Battery cell, battery device, and electric device
By adding a lithium replenishing agent to the positive electrode film layer of the battery cell and adding a compound of organic and inorganic lithium salts to the electrolyte, CEI and SEI films are formed, which solves the problem that the battery cannot simultaneously meet the requirements of long life and high power, and improves the cycle performance and dynamic performance of the battery.
Patent Information
- Application Number
- CN202411161598.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2044-08-22
AI Technical Summary
Existing battery technology cannot simultaneously meet the requirements of long lifespan and high power.
By adding a lithium supplement to the positive electrode film layer of the battery cell and adding a compound of organic and inorganic lithium salts to the electrolyte, a dense solid electrolyte interphase (CEI) film and a low-resistance solid electrolyte interphase (SEI) film are formed to improve the cycle performance and power performance of the battery.
It improves the cycle performance and power performance of individual battery cells, reduces the risk of electrolyte oxidation and decomposition, and enhances the lithium-ion insertion/extraction rate and battery kinetic performance.
Smart Images

Figure CN119994197B_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of batteries, specifically to battery cells, battery devices, and electrical equipment. Background Technology
[0002] Batteries are not only used in energy storage systems for hydropower, thermal power, wind power, and solar power plants, but also widely used in electric vehicles such as electric bicycles, electric motorcycles, and electric cars, as well as in military equipment and aerospace. However, current battery technologies cannot simultaneously meet the demands for long lifespan and high power output. Summary of the Invention
[0003] The first aspect of this application provides a battery cell, the battery cell comprising a positive electrode sheet, the positive electrode sheet comprising a positive electrode film layer comprising lithium iron phosphate material and a lithium replenishing agent; a negative electrode sheet, the negative electrode sheet comprising a negative electrode film layer comprising a negative electrode active material comprising graphite; a separator membrane located between the positive electrode sheet and the negative electrode sheet; and an electrolyte comprising a lithium salt, the lithium salt comprising an organic lithium salt and an inorganic lithium salt, the organic lithium salt comprising at least one of lithium fluorosulfonylimide, lithium fluorooxalate borate, and lithium fluorooxalate phosphate, the inorganic lithium salt comprising at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, and lithium fluorosulfonate, the mass ratio of the inorganic lithium salt to the organic lithium salt being (6-2):1. Thus, on the one hand, while improving the cycle performance of the battery cell, a dense solid electrolyte interphase (CEI) film is formed on the surface of the lithium replenisher, reducing the risk of electrolyte oxidation and decomposition and improving the cycle performance of the battery; on the other hand, the combination of organic lithium salt and inorganic lithium salt can form a solid electrolyte interphase (SEI) film with low impedance and good toughness on the graphite surface, thereby improving the power performance of the battery cell.
[0004] According to some embodiments of this application, the organic lithium salt includes at least one of lithium bis(fluorosulfonyl)imide and lithium bis(trifluorosulfonyl)imide, and the mass percentage of the organic lithium salt is 1%-4% based on the total mass of the electrolyte.
[0005] According to some embodiments of this application, the inorganic lithium salt includes lithium hexafluorophosphate, and the mass percentage of the inorganic lithium salt is 7.5%-12% based on the total mass of the electrolyte.
[0006] Therefore, by keeping the contents of organic and inorganic lithium salts within the above range, a low-resistance and tough SEI film is formed on the negative electrode surface, which improves the lithium ion insertion / extraction rate, reduces the probability of SEI film damage caused by graphite expansion, and improves the cycle performance of the battery cell.
[0007] According to some embodiments of this application, the OI value of the graphite is 2-5. Therefore, by reducing the OI value of the graphite, the lithium insertion / extraction rate is increased, thereby improving the kinetic performance of the battery cell.
[0008] According to some embodiments of this application, the volume average particle size Dv50 of the graphite is 8 μm-14 μm. Therefore, by reducing the volume average particle size of the graphite, the lithium insertion / extraction rate is increased, thereby improving the kinetic performance of the battery cell.
[0009] According to some embodiments of this application, the graphite includes artificial graphite. Therefore, artificial graphite has a relatively small number of active sites, which can improve the cycle life of the battery cell.
[0010] According to some embodiments of this application, the lithium supplement includes Li x M y O z M includes at least one of Ni, Co, V, Cr, Mn, Fe, Mo, Cu, and Zn, where 0 < x ≤ 5, 1 ≤ y ≤ 3, and 2 ≤ z ≤ 8.
[0011] According to some embodiments of this application, the lithium replenishing agent includes at least one of Li2NiO2 and Li5FeO4.
[0012] According to some embodiments of this application, the lithium supplement includes Li n NiO m Li e FeO f At least one of the following, wherein 0 < m ≤ 2, 0 ≤ n ≤ 2, 0 ≤ e ≤ 5, and 0 < f ≤ 4.
[0013] According to some embodiments of this application, the lithium supplement includes NiO. m and Li p FeO q At least one of the following, wherein 0 < m ≤ 2, 0 ≤ p ≤ 1, and 0 < q ≤ 2.
