Aluminum-plastic film coatings, aluminum-plastic films and their applications

By forming a coating on the aluminum-plastic film and utilizing a combination of active adsorbent materials and modifiers, the problems of easy leakage and damage of the aluminum-plastic film are solved, and the gas adsorption and impact resistance are improved, thus protecting the internal structure of the battery.

CN119286316BActive Publication Date: 2026-11-17ZHEJIANG LIWINON ELECTRONIC TECHNOLOGY CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411339647.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-25
Publication Date
2026-11-17
Estimated Expiration
2044-09-25

AI Technical Summary

Technical Problem

Existing aluminum-plastic films are prone to leakage in soft-pack batteries due to gas generation inside the cell, and are easily damaged at rounded corners or dent edges, lacking effective gas adsorption and impact resistance.

Method used

A coating is formed on the aluminum-plastic film. Using porous materials such as active adsorbents like γ-alumina, combined with the modifier isobutylene-maleic anhydride copolymer, a coating with good impact resistance is formed. This coating adsorbs gas inside the battery and releases electrolyte, protecting the R-corners from damage.

Benefits of technology

It effectively adsorbs gas inside the battery, reduces leakage, improves battery performance, and protects the R-angle under high impact, meeting impact resistance requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119286316B_ABST
    Figure CN119286316B_ABST
Patent Text Reader

Abstract

This application discloses aluminum-plastic film coatings, aluminum-plastic films, and their applications. The aluminum-plastic film coating comprises an active adsorbent material, a modifier, a binder, a coupling agent, and an oil-based solvent. The active adsorbent material has a specific surface area ≥150 m². 2 Porous materials with a Mohs hardness ≥3 and a modifier including isobutylene-maleic anhydride copolymer. The active adsorbent material possesses numerous surface active sites, surface micro / nano structures, and a large number of micropores. The Coulomb force between the micropores and the active adsorbent material generates adsorption. The resulting coating, in contact with the electrolyte, achieves electrolyte retention. During later stages of cycling, as the electrolyte is consumed, the active adsorbent material effectively adsorbs internally generated gases and releases some electrolyte, thereby improving various battery performance characteristics. Furthermore, the active adsorbent material is sufficient to impart more effective impact resistance to the aluminum-plastic film, thus providing support during denting and protecting the R-angle aluminum foil residue beneath deep dents.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of lithium-ion battery technology, and in particular to aluminum-plastic film coatings, aluminum-plastic films and their applications. Background Technology

[0002] Soft-pack batteries typically use aluminum-plastic film as a protective film for the battery cell. Existing aluminum-plastic film structures consist of layers of polyethylene terephthalate (PET) / nylon, an aluminum foil layer, and a cast polypropylene (CPP) layer, formed through multi-layer co-extrusion casting or multi-layer lamination processes. Failure of the aluminum-plastic film in soft-pack batteries mainly manifests as leakage. Besides abnormal encapsulation, one cause of leakage is the generation of gas inside the battery cell, and another is damage to the rounded corners or the bottom edge of dents. Therefore, it is necessary to provide an aluminum-plastic film that can absorb gas inside the battery while possessing good impact resistance to prevent breakage. Summary of the Invention

[0003] This application aims to at least solve one of the technical problems existing in the prior art. To this end, this application proposes an aluminum-plastic film coating, an aluminum-plastic film, and its application. The coating formed on the aluminum-plastic film can effectively adsorb the gas inside the battery, while also possessing good impact resistance to prevent damage.

[0004] A first aspect of this application provides an aluminum-plastic film coating, comprising an active adsorbent material, a modifier, a binder, a coupling agent, and an oil-based solvent, wherein the active adsorbent material has a specific surface area ≥150 m². 2 Porous materials with a Mohs hardness ≥3 per g, and modifiers include isobutylene-maleic anhydride copolymer.

