Electrolyte, preparation method thereof and lithium ion battery

By adding additive A containing a specific structure to the electrolyte solution of lithium-ion batteries, the problem of solid electrolyte interface film damage caused by volume changes during charging and discharging of silicon carbon anode material is solved, and the circulation and storage performance of the battery are improved.

CN119864505AActive Publication Date: 2025-04-22EVE ENERGY CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411898039.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-12-20
Publication Date
2025-04-22
Estimated Expiration
2044-12-20

AI Technical Summary

Technical Problem

The volume change of silicon carbon anode material in lithium-ion batteries during charging and discharging leads to the destruction of the solid electrolyte interface film, affecting the circulation and storage performance of the battery.

Method used

Add additive A to the electrolyte solution, and its structure includes fluorine atoms, boron atoms, carbonyl, siliconethyl and benzene rings to form a stable solid electrolyte interface film, enhancing its mechanical strength and toughness, and inhibiting the volume expansion of the silicon-carbon negative electrode.

Benefits of technology

Through additive A, the circulation and storage performance of lithium-ion batteries are improved, and the rupture of the solid electrolyte interface film and the side reaction between the electrolyte and the negative electrode are reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention provides an electrolyte, a preparation method thereof and a lithium ion battery. The electrolyte comprises an organic solvent, a lithium salt and an additive A. The structure of the additive A contains fluorine atoms, boron atoms, carbonyl groups, siloxane groups and benzene rings, so that a solid electrolyte interface film with relatively high mechanical strength and toughness can be formed on the surface of the negative electrode, and the volume expansion of the silicon-carbon negative electrode in the charge-discharge process is inhibited; and the damage of stress generated by volume expansion of the silicon-carbon negative electrode in the charging and discharging process to a solid electrolyte interface film is reduced, so that the cycle performance and the storage performance of the battery are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of batteries, and in particular to an electrolyte, a preparation method thereof and a lithium ion battery. Background Art

[0002] Lithium-ion batteries are one of the main energy storage technologies in the new energy market due to their high energy density, portability, strong designability and high safety. Silicon-carbon anodes have a high theoretical specific capacity and are expected to improve the mass and volume energy density of lithium-ion batteries.

[0003] However, the silicon in the silicon-carbon negative electrode will undergo significant volume changes during the process of lithium insertion and removal, which can easily lead to volume expansion of the silicon-carbon negative electrode material during charging and discharging. The solid electrolyte interface film on the surface of the silicon-carbon negative electrode material can hardly withstand the damage caused by the expansion of the silicon negative electrode during the battery cycle, affecting the cycle performance and storage performance of the lithium-ion battery. Summary of the invention

[0004] The embodiments of the present invention provide an electrolyte, a preparation method thereof and a lithium-ion battery, which can improve the technical problem that the solid electrolyte interface film on the surface of the silicon-carbon negative electrode material is difficult to withstand the damage caused by the expansion of the silicon negative electrode during the battery cycle, affecting the cycle performance and storage performance of the lithium-ion battery.

[0005] In a first aspect, an embodiment of the present invention provides an electrolyte, wherein the electrolyte comprises an organic solvent, a lithium salt and an additive A;

[0006] The structure of the additive A includes fluorine atoms, boron atoms, carbonyl groups, siloxane groups and benzene rings.

[0007] In one embodiment, the structure of the additive A is shown in Formula I:

[0008]

[0009] In one embodiment, the mass percentage of the additive A in the electrolyte is 5%-10%.

[0010] In one embodiment, the electrolyte further includes a film-forming agent, and the film-forming agent includes at least one of vinyl sulfite, propylene sulfite, fluoroethylene carbonate, and vinylene carbonate.

[0011] In one embodiment, the mass percentage of the film-forming agent in the electrolyte is 3%-5%.

[0012] In one embodiment, the lithium salt includes at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium hexafluoroarsenate, lithium difluorophosphate, lithium trifluoromethanesulfonate, and lithium bis(fluorosulfonyl)imide; and / or

[0013] The mass percentage of the lithium salt in the electrolyte is 12%-15%.

[0014] In one embodiment, the organic solvent comprises ethylene carbonate, dimethyl carbonate and ethyl methyl carbonate, and the mass ratio of the ethylene carbonate, the dimethyl carbonate and the ethyl methyl carbonate is (1-3):(1-3):(4-8); and / or

[0015] The mass percentage of the organic solvent in the electrolyte is 70%-80%.

[0016] In a second aspect, an embodiment of the present invention provides a method for preparing the electrolyte as described above, the method comprising the following steps:

[0017] Under a protective atmosphere, the organic solvent, lithium salt, additive A and other raw materials in the formulated amounts are mixed evenly to obtain the electrolyte.

[0018] In one embodiment, the other raw materials include a film-forming agent.

