone difluorosulfonate, triallyl phosphate, tripropargyl phosphate, 2,4-butane sultone, isocyanoethyl methacrylate, methylene disulfonate, tris(trimethylsilyl)borate, tris(trimethylsilyl)phosphate and tris(vinyldimethylsilyl)phosphate.
9. A lithium ion battery comprising a positive electrode material and a negative electrode material, characterized in that: It also includes the non-aqueous electrolyte according to any one of claims 1 to 8.
10. The lithium ion battery according to claim 9, characterized in that: The positive electrode material is selected from nickel cobalt manganese oxide, and the chemical formula of the nickel cobalt manganese oxide is LiNi x Co y Mn (1-x-y) M z O2, wherein 0.6≤x<0.9, x+y<1, 0≤z<0.08, and M is at least one of Al, Mg, Zr and Ti.