[0005] The aluminum-plastic film coating according to the first aspect of this application has the following beneficial effects:

[0006] The active adsorbent material meeting the above characteristics possesses numerous surface active sites and surface micro / nano structures, forming a large number of micropores smaller than 1 nm internally. The Coulomb force between the micropores and the active adsorbent material generates adsorption. The resulting coating, in contact with the electrolyte, achieves electrolyte retention. During later stages of cycling, as the electrolyte is consumed, the active adsorbent material effectively adsorbs internally generated gases and releases some electrolyte, thereby improving various battery performance characteristics. Furthermore, the active adsorbent material meeting the aforementioned Mohs hardness requirements is sufficient to impart more effective impact resistance to the aluminum-plastic film, thus providing support during denting and protecting the R-angle aluminum foil residue beneath deep dents.

[0007] In addition, during the practical process, it was noted that active adsorbent materials with high specific surface area are prone to capillary water absorption. If the active adsorbent material is simply coated, moisture may be introduced into the battery cell, generating gas and causing a decrease in battery performance. However, the modifier isobutylene-maleic anhydride copolymer, as an amphiphilic polymer, can be uniformly distributed on the surface of the active adsorbent material through solvent dissolution. After heat treatment, the CO bond in the CONH4 group breaks and generates imide groups, avoiding the capillary water absorption phenomenon of the active adsorbent material and further reducing gas generation.

[0008] In some embodiments of this application, the mass ratio of the modifier to the active adsorbent is 0.00005 to 0.0002:1, for example, it can be 0.00005:1, 0.00006:1, 0.00007:1, 0.00008:1, 0.00009:1, 0.0001:1, 0.00012:1, 0.00014:1, 0.00016:1, 0.00018:1, or 0.0002:1.

[0009] In some embodiments of this application, the mass ratio of binder to active adsorbent material is 1 to 3:10, for example, it can be 1:10, 2:10, or 3:10.

[0010] In some embodiments of this application, the mass ratio of coupling agent to active adsorbent material is 1 to 3:10, for example, it can be 1:10, 2:10, or 3:10.

[0011] In some embodiments of this application, the active adsorbent material includes at least one of γ-alumina, titanium dioxide, boehmite, and pseudoboehmite.

[0012] In some embodiments of this application, the active adsorbent material includes at least one of γ-alumina and boehmite.

[0013] In some embodiments of this application, the active adsorbent material includes γ-alumina. Using γ-alumina achieves both impact resistance and gas adsorption efficiency while avoiding the introduction of new impurities (such as activated carbon, molecular sieves, titanium hydroxide, titanium oxide, etc.) into the battery cell. In contrast, boehmite and gibbsite have slightly lower Mohs hardness, and are less effective in improving the mechanical properties of aluminum-plastic films, such as impact resistance.

[0014] In some embodiments of this application, the purity of γ-alumina is ≥99.9%, and the specific surface area is ≥150 m². 2 / g.

[0015] In some embodiments of this application, the purity of the pseudoboehmite is ≥99.9%, and the specific surface area is ≥230 m². 2 / g.

[0016] In some embodiments of this application, the Mohs hardness of boehmite and boehmite is 3 to 4, the Mohs hardness of γ-alumina is 6 to 8, and the Mohs hardness of titanium dioxide is 5 to 6.

[0017] In some embodiments of this application, the binder includes at least one of polyvinylidene fluoride (PVDF), styrene-acrylic acid copolymer, and polyvinyl acetate.

[0018] In some embodiments of this application, the combination of polyvinylidene fluoride binder with modifier and active adsorbent material has a better effect on improving impact resistance and temperature resistance.

[0019] In some embodiments of this application, the coupling agent includes at least one selected from aluminate coupling agents, phthalate coupling agents, silane coupling agents, phosphate coupling agents, and borate coupling agents. These coupling agents have one inorganic-philic group and one organic-philic group, and their addition to coatings can improve the dispersion of active adsorbent materials in organic solvents.

[0020] In some embodiments of this application, the coupling agent includes an aluminate coupling agent. The aluminate has the molecular formula [Al(OR)3]. n (R is alkyl or allyl), as an aluminum source, it does not introduce new impurity elements. In addition, compared with other coupling agents (such as borate ester coupling agents, phosphate ester coupling agents, silane coupling agents), it is light in color, non-toxic, has little taste, and is inexpensive.