[0014] Therefore, the decomposition of lithium replenishment agents can compensate for the active lithium ions consumed in the formation of the SEI film, thereby improving the initial efficiency and energy density of the battery cell.
[0015] According to some embodiments of this application, the electrolyte further includes a solvent, which comprises cyclic carbonates and linear carbonates. This increases the dielectric constant of the electrolyte, reduces its viscosity, and improves the migration rate of lithium ions.
[0016] According to some embodiments of this application, based on the total mass of the electrolyte, the cyclic carbonate accounts for 15%-25% of the mass, and the linear carbonate accounts for 50%-70% of the mass. This increases the dielectric constant of the electrolyte, reduces its viscosity, and improves the migration rate of lithium ions.
[0017] According to some embodiments of this application, the cyclic carbonate includes at least one of ethylene carbonate or propylene carbonate; and / or the linear carbonate includes at least one of dimethyl carbonate, ethyl methyl carbonate, and diethyl carbonate.
[0018] According to some embodiments of this application, the linear carbonate comprises dimethyl carbonate and ethyl methyl carbonate, wherein the mass percentage of dimethyl carbonate is 30%-40% and the mass percentage of ethyl methyl carbonate is 30%-40% based on the total mass of the electrolyte. This reduces the viscosity of the electrolyte.
[0019] According to some embodiments of this application, the electrolyte comprises a linear carboxylic acid ester, and the mass percentage of the linear carboxylic acid ester is 5%-15% based on the total mass of the electrolyte. This improves the conductivity of the electrolyte and enhances the kinetic performance of the battery cell.
[0020] According to some embodiments of this application, the linear carboxylic acid ester includes at least one selected from methyl formate, methyl acetate, ethyl formate, and ethyl acetate. This improves the conductivity of the electrolyte and enhances the kinetic performance of the battery cell.
[0021] According to some embodiments of this application, the electrolyte further includes additives, which include at least one of fluorine-containing additives or phosphorus-containing additives. This forms a stable CEI film on the positive electrode surface, reducing the risk of continuous gas generation from electrolyte decomposition caused by high voltage during the formation stage.
[0022] According to some embodiments of this application, the additives include fluorine-containing additives and phosphorus-containing additives, and the sum of the masses of the fluorine-containing additives and the phosphorus-containing additives accounts for 0.05%-1% based on the total mass of the electrolyte. This forms a stable CEI film on the positive electrode surface, reducing the risk of continuous gas generation from electrolyte decomposition caused by high voltage during the formation stage.
[0023] According to some embodiments of this application, based on the total mass of the electrolyte, the mass percentage of the fluorine-containing additive is 0.05%-0.5%, and the mass percentage of the phosphorus-containing additive is 0.05%-0.5%. This forms a stable CEI film on the positive electrode surface, reducing the risk of continuous gas generation from electrolyte decomposition caused by high voltage during the formation stage.
[0024] According to some embodiments of this application, the fluorinated additive includes at least one of fluoroethylene carbonate, difluoroethylene carbonate, and perfluoroalkyl ethylene carbonate; and / or the phosphorus-containing additive includes at least one of tris(trimethylsilyl)phosphate, triphenylphosphine oxide, tris(2,2,2-trifluoroethyl) phosphite, trimethylolpropane, tris(2,2,2-trifluoroethyl) phosphate, and 2-trifluoroethoxy-2-oxo-1,3,2-dioxophosphazenecyclopentane. This forms a stable CEI film on the positive electrode surface, reducing the risk of continuous gas generation from electrolyte decomposition caused by high voltage during the formation stage.
[0025] According to some embodiments of this application, the additive further includes carbonate additives, including at least one selected from vinylene carbonate, propylene carbonate, and vinyl ethylene carbonate. This increases the polymer content in the SEI film, improves the stability of the SEI film, and enhances the cycle life of the battery cell.
[0026] According to some embodiments of this application, the carbonate additive includes vinylene carbonate, and the mass percentage of vinylene carbonate is 0.5%-3% based on the total mass of the electrolyte. This allows for the formation of a polymer-containing SEI film on the negative electrode surface, improving the stability of the SEI film and increasing the lifespan of the battery cell.
[0027] According to some embodiments of this application, at least a portion of the surface of the lithium iron phosphate has a first carbon coating layer, the mass percentage of which is 0.5%-1.5% based on the total mass of the lithium iron phosphate; and / or at least a portion of the surface of the lithium supplement has a second carbon coating layer, the mass percentage of which is 1%-5% based on the total mass of the lithium supplement. Thus, carbon coating of at least a portion of the surface of the lithium iron phosphate can improve the electronic conductivity of the electrode; carbon coating of at least a portion of the surface of the lithium supplement can reduce the number of exposed active sites, thereby reducing the probability of reaction with the electrolyte.