[0019] In one embodiment, the mixing is stirring mixing, the mixing temperature is 25° C.-30° C., and / or the mixing time is 50 min-60 min; and / or

[0020] The protective atmosphere includes a nitrogen atmosphere and / or an argon atmosphere.

[0021] In a third aspect, an embodiment of the present invention provides a lithium-ion battery, wherein the lithium-ion battery comprises the electrolyte as described above or the electrolyte prepared by the method as described above.

[0022] In one embodiment, the lithium-ion battery further comprises a positive electrode, a negative electrode and a separator;

[0023] The material of the positive electrode includes lithium iron manganese phosphate and / or nickel-cobalt-manganese ternary material, and / or the material of the negative electrode includes silicon-carbon material.

[0024] Beneficial effects of the embodiments of the present invention:

[0025] In an embodiment of the present invention, an additive A is added to the electrolyte. On the one hand, the structure of the additive A contains fluorine atoms, which can form a solid electrolyte interface film containing inorganic substances such as lithium fluoride on the surface of the negative electrode during the charge and discharge process of the battery. The lithium fluoride makes the formed solid electrolyte interface film have high mechanical strength and stability, which can inhibit the volume expansion of the silicon-carbon negative electrode during the charge and discharge process, and reduce the damage to the solid electrolyte interface film caused by the stress generated by the volume expansion of the silicon-carbon negative electrode during the charge and discharge process; in addition, the structure of the additive A contains carbonyl groups, which can undergo polymerization reaction on the surface of the negative electrode to form a polycarbonate polymer film. The polycarbonate polymer film can reduce the direct contact between the electrolyte and the negative electrode material, reduce the decomposition of the negative electrode material, and at the same time alleviate the silicon-carbon The volume expansion of the material destroys the electrode structure; on the other hand, the structure of additive A contains boron atoms, which can undergo oxidative decomposition during the charge and discharge process, thereby forming a stable borate film on the surface of the silicon-carbon negative electrode. The borate film has good flexibility and mechanical strength, and can adapt to the volume changes of the silicon-carbon negative electrode during the charge and discharge process, thereby reducing the rupture of the solid electrolyte interface film on the surface of the silicon-carbon negative electrode and reducing the occurrence of side reactions between the electrolyte and the silicon-carbon negative electrode; in addition, the structure of additive A contains siloxane groups, which can effectively form a Si-O-Si cross-linked structure on the surface of the silicon-carbon negative electrode, which can enhance the toughness of the solid electrolyte interface film on the surface of the silicon-carbon negative electrode, and effectively inhibit the expansion of the silicon-carbon negative electrode, thereby improving the cycle performance and storage performance of the battery. DETAILED DESCRIPTION

[0026] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments in the present invention, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the present invention. In addition, it should be understood that the specific implementation methods described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention. In the present invention, unless otherwise specified, the directional words used, such as "upper" and "lower", generally refer to the upper and lower parts of the device in actual use or working state; while "inside" and "outside" refer to the outline of the device.

[0027] In the related technology, silicon-carbon negative electrode materials are prone to volume expansion during the charging and discharging process. The solid electrolyte interface film on the surface of the silicon-carbon negative electrode material can hardly withstand the damage caused by the expansion of the silicon negative electrode during the battery cycle, which affects the cycle performance and storage performance of the lithium-ion battery and needs further improvement.

[0028] To solve the above problems, an embodiment of the present application provides an electrolyte, which includes an organic solvent, a lithium salt and an additive A, wherein the structure of the additive A includes a fluorine atom, a boron atom, a carbonyl group, a siloxane group and a benzene ring.

[0029] In this embodiment, additive A is added to the electrolyte. On the one hand, the structure of additive A contains fluorine atoms, which can form a solid electrolyte interface film containing inorganic substances such as lithium fluoride on the surface of the negative electrode during the charge and discharge process of the battery. Lithium fluoride makes the formed solid electrolyte interface film have high mechanical strength and stability, which can inhibit the volume expansion of the silicon-carbon negative electrode during the charge and discharge process, and reduce the damage to the solid electrolyte interface film caused by the stress generated by the volume expansion of the silicon-carbon negative electrode during the charge and discharge process; in addition, the structure of additive A contains carbonyl groups, which can undergo polymerization reaction on the surface of the negative electrode to form a polycarbonate polymer film. The polycarbonate polymer film can reduce the direct contact between the electrolyte and the negative electrode material, reduce the decomposition of the negative electrode material, and at the same time alleviate the damage to the electrode structure caused by the volume expansion of the silicon-carbon material; on the other hand, the structure of additive A Containing boron atoms, it can be oxidized and decomposed during the charge and discharge process, and then form a stable borate film on the surface of the silicon-carbon negative electrode. The borate film has good flexibility and mechanical strength, and can adapt to the volume change of the silicon-carbon negative electrode during the charge and discharge process, thereby reducing the rupture of the solid electrolyte interface film on the surface of the silicon-carbon negative electrode and reducing the occurrence of side reactions between the electrolyte and the silicon-carbon negative electrode; in addition, the structure of additive A contains siloxane groups, which can effectively form a Si-O-Si cross-linked structure on the surface of the silicon-carbon negative electrode, which can enhance the toughness of the solid electrolyte interface film on the surface of the silicon-carbon negative electrode and effectively inhibit the expansion of the silicon-carbon negative electrode, thereby improving the cycle performance and storage performance of the battery; in addition, the structure of additive A contains benzene rings, and additive A can form a protective film on the surface of the positive electrode, which can reduce the side reactions between the electrolyte and the positive electrode under high voltage systems. In one embodiment, the structure of additive A is shown in Formula I:

[0030]

[0031] In this embodiment, the CAS number of additive A is 1622303-27-8, and the name of additive A is: Benzamide, N-[2-[[[(1,1-dimethylethyl)dimethylsilyl]oxy]methyl]-3-(4,4,5,5-tetramethy l-1,3,2-dioxaborolan-2-yl)phenyl]-4-[1-(trifluoromethyl)cyclopropyl]. Additive A can be purchased directly from commercial sources, and the raw materials are easily available. The synthesis steps of additive A can be saved, and the production process of the electrolyte can be simplified.

[0032] In one embodiment, the mass percentage of additive A in the electrolyte is 5%-10%. In this embodiment, if the content of additive A is too little, the effect of additive A on improving the mechanical strength and toughness of the solid electrolyte interface film is not ideal; if additive A is too much, it is easy to cause increased gas production and increased impedance. Optionally, the mass percentage of additive A in the electrolyte can be any one of 5%, 6%, 7%, 8%, 9%, 10%, etc. or a range between any two.

[0033] In one embodiment, the electrolyte further includes a film former, and the film former includes at least one of vinyl sulfite, propylene sulfite, fluoroethylene carbonate, and vinylene carbonate. In this embodiment, fluoroethylene carbonate and vinylene carbonate can form a dense solid electrolyte interface film on the surface of the silicon-carbon negative electrode; additives such as vinyl sulfite and propylene sulfite can assist in film formation at the positive and negative electrodes, and have high thermal stability. The present invention further improves the high-temperature storage performance and cycle performance of the battery by adding a film former and additive A to the electrolyte and utilizing the synergistic effect between the film former and additive A.

[0034] In one embodiment, the mass percentage of the film-forming agent in the electrolyte is 3%-5%. In this embodiment, if the content of the film-forming agent is too little, it is easy to cause the film-forming agent to form a dense solid electrolyte interface film on the surface of the silicon-carbon negative electrode. The effect is not ideal. If the content of the film-forming agent is too much, it is easy to cause the impedance to be too large and aggravate the high-temperature gas production. Optionally, the mass percentage of the film-forming agent in the electrolyte can be any one of 3%, 3.5%, 4%, 4.5%, 5%, etc., or a range between any two.

[0035] In one embodiment, the lithium salt includes at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium hexafluoroarsenate, lithium difluorophosphate, lithium trifluoromethanesulfonate, and lithium bis(fluorosulfonyl)imide.

[0036] In one embodiment, the mass percentage of lithium salt in the electrolyte is 12%-15%. Optionally, the mass percentage of lithium salt in the electrolyte can be any one of 12%, 12.5%, 13%, 13.5%, 14%, 14.5%, 15%, etc., or a range between any two.

[0037] In one embodiment, the organic solvent includes ethylene carbonate, dimethyl carbonate, and ethyl methyl carbonate, and the mass ratio of ethylene carbonate, dimethyl carbonate, and ethyl methyl carbonate is (1-3):(1-3):(4-8). Optionally, the mass ratio of ethylene carbonate, dimethyl carbonate, and ethyl methyl carbonate can be any one of 1:1:4, 1:1:6, 1:1:8, 1:2:4, 1:3:4, 3:1:8, 3:3:8, etc., or a range between any two of them.

[0038] In one embodiment, the mass percentage of the organic solvent in the electrolyte is 70%-80%. Optionally, the mass percentage of the organic solvent in the electrolyte can be any one of 70%, 72%, 74%, 76%, 78%, 80%, etc. or a range between any two.

[0039] The present application also provides a method for preparing the electrolyte as described above, comprising the following steps:

[0040] S1. Under a protective atmosphere, uniformly mix the formulated amount of organic solvent, lithium salt, additive A and other raw materials to obtain the electrolyte.

[0041] The preparation method provided by the invention has simple operation and short process and can meet the needs of industrial large-scale production.