[0021] In some embodiments of this application, the oily solvent includes a first solvent and a second solvent; wherein the first solvent includes at least one selected from N-methylpyrrolidone (NMP), dimethylformamide, carbon tetrachloride, toluene-dichloroethane, acetone, and isopropanol; and the second solvent includes at least one selected from dimethyl carbonate and N,N-dimethylformamide. Because the active adsorbent material itself has a large specific surface area, it is difficult to wet and disperse uniformly in water; therefore, an oily solvent is used for dispersion. For this purpose, the first solvent is used to dissolve or disperse the active adsorbent material and the coupling agent, and the second solvent is used to dissolve or disperse the modifier, so that all components can achieve high dispersion, thereby improving the adsorption effect on the gas.

[0022] In some embodiments of this application, the mass ratio of the first solvent to the active adsorbent material is 100:10 to 15, for example, it can be 100:10, 100:11, 100:12, 100:13, 100:14, or 100:15.

[0023] In some embodiments of this application, the ratio of the modifier to the second solvent is 1g:0.5 to 1.5L, for example, it can be 1g:0.5L, 1g:0.6L, 1g:0.7L, 1g:0.8L, 1g:0.9L, 1g:1.0L, 1g:1.1L, 1g:1.2L, 1g:1.3L, 1g:1.4L, or 1g:1.5L.

[0024] The surface of activated adsorbent materials has numerous active sites and a micro / nano structure, forming many pores and mesopores. The Coulomb force between the mesopores and the activated adsorbent material generates adsorption, which can adsorb gases generated inside the battery cell. Using inorganic ceramic materials such as γ-alumina in combination with polyvinylidene fluoride (PVDF) can give the inner layer of the aluminum-plastic film high-temperature resistance, flame retardancy, and impact resistance. This protects the battery cell in case of failure and prevents damage to the radius (R) corners of the aluminum-plastic film under high-impact depths.

[0025] A second aspect of this application provides an aluminum-plastic film comprising a first insulating polymer layer, an aluminum foil layer, and a second insulating polymer layer disposed sequentially. The first insulating polymer layer is further provided with a functional coating on the side away from the aluminum foil layer, the functional coating being made of the aforementioned aluminum-plastic film coating.

[0026] The second insulating polymer layer provides certain heat resistance, abrasion resistance, puncture resistance, and bending resistance, effectively protecting the aluminum foil layer. It is typically made of at least one of the following materials: nylon, polyester (such as polyethylene terephthalate), etc. The first insulating polymer layer provides heat sealing and is made of at least one of the following materials: polypropylene, polyethylene, ethylene-acrylic acid copolymer, ion-crosslinked polymer resin, etc.

[0027] In some embodiments of this application, the aluminum-plastic film includes a polypropylene layer, an aluminum foil layer, and a nylon layer arranged sequentially. The side of the polypropylene layer away from the aluminum foil layer is also provided with a functional coating, which is made of the aforementioned aluminum-plastic film coating.

[0028] In some embodiments of this application, the aluminum-plastic film includes a pitted area, and a functional coating covers the pitted area.

[0029] In some embodiments of this application, the aluminum-plastic film also includes a heat-sealing area around the punching area, which includes a top sealing area, a side sealing area, and a secondary sealing area.

[0030] In some embodiments of this application, the area of ​​the functional coating on the aluminum-plastic film is more than 1.1 times the area of ​​the crater area.

[0031] In some embodiments of this application, the distance from the edge of the functional coating on the aluminum-plastic film to the inner side of the heat-sealing area is ≥5mm. The inner side refers to the side closest to the pitted area.

[0032] If the functional coating area is too large and too close to the heat-sealing inner side, discontinuous heat sealing (point-like) may occur in the heat-sealing area during the melting process of the heated polypropylene layer. During long-term immersion in electrolyte, leakage is likely to occur through the coating, affecting the heat-sealing effect and causing leakage. On the other hand, if the functional coating area is too small, it cannot better protect the R-corner aluminum foil residue under the crater.