[0042] In one embodiment, the other raw materials further include a film-forming agent.

[0043] In one embodiment, the protective atmosphere includes a nitrogen atmosphere and / or an argon atmosphere.

[0044] In one embodiment, the mixing is stirring mixing, the mixing temperature is 25°C-30°C, and the mixing time is 50min-60min. In this embodiment, the mixing temperature is 25°C-30°C, which can reduce the decomposition of lithium salt, additive A and film-forming agent at high temperature. Optionally, the mixing temperature can be any one of 25°C, 26°C, 27°C, 28°C, 29°C, 30°C, etc. or a range between any two; the mixing time can be any one of 50min, 52min, 54min, 56min, 58min, 60min, etc. or a range between any two.

[0045] The present application also provides a lithium-ion battery, which includes the electrolyte as described above or the electrolyte prepared by the method as described above.

[0046] In this embodiment, the electrolyte of the lithium-ion battery contains additive A. On the one hand, the structure of additive A contains fluorine atoms, which can form a solid electrolyte interface film containing inorganic substances such as lithium fluoride on the surface of the negative electrode during the charge and discharge process of the battery. Lithium fluoride makes the formed solid electrolyte interface film have high mechanical strength and stability, which can inhibit the volume expansion of the silicon-carbon negative electrode during the charge and discharge process, and reduce the damage to the solid electrolyte interface film caused by the stress generated by the volume expansion of the silicon-carbon negative electrode during the charge and discharge process; in addition, the structure of additive A contains carbonyl groups, which can undergo polymerization reaction on the surface of the negative electrode to form a polycarbonate polymer film. The polycarbonate polymer film can reduce the direct contact between the electrolyte and the negative electrode material, reduce the decomposition of the negative electrode material, and at the same time alleviate the damage to the electrode structure caused by the volume expansion of the silicon-carbon negative electrode material; on the other hand, the structure of additive A The structure of additive A contains boron atoms, and additive A can be oxidized and decomposed during the charge and discharge process, thereby forming a stable borate film on the surface of the silicon-carbon negative electrode. The borate film has good flexibility and mechanical strength, can adapt to the volume change of the silicon-carbon negative electrode during the charge and discharge process, and improve the flexibility of the solid electrolyte interface film, thereby reducing the rupture of the solid electrolyte interface film on the surface of the silicon-carbon negative electrode and reducing the occurrence of side reactions between the electrolyte and the silicon-carbon negative electrode; in addition, the structure of additive A contains siloxane groups, which can effectively form a Si-O-Si cross-linked structure on the surface of the silicon-carbon negative electrode, which can enhance the toughness of the solid electrolyte interface film on the surface of the silicon-carbon negative electrode and effectively inhibit the expansion of the silicon-carbon negative electrode; in addition, the structure of additive A contains benzene rings, and additive A can form a protective film on the positive electrode surface, which can reduce the side reactions between the electrolyte and the positive electrode under high voltage systems. Additive A can improve the mechanical strength, toughness and stability of the solid electrolyte interface film on the surface of the silicon-carbon negative electrode, thereby improving the cycle performance and storage performance of the battery.

[0047] In one embodiment, the lithium-ion battery further comprises a positive electrode, a negative electrode and a separator; the material of the positive electrode comprises lithium iron manganese phosphate and / or nickel-cobalt-manganese ternary material; the material of the negative electrode comprises silicon-carbon material.

[0048] The above scheme is further described below in conjunction with specific implementation examples. The preferred embodiments of the present application are described in detail as follows:

[0049] Example 1

[0050] This embodiment provides an electrolyte, which is composed of an organic solvent, a lithium salt, a film-forming agent and an additive A;

[0051] The organic solvent is composed of ethylene carbonate, dimethyl carbonate and ethyl methyl carbonate, the mass ratio of ethylene carbonate, dimethyl carbonate and ethyl methyl carbonate is 15:15:70, and the mass fraction of the organic solvent in the electrolyte is 79.5%;

[0052] The lithium salt is lithium hexafluorophosphate, and the mass fraction of the lithium salt in the electrolyte is 12.5%;

[0053] The film-forming agent is vinylene carbonate, and the mass fraction of the film-forming agent in the electrolyte is 3%;

[0054] The mass fraction of additive A in the electrolyte is 5%.

[0055] This embodiment also provides a method for preparing the above electrolyte, and the specific method is as follows:

[0056] (1) Under an argon atmosphere, a lithium salt in a prescribed amount is added to an organic solvent, and then a film-forming agent is added, and finally an additive A is added, and the mixture is stirred at 25° C. to obtain an electrolyte.

[0057] Example 2

[0058] This embodiment provides an electrolyte, which is composed of an organic solvent, a lithium salt, a film-forming agent and an additive A;

[0059] The organic solvent is composed of ethylene carbonate, dimethyl carbonate and ethyl methyl carbonate, the mass ratio of ethylene carbonate, dimethyl carbonate and ethyl methyl carbonate is 15:15:70, and the mass fraction of the organic solvent in the electrolyte is 77.5%;

[0060] The lithium salt is lithium hexafluorophosphate, and the mass fraction of the lithium salt in the electrolyte is 12.5%;

[0061] The film-forming agent is vinylene carbonate, and the mass fraction of the film-forming agent in the electrolyte is 3%;

[0062] The mass fraction of additive A in the electrolyte is 7%.

[0063] This embodiment also provides a method for preparing the above electrolyte, and the specific method is as follows:

[0064] (1) Under an argon atmosphere, a lithium salt in a prescribed amount is added to an organic solvent, and then a film-forming agent is added, and finally an additive A is added, and the mixture is stirred at 25° C. to obtain an electrolyte.

[0065] Example 3

[0066] This embodiment provides an electrolyte, which is composed of an organic solvent, a lithium salt, a film-forming agent and an additive A;

[0067] The organic solvent is composed of ethylene carbonate, dimethyl carbonate and ethyl methyl carbonate, the mass ratio of ethylene carbonate, dimethyl carbonate and ethyl methyl carbonate is 15:15:70, and the mass fraction of the organic solvent in the electrolyte is 75.5%;

[0068] The lithium salt is lithium hexafluorophosphate, and the mass fraction of the lithium salt in the electrolyte is 12.5%;

[0069] The film-forming agent is vinylene carbonate, and the mass fraction of the film-forming agent in the electrolyte is 3%;

[0070] The mass fraction of additive A in the electrolyte is 9%.

[0071] This embodiment also provides a method for preparing the above electrolyte, and the specific method is as follows:

[0072] (1) Under an argon atmosphere, a lithium salt in a prescribed amount is added to an organic solvent, and then a film-forming agent is added, and finally an additive A is added, and the mixture is stirred at 25° C. to obtain an electrolyte.

[0073] Example 4

[0074] This embodiment provides an electrolyte, which is composed of an organic solvent, a lithium salt, a film-forming agent and an additive A;

[0075] The organic solvent is composed of ethylene carbonate, dimethyl carbonate and ethyl methyl carbonate, the mass ratio of ethylene carbonate, dimethyl carbonate and ethyl methyl carbonate is 15:15:70, and the mass fraction of the organic solvent in the electrolyte is 76.5%;

[0076] The lithium salt is lithium hexafluorophosphate, and the mass fraction of the lithium salt in the electrolyte is 12.5%;

[0077] The film-forming agent is vinylene carbonate, and the mass fraction of the film-forming agent in the electrolyte is 4%;

[0078] The mass fraction of additive A in the electrolyte is 7%.

[0079] This embodiment also provides a method for preparing the above electrolyte, and the specific method is as follows:

[0080] (1) Under an argon atmosphere, a lithium salt in a prescribed amount is added to an organic solvent, and then a film-forming agent is added, and finally an additive A is added, and the mixture is stirred at 25° C. to obtain an electrolyte.

[0081] Example 5

[0082] This embodiment provides an electrolyte, which is composed of an organic solvent, a lithium salt, a film-forming agent and an additive A;

[0083] The organic solvent is composed of ethylene carbonate, dimethyl carbonate and ethyl methyl carbonate, the mass ratio of ethylene carbonate, dimethyl carbonate and ethyl methyl carbonate is 15:15:70, and the mass fraction of the organic solvent in the electrolyte is 75.5%;

[0084] The lithium salt is lithium hexafluorophosphate, and the mass fraction of the lithium salt in the electrolyte is 12.5%;

[0085] The film-forming agent is vinylene carbonate, and the mass fraction of the film-forming agent in the electrolyte is 5%;

[0086] The mass fraction of additive A in the electrolyte is 7%.

[0087] This embodiment also provides a method for preparing the above electrolyte, and the specific method is as follows:

[0088] (1) Under an argon atmosphere, a lithium salt in a prescribed amount is added to an organic solvent, and then a film-forming agent is added, and finally an additive A is added, and the mixture is stirred at 25° C. to obtain an electrolyte.

[0089] Example 6

[0090] This embodiment provides an electrolyte, which is composed of an organic solvent, a lithium salt, a film-forming agent and an additive A;

[0091] The organic solvent is composed of ethylene carbonate, dimethyl carbonate and ethyl methyl carbonate, the mass ratio of ethylene carbonate, dimethyl carbonate and ethyl methyl carbonate is 15:15:70, and the mass fraction of the organic solvent in the electrolyte is 81.5%;

[0092] The lithium salt is lithium hexafluorophosphate, and the mass fraction of the lithium salt in the electrolyte is 12.5%;

[0093] The film-forming agent is vinylene carbonate, and the mass fraction of the film-forming agent in the electrolyte is 3%;

[0094] The mass fraction of additive A in the electrolyte is 3%.