[0033] In some embodiments of this application, the aluminum-plastic film satisfies T / 1000≤M×D≤A;

[0034] Where T is the depth of the crater, and it is less than 15mm;

[0035] M represents the Mohs hardness of the active adsorption material;

[0036] D is the thickness of the functional coating, and D is 2 to 10 μm;

[0037] A represents the thickness of the aluminum foil layer.

[0038] To ensure that the aluminum-plastic film can protect the aluminum foil residue at the R-corner under high-impact conditions without taking up too much space in the battery cell and avoiding excessive thickness that could affect the ED of the battery cell itself, the aluminum-plastic film must meet the above conditions.

[0039] This application also relates to a method for preparing aluminum-plastic film, including the following steps:

[0040] The aluminum-plastic film coating is applied to the pitted area, and then heat-treated to form a functional coating.

[0041] In some embodiments of this application, the heat treatment temperature is 80 to 150°C, for example, it can be 80°C, 90°C, 100°C, 110°C, 120°C, 130°C, 140°C, or 150°C.

[0042] In some embodiments of this application, the coating method is gravure intermittent coating.

[0043] A third aspect of this application provides a lithium-ion battery comprising the aforementioned aluminum-plastic film.

[0044] In some embodiments of this application, a lithium-ion battery includes a cell and an aluminum-plastic film covering the cell. The cell includes a positive electrode, a negative electrode, an electrolyte, and a separator. The positive electrode, negative electrode, and separator are obtained by winding or other methods to form the cell and thus a lithium-ion battery.

[0045] In some embodiments of this application, the positive current collector and the negative current collector are each independently selected from at least one of the following metal materials: metal foil (such as aluminum foil, silver foil, tin foil, iron foil, titanium foil, nickel foil, copper foil or alloy foil of the above metals) and metal mesh (such as aluminum mesh, silver mesh, tin mesh, iron mesh, titanium mesh, nickel mesh, copper mesh or alloy mesh of the above metals).

[0046] In some embodiments of this application, the positive (negative) electrode includes a positive (negative) current collector and a positive (negative) active material layer.

[0047] In some embodiments of this application, the positive electrode active material layer includes a positive electrode active material, including but not limited to at least one of lithium cobalt oxide, lithium manganese oxide, lithium iron phosphate, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, and lithium nickel manganese aluminum oxide. The negative electrode active material layer includes a negative electrode active material, including but not limited to at least one of carbon materials, silicon materials, and silicon-carbon materials.

[0048] A fourth aspect of this application provides an electrical device. The electrical device includes the aforementioned lithium-ion battery.

[0049] Electrical equipment refers to any device that can utilize electrical energy and convert it into mechanical energy, thermal energy, light energy, or one or more other forms of energy, such as electric motors, electric heaters, and electric light sources. This includes mobile devices, electric vehicles, electric trains, ships and satellites, and energy storage systems. Mobile devices can be mobile phones, laptops, drones, robot vacuum cleaners, e-cigarettes, etc.; electric vehicles can be pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.

[0050] Additional aspects and advantages of this application will be set forth in part in the description which follows, and in part will be obvious from the description, or may be learned by practice of this application. Attached Figure Description

[0051] Figure 1 This is a schematic diagram of the structure of an aluminum-plastic film according to an embodiment of this application.

[0052] Reference numerals: Aluminum-plastic film 100, punching area 110, side sealing area 120, top sealing area 130, second sealing area 140, air bag area 150, first sealing area 160, first functional coating 210, second functional coating 220. Detailed Implementation

[0053] The following will clearly and completely describe the concept and technical effects of this application in conjunction with embodiments, so as to fully understand the purpose, features and effects of this application. Obviously, the described embodiments are only some embodiments of this application, not all embodiments. Other embodiments obtained by those skilled in the art based on the embodiments of this application without creative effort are all within the scope of protection of this application.

[0054] The embodiments of this application are described in detail below. The described embodiments are exemplary and are only used to explain this application, and should not be construed as limiting this application.