[0095] This embodiment also provides a method for preparing the above electrolyte, and the specific method is as follows:

[0096] (1) Under an argon atmosphere, a lithium salt in a prescribed amount is added to an organic solvent, and then a film-forming agent is added, and finally an additive A is added, and the mixture is stirred at 25° C. to obtain an electrolyte.

[0097] Example 7

[0098] This embodiment provides an electrolyte, which is composed of an organic solvent, a lithium salt, a film-forming agent and an additive A;

[0099] The organic solvent is composed of ethylene carbonate, dimethyl carbonate and ethyl methyl carbonate, the mass ratio of ethylene carbonate, dimethyl carbonate and ethyl methyl carbonate is 15:15:70, and the mass fraction of the organic solvent in the electrolyte is 72.5%;

[0100] The lithium salt is lithium hexafluorophosphate, and the mass fraction of the lithium salt in the electrolyte is 12.5%;

[0101] The film-forming agent is vinylene carbonate, and the mass fraction of the film-forming agent in the electrolyte is 3%;

[0102] The mass fraction of additive A in the electrolyte is 12%.

[0103] This embodiment also provides a method for preparing the above electrolyte, and the specific method is as follows:

[0104] (1) Under an argon atmosphere, a lithium salt in a prescribed amount is added to an organic solvent, and then a film-forming agent is added, and finally an additive A is added, and the mixture is stirred at 25° C. to obtain an electrolyte.

[0105] Example 8

[0106] This embodiment provides an electrolyte, which is composed of an organic solvent, a lithium salt, a film-forming agent and an additive A;

[0107] The organic solvent is composed of ethylene carbonate, dimethyl carbonate and ethyl methyl carbonate, the mass ratio of ethylene carbonate, dimethyl carbonate and ethyl methyl carbonate is 15:15:70, and the mass fraction of the organic solvent in the electrolyte is 78.5%;

[0108] The lithium salt is lithium hexafluorophosphate, and the mass fraction of the lithium salt in the electrolyte is 12.5%;

[0109] The film-forming agent is vinylene carbonate, and the mass fraction of the film-forming agent in the electrolyte is 2%;

[0110] The mass fraction of additive A in the electrolyte is 7%.

[0111] This embodiment also provides a method for preparing the above electrolyte, and the specific method is as follows:

[0112] (1) Under an argon atmosphere, a lithium salt in a prescribed amount is added to an organic solvent, and then a film-forming agent is added, and finally an additive A is added, and the mixture is stirred at 25° C. to obtain an electrolyte.

[0113] Example 9

[0114] This embodiment provides an electrolyte, which is composed of an organic solvent, a lithium salt, a film-forming agent and an additive A;

[0115] The organic solvent is composed of ethylene carbonate, dimethyl carbonate and ethyl methyl carbonate, the mass ratio of ethylene carbonate, dimethyl carbonate and ethyl methyl carbonate is 15:15:70, and the mass fraction of the organic solvent in the electrolyte is 73.5%;

[0116] The lithium salt is lithium hexafluorophosphate, and the mass fraction of the lithium salt in the electrolyte is 12.5%;

[0117] The film-forming agent is vinylene carbonate, and the mass fraction of the film-forming agent in the electrolyte is 7%;

[0118] The mass fraction of additive A in the electrolyte is 7%.

[0119] This embodiment also provides a method for preparing the above electrolyte, and the specific method is as follows:

[0120] (1) Under an argon atmosphere, a lithium salt in a prescribed amount is added to an organic solvent, and then a film-forming agent is added, and finally an additive A is added, and the mixture is stirred at 25° C. to obtain an electrolyte.

[0121] Example 10

[0122] This embodiment provides an electrolyte, which is composed of an organic solvent, a lithium salt, a film-forming agent and an additive A;

[0123] The organic solvent is composed of ethylene carbonate, dimethyl carbonate and ethyl methyl carbonate, the mass ratio of ethylene carbonate, dimethyl carbonate and ethyl methyl carbonate is 15:15:70, and the mass fraction of the organic solvent in the electrolyte is 74.5%;

[0124] The lithium salt is lithium hexafluorophosphate, and the mass fraction of the lithium salt in the electrolyte is 12.5%;

[0125] The film-forming agent is vinylene carbonate, and the mass fraction of the film-forming agent in the electrolyte is 3%;

[0126] The mass fraction of additive A in the electrolyte is 10%.

[0127] This embodiment also provides a method for preparing the above electrolyte, and the specific method is as follows:

[0128] (1) Under an argon atmosphere, a lithium salt in a prescribed amount is added to an organic solvent, and then a film-forming agent is added, and finally an additive A is added, and the mixture is stirred at 25° C. to obtain an electrolyte.

[0129] Comparative Example 1

[0130] The difference between Comparative Example 1 and Example 1 is:

[0131] The mass fraction of lithium salt in the electrolyte is 12.5%, the mass fraction of organic solvent in the electrolyte is 84.5%, the mass fraction of film-forming agent in the electrolyte is 3%, the mass fraction of additive A in the electrolyte is 0, and the rest is the same as in Example 1.

[0132] Comparative Example 2

[0133] The difference between Comparative Example 2 and Example 1 is:

[0134] The mass fraction of lithium salt in the electrolyte is 12.5%, the mass fraction of organic solvent in the electrolyte is 80.5%, the mass fraction of film-forming agent in the electrolyte is 0, the mass fraction of additive A in the electrolyte is 7%, and the rest is the same as in Example 1.

[0135] Test Method

[0136] The electrolytes prepared in Examples 1 to 10 and Comparative Examples 1 and 2 were injected with LiMn 0.5 Fe 0.5 In the PO4-silicon-carbon system lithium-ion battery, performance testing is carried out using lithium-ion batteries.

[0137] (I) The method for making a lithium-ion battery is:

[0138] Production of positive electrode:

[0139] The positive electrode active material LiMn 0.5 Fe 0.5 PO4, conductive agent acetylene black, and binder polyvinylidene fluoride (PVDF) are fully stirred and mixed in N-methylpyrrolidone (NMP) solvent in a weight ratio of 96:2:2 to form a uniform positive electrode slurry; the slurry is coated on the positive electrode current collector aluminum foil, dried, and cold pressed to obtain a positive electrode sheet.

[0140] Negative electrode production:

[0141] The negative electrode active material silicon carbon, the conductive agent acetylene black, the binder hexylene rubber (SBR), and the thickener sodium carboxymethyl cellulose (CMC) are fully stirred and mixed in a proper amount of deionized water solvent at a weight ratio of 95:2:2:1 to form a uniform anode slurry; the slurry is coated on the anode current collector copper foil, dried, and cold pressed to obtain a negative electrode sheet.

[0142] Lithium-ion battery production:

[0143] The positive electrode sheet, PE separator, and negative electrode sheet are stacked in order, and then wound to obtain a bare battery cell; the bare battery cell is placed in an outer packaging bag, and the electrolytes obtained in Examples 1-10 and Comparative Examples 1-2 are respectively injected into the dried battery, and a lithium-ion battery is obtained through vacuum packaging, standing, formation, shaping and other processes.

[0144] (ii) 60℃ storage 30d test:

[0145] The lithium-ion battery was charged to 4.5V at 1.0C constant current and constant voltage at 25°C, left to stand for 5 minutes, and then discharged to 2.5V at 0.1C. The released capacity was recorded as the initial capacity C0. Then, it was charged to 4.5V at 1.0C constant current and constant voltage, and the initial thickness was measured, which was recorded as T0. After that, the battery was stored at 60°C±2°C. After 30 days of open circuit storage, the battery was taken out and the hot thickness T1 was tested. Then, the battery was charged and discharged at 1.0C, and the remaining capacity C1 and the recovery capacity C2 were tested. Then, the thermal thickness change rate, capacity retention rate, and capacity recovery rate were calculated. The calculation formula is as follows:

[0146] Capacity retention rate of lithium-ion battery after storage at 60°C for 30 days (%) = (C1 / C0) × 100%;

[0147] Capacity recovery rate of lithium-ion battery after storage at 60°C for 30 days (%) = (C2 / C0) × 100%;

[0148] The thermal thickness change rate (%) of the lithium-ion battery after storage at 60°C for 30 days = (T1-T0) / T0×100%.

[0149] (III) 25℃ 1C charge and discharge cycle test:

[0150] At 25°C, the lithium-ion battery is charged at a constant current of 1C (nominal capacity) to a voltage of 4.2V, then charged at a constant voltage of 4.2V to a current ≤ 0.05C, left for 10 minutes, and then discharged at a constant current of 1C to a cut-off voltage of 2.8V. The above is one charge and discharge cycle. The lithium-ion battery is subjected to 1000 charge and discharge cycles at 25°C under the above conditions.

[0151] The capacity retention rate (%) of a lithium-ion battery after N cycles = (discharge capacity at the Nth cycle / initial discharge capacity) × 100%, where N is the number of cycles of the lithium-ion battery.

[0152] The test results are shown in Table 1 below:

[0153] Table 1

[0154]

[0155]

[0156] According to the test results in Table 1, the electrolyte provided in the embodiment contains additive A, which can participate in the negative electrode film formation, improve the mechanical strength and toughness of the solid electrolyte interface film on the surface of the negative electrode, inhibit the volume expansion of the silicon-carbon negative electrode during the charge and discharge process, reduce the stress caused by the volume expansion of the silicon-carbon negative electrode during the charge and discharge process. The damage to the solid electrolyte interface film reduces the side reaction between the electrolyte and the silicon-carbon negative electrode, and improves the battery cycle performance and storage performance.