[0055] In the description of this application, "several" means one or more, "multiple" means two or more, "greater than," "less than," and "exceeding" are understood to exclude the stated number, while "above," "below," and "within" are understood to include the stated number, and "approximately" means within the range of ±20%, 10%, 8%, 5%, 4%, 3%, 2%, 1%, 0.5%, 0.2%, 0.1%, etc. of the stated number. The use of "first" and "second" is merely for distinguishing technical features and should not be construed as indicating or implying relative importance, or implicitly indicating the number of indicated technical features, or implicitly indicating the order of the indicated technical features.

[0056] In the description of this application, the terms "one embodiment," "some embodiments," "illustrative embodiment," "example," "specific example," or "some examples," etc., refer to specific features, structures, materials, or characteristics described in connection with that embodiment or example, which are included in at least one embodiment or example of this application. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples.

[0057] The present application will be described below with reference to specific embodiments.

[0058] Example 1

[0059] This embodiment provides an aluminum-plastic film coating, the preparation process of which is as follows:

[0060] 1) Weigh 2.0 kg of γ-alumina (Mohs hardness 6.5, specific surface area 168 m²). 2 Add 18 kg of NMP (the first solvent) and 0.25 kg of aluminate coupling agent to the ball mill, turn on the ball mill cooling circulation device, control the temperature below 50°C during the ball milling process, set the ball mill parameters to 30 Hz, use alumina as the ball milling medium, and stir for 1 hour. Stop stirring to obtain the primary slurry.

[0061] 2) Mix 0.1g of the modifier isobutylene-maleic anhydride copolymer (ISOBAM-104) powder with 0.1L of the second solvent dimethyl carbonate to obtain the modified solution.

[0062] 3) Add 0.2 kg PVDF and the modified liquid to the above primary slurry, and continue stirring for 2 hours at a ball mill setting of 50 Hz to obtain the aluminum-plastic film coating.

[0063] This embodiment also relates to an aluminum-plastic film, see reference. Figure 1The aluminum-plastic film 100 includes a perforated area 110, a side sealing area 120, a top sealing area 130, a secondary sealing area 140, an air bag area 150, and a final sealing area 160. Additionally, the aluminum-plastic film is sequentially provided with a cast polypropylene (CPP) layer, an aluminum foil layer, and a nylon layer, with the aluminum foil layer having a thickness of 40 μm.

[0064] This embodiment also relates to a coating method for aluminum-plastic film coatings, as detailed below:

[0065] Combination Figure 1 The aluminum-plastic film coating is applied to the perforated area 110 of the CPP layer of the aluminum-plastic film using an intermittent gravure coating method, and the same coating is applied to the back area of ​​the perforation opposite the fold line. After drying with hot air at 120°C, a first functional coating 210 and a second functional coating 220 are formed on the CPP layer, resulting in an aluminum-plastic film with functional coatings. The thickness of the functional coatings is 4μm.

[0066] In addition, the first functional coating 210 covers the stamping area 110, but at the same time, sufficient gaps must be left between it and the heat-sealing areas such as the side sealing area 120, the top sealing area 130, and the second sealing area 140. Specifically, the distances d1, d2, and d3 from the edge of the first functional coating 210 to the inner side of the aforementioned heat-sealing areas are all controlled to be 5 mm.

[0067] Subsequently, dent tests were conducted on the aluminum-plastic film with functional coatings, with dent depths of 5mm, 6mm, 7mm, 8mm, and 9mm respectively.

[0068] Example 2

[0069] This embodiment provides an aluminum-plastic film coating and an aluminum-plastic film with a functional coating. The difference from Embodiment 1 is that the active adsorbent is boehmite (Mohs hardness 3.5, specific surface area 294 m²). 2 / g).

[0070] Example 3

[0071] This embodiment provides an aluminum-plastic film coating and an aluminum-plastic film with a functional coating. Referring to Embodiment 2, the pit depth is set to 9mm, and the thickness of the functional coating is 2μm, 3μm, 4μm, 9μm, and 10μm respectively.

[0072] Example 4

[0073] This embodiment provides an aluminum-plastic film coating and an aluminum-plastic film with a functional coating. Referring to Embodiment 1, the pit depth is set to 9mm, and the thickness of the functional coating is 6μm, 7μm, and 8μm respectively.

[0074] Comparative Example 1

[0075] This comparative example provides an aluminum-plastic film, which differs from Example 1 in that the functional coating of Example 1 is omitted, and the pit depths are 5mm, 6mm, 7mm, 8mm, and 9mm respectively.

[0076] Comparative Example 2

[0077] This comparative example provides an aluminum-plastic film coating and an aluminum-plastic film with a functional coating. The difference from Example 1 is that the aluminum-plastic film coating does not contain the modifier ISOBAM-104.

[0078] Comparative Example 3

[0079] The difference from Implementation 1 is that γ-alumina (Mohs hardness 6.5, specific surface area 168m²) is used. 2 / g) was replaced with KS6 graphite (Mohs hardness 1, specific surface area 17m). 2 / g).

[0080] Test preparation

[0081] The aluminum-plastic film from Examples 1 and 2, and Comparative Examples 1, 2, and 3, was used in a 1.5Ah soft-pack stacked lithium-ion battery. The depth of the perforation in the aluminum-plastic film was 1.1 times the thickness of the bare cell, and a single perforation method was used. The lithium-ion battery includes a positive electrode, a negative electrode, a separator, and an electrolyte. The positive electrode active material is NCM ternary material, and the negative electrode active material is graphite. The finished cell was obtained through processes such as coating, rolling, die-cutting, stacking, welding, heat sealing, baking, electrolyte injection, formation, and capacity testing.

[0082] Performance testing

[0083] Test 1

[0084] After the denting was completed in Examples 1 and 2, and Comparative Example 1, the residual rate of the aluminum layer at the R-corner was tested. The residual rate was calculated as: R-corner aluminum layer thickness after denting / original aluminum layer thickness. Industry standards generally require an R-corner aluminum foil residual rate >50%. The results are shown in the table below.

[0085] Table 1. Residual R-angle aluminum foil of the Examples and Comparative Examples

[0086]

[0087] As can be seen from the results in the table, after the improvement of the functional coating in the embodiment, the residual rate of the R-corner Al layer after the aluminum-plastic film is significantly improved under different dent depths, and its functional coating has impact resistance under high dent depths.

[0088] Test 2

[0089] After the prepared battery cells were placed at 100% SOC and 85℃ for 10 days, the liquid drop volume V1 was measured using the water displacement method, and the gas production was equal to V1. The results are shown in the table below:

[0090] Table 2. Gas production of the examples and comparative examples

[0091] Serial Number Gas production (ml) Comparative Example 1 2.8 Comparative Example 2 1.6 Comparative Example 3 2.7 Example 1 0.2 Example 2 0.3

[0092] The results in the table show that the improved functional coating in the examples significantly reduced the gas production of the finished battery cells, indicating that the aluminum-plastic film with the functional coating effectively adsorbs gases inside the battery cells. While the functional coating in Comparative Example 2 (without modifier) ​​also reduced the gas production of the finished battery cells, the reduction was more significant because its coating had a higher moisture content, leading to increased gas production and reduced adsorption. In contrast, the functional coating in Comparative Example 3, obtained using a porous material with lower Mohs hardness and smaller specific surface area, produced a finished battery cell with a gas production comparable to that of Comparative Example 1 (without a functional coating).

[0093] Test 3

[0094] The aluminum-plastic films from Example 1 and Comparative Example 2 were then subjected to the baking process according to test preparation 1). A Karl Fischer moisture meter was used to test the moisture content of the coated area, and the results are shown in the table below.

[0095] Table 3. Comparison of different moisture contents

[0096] Serial Number Moisture content (ppm) Example 1 200 Comparative Example 2 600

[0097] The results in the table show that when the modifier is omitted, the moisture content of the coated area of ​​the aluminum-plastic film functional coating increases significantly. Therefore, adding the modifier can effectively improve the capillary water absorption phenomenon of the active adsorbent material.