[0157] From the analysis of Example 1, Example 2, Example 3, Example 10, Example 6 and Example 7, it can be known that by controlling the mass percentage of additive A in the electrolyte within an appropriate range, gas production and battery impedance can be reduced, the mechanical strength and toughness of the solid electrolyte interface film on the surface of the negative electrode can be ensured, and the cycle performance and storage performance of the battery can be improved.

[0158] From the analysis of Example 1, Example 4, Example 5, Example 8 and Example 9, it can be known that by controlling the mass percentage of the film-forming agent in the electrolyte within an appropriate range, gas production and battery impedance can be reduced, thereby ensuring the mechanical strength and toughness of the solid electrolyte interface film on the surface of the negative electrode, which is more conducive to improving the cycle performance and storage performance of the battery.

[0159] From the analysis of Examples 1 to 10 and Comparative Example 2, it can be seen that by adding a film former and additive A to the electrolyte and utilizing the synergistic effect between the film former and additive A, the storage performance and cycle performance of the battery can be further improved.

[0160] The embodiments of the present invention are described in detail above. Specific examples are used herein to illustrate the principles and implementation methods of the present invention. The description of the above embodiments is only used to help understand the method of the present invention and its core idea. At the same time, for those skilled in the art, according to the idea of ​​the present invention, there will be changes in the specific implementation methods and application scope. In summary, the content of this specification should not be understood as a limitation on the present invention.

Claims

1. An electrolyte, characterized in that: Including organic solvent, lithium salt and additive A; The structure of the additive A includes fluorine atoms, boron atoms, carbonyl groups, siloxane groups and benzene rings.

2. The electrolyte according to claim 1, characterized in that The structure of the additive A is shown in Formula I:

3. The electrolyte according to claim 1 or 2, characterized in that The mass percentage of the additive A in the electrolyte is 5%-10%.

4. The electrolyte according to claim 1 or 2, characterized in that The electrolyte further includes a film former, and the film former includes at least one of vinyl sulfite, propylene sulfite, fluoroethylene carbonate, and vinylene carbonate.

5. The electrolyte according to claim 4, characterized in that The mass percentage of the film-forming agent in the electrolyte is 3%-5%.

6. The electrolyte according to claim 1 or 2, characterized in that The lithium salt comprises at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium hexafluoroarsenate, lithium difluorophosphate, lithium trifluoromethanesulfonate, and lithium bis(fluorosulfonyl)imide; and / or The mass percentage of the lithium salt in the electrolyte is 12%-15%.

7. The electrolyte according to claim 1 or 2, characterized in that: The organic solvent comprises ethylene carbonate, dimethyl carbonate and ethyl methyl carbonate, and the mass ratio of the ethylene carbonate, the dimethyl carbonate and the ethyl methyl carbonate is (1-3):(1-3):(4-8); and / or The mass percentage of the organic solvent in the electrolyte is 70%-80%.

8. A method for preparing an electrolyte according to any one of claims 1 to 7, characterized in that: The method comprises the following steps: Under a protective atmosphere, the organic solvent, lithium salt, additive A and other raw materials in the formulated amounts are mixed evenly to obtain the electrolyte.

9. The method for preparing an electrolyte according to claim 8, characterized in that: The other raw materials include film formers.

10. The method for preparing an electrolyte according to claim 8 or 9, characterized in that: The mixing is stirring mixing, the mixing temperature is 25° C.-30° C., and / or the mixing time is 50 min-60 min; and / or The protective atmosphere includes a nitrogen atmosphere and / or an argon atmosphere.

11. A lithium ion battery, characterized in that: The lithium-ion battery comprises the electrolyte according to any one of claims 1 to 7 or the electrolyte prepared by the method according to any one of claims 8 to 10.

12. The lithium ion battery according to claim 11, characterized in that The lithium-ion battery also includes a positive electrode, a negative electrode and a separator; The material of the positive electrode includes lithium iron manganese phosphate and / or nickel-cobalt-manganese ternary material, and / or the material of the negative electrode includes silicon-carbon material.

Citation Information

Patent Citations

  • Lithium ion battery electrolyte and lithium ion battery containing same

    CN113140796A

  • HIGH VOLTAGE ELECTROLYTE (Muldoon, Allred)

    US20100209780A1

  • Substituted 1 h-pyrrolopyridinone derivatives as kinase inhibitors

    WO2014125408A2

  • Lithium-ion battery electrolyte and lithium-ion battery

    WO2024114166A1