[0098] Test 4

[0099] After applying the functional coating to Examples 3 and 4, the residual rate of the R-angle aluminum foil layer was tested compared with Comparative Examples 1 and 3. The residual rate was calculated as: R-angle aluminum foil layer thickness after denting / original aluminum foil layer thickness. Industry standards generally require an R-angle aluminum foil residual rate > 50%. The results are as follows:

[0100] Table 4. Effect of different coating thicknesses on R-angle residual rate

[0101]

[0102] The results in the table show that when the Mohs hardness and thickness of the selected material do not reach a certain level, the residual radius (R-angle) rate, although improved, still does not meet industry standard requirements. Conversely, when the thickness is too large, the residual radius rate meets industry standards, but the overall residual rate does not change significantly. The material and coating thickness of the functional layer can be selected based on different requirements, referring to the following formula:

[0103] T / 1000≤M×D≤A;

[0104] Where T is the depth of the crater; T < 15 mm;

[0105] M represents the Mohs hardness of the active adsorption material;

[0106] D represents the thickness of the functional coating; 2μm ≤ D ≤ 10μm;

[0107] A represents the thickness of the aluminum foil layer in the aluminum-plastic film.

[0108] The present application has been described in detail above with reference to the embodiments. However, the present application is not limited to the above embodiments. Within the scope of knowledge possessed by those skilled in the art, various changes can be made without departing from the spirit of the present application. Furthermore, unless otherwise specified, the embodiments and features in the embodiments of the present application can be combined with each other.

Claims

1. An aluminum-plastic film coating, characterized by, comprising an active adsorbent material, a modifier, a binder, a coupling agent and an oily solvent, the active adsorbent material being a porous material having a specific surface area ≥ 150 m 2 / g and a Mohs hardness ≥ 3, the modifier comprising an isobutylene-maleic anhydride copolymer; The mass ratio of the modifier to the active adsorbent is 0.00005~0.0002:1, the mass ratio of the binder to the active adsorbent is 1~3:10, and the mass ratio of the coupling agent to the active adsorbent is 1~3:

10. The active adsorbent material includes at least one of γ-alumina, titanium dioxide, boehmite, and pseudoboehmite; the binder includes at least one of polyvinylidene fluoride, styrene-acrylic acid copolymer, and polyvinyl acetate. The oily solvent includes a first solvent and a second solvent. The first solvent includes at least one of N-methylpyrrolidone, dimethylformamide, carbon tetrachloride, toluene dichloroethane, acetone, and isopropanol. The second solvent includes at least one of dimethyl carbonate and N,N-dimethylformamide. The mass ratio of the first solvent to the active adsorbent is 100:10~15, and the ratio of the modifier to the second solvent is 1g:0.5~1.5L.

2. The ACF coating according to claim 1, characterized in that The coupling agent includes at least one of aluminate coupling agents, phthalate coupling agents, silane coupling agents, phosphate coupling agents, and borate coupling agents.

3. An aluminum-plastic film, characterized in that, The aluminum-plastic film includes a first insulating polymer layer, an aluminum foil layer, and a second insulating polymer layer arranged sequentially. The first insulating polymer layer is further provided with a functional coating on the side away from the aluminum foil layer. The functional coating is made of the aluminum-plastic film coating according to any one of claims 1 to 2.

4. The aluminum-plastic film according to claim 3, characterized in that, The aluminum-plastic film includes a pitted area, and the functional coating covers the pitted area.

5. The aluminum-plastic film according to claim 4, characterized in that, The aluminum-plastic film satisfies T / 1000≤M×D≤A; Where T is the depth of the crater, and it is less than 15 mm; M represents the Mohs hardness of the active adsorption material; D is the thickness of the functional coating, and D is 2~10 μm; A represents the thickness of the aluminum foil layer.

6. A lithium-ion battery, characterized in that, Includes the aluminum-plastic film as described in any one of claims 3 to 5.

7. Electrical equipment, characterized in that, Including the lithium-ion battery as described in claim 6.

Citation Information

Patent Citations

  • Metal composite film capable of adsorbing gas, preparation method of metal composite film and bagged battery

    CN113889711A

  • Metal composite film capable of adsorbing gas and preparation method therefor, and pouch battery

    WO2023035762A1