[0028] According to some embodiments of this application, the mass percentage of the lithium replenishing agent is 0.5%-5% based on the total mass of the positive electrode film. This improves the lithium replenishment effect and increases the energy density of the battery cell.
[0029] According to some embodiments of this application, the coating weight of the positive electrode film is 10 mg / cm³. 2 -25mg / cm 2 .
[0030] According to some embodiments of this application, the compaction density of the positive electrode film is 2.2 g / cm³. 3 -2.6g / cm 3 .
[0031] Therefore, by keeping the coating weight and compaction density of the positive electrode film within the above range, the energy density of the battery cell can be increased.
[0032] According to some embodiments of this application, the coating weight of the negative electrode film is 5 mg / cm³. 2 -15mg / cm 2 .
[0033] According to some embodiments of this application, the compaction density of the negative electrode film is 1.2 g / cm³. 3 -1.7g / cm 3 .
[0034] Therefore, by keeping the coating weight and compaction density of the negative electrode film within the above range, the energy density of the battery cell can be increased.
[0035] According to some embodiments of this application, the separator includes a base film, at least one side of which has a coating. This reduces the risk of oxidation of the base film due to high pressure during formation.
[0036] According to some embodiments of this application, the thickness of the separator is 7μm-15μm. This reduces the risk of oxidation of the base film due to high pressure during formation.
[0037] According to some embodiments of this application, the electrolyte injection coefficient of the battery cell is 3g / Ah-3.8g / Ah. This increases the electrolyte content in the battery cell and improves its kinetic performance.
[0038] The second aspect of this application provides a battery device, including the battery cell provided in the first aspect of this application, wherein the battery device is at least one of a battery module, a battery pack, and an energy storage device.
[0039] A third aspect of this application provides an electrical device, including a battery cell provided in the first aspect of this application or a battery device provided in the second aspect of this application, wherein the battery cell or the battery device is used to provide electrical energy.
[0040] Additional aspects and advantages of this application will be set forth in part in the description which follows, and in part will be obvious from the description, or may be learned by practice of this application. Attached Figure Description
[0041] Various other advantages and benefits will become apparent to those skilled in the art upon reading the detailed description of the preferred embodiments below. The accompanying drawings are for illustrative purposes only and are not intended to limit the scope of this application. Furthermore, the same reference numerals denote the same parts throughout the drawings. In the drawings:
[0042] Figure 1This is a schematic diagram of a battery cell according to one embodiment of this application.
[0043] Figure 2 yes Figure 1 An exploded view of a battery cell according to one embodiment of this application is shown.
[0044] Figure 3 This is a schematic diagram of a battery module according to one embodiment of this application.
[0045] Figure 4 This is a schematic diagram of a battery pack according to one embodiment of this application.
[0046] Figure 5 yes Figure 4 An exploded view of a battery pack according to one embodiment of this application is shown.
[0047] Figure 6 This is a schematic diagram of an electrical device using a battery device as a power source according to an embodiment of this application.
[0048] Explanation of reference numerals in the attached figures:
[0049] 1 Battery pack; 2 Upper housing; 3 Lower housing; 4 Battery module; 5 Battery cell; 51 Housing; 52 Electrode assembly; 53 Cover plate. Detailed Implementation
[0050] The embodiments of the technical solution of this application are described in detail below. The following embodiments are only used to illustrate the technical solution of this application more clearly, and are therefore only examples, and should not be used to limit the scope of protection of this application.
[0051] In this document, the term "embodiment" means that a particular feature, structure, or characteristic described in connection with an embodiment may be included in at least one embodiment of this application. The appearance of this phrase in various places throughout the specification does not necessarily refer to the same embodiment, nor is it a separate or alternative embodiment mutually exclusive with other embodiments. It will be explicitly and implicitly understood by those skilled in the art that the embodiments described herein can be combined with other embodiments.
[0052] Unless otherwise specified, all embodiments and optional embodiments of this application can be combined to form new technical solutions.
[0053] Unless otherwise specified, all technical features and optional technical features of this application may be combined to form new technical solutions.
[0054] Unless otherwise specified, all steps in this application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or it may include steps (b) and (a) performed sequentially. For example, the mention that the method may also include step (c) indicates that step (c) may be added to the method in any order. For example, the method may include steps (a), (b), and (c), or it may include steps (a), (c), and (b), or it may include steps (c), (a), and (b), etc.
[0055] Currently, judging from the development of the market, batteries are being used more and more widely, and can be applied to energy storage power systems such as hydropower, thermal power, wind power and solar power plants. However, the individual battery cells in related technologies cannot simultaneously meet the requirements of long life and high power.
[0056] This application aims to develop a battery cell that combines long lifespan and high power. By incorporating a lithium replenishing agent in the positive electrode film layer, the lithium loss caused by the formation of the SEI film during the formation stage is compensated, thereby improving the cycle performance of the battery cell. However, the lithium replenishing agent easily generates high-valence transition metal oxides in the battery cell, which pose a risk of electrolyte oxidation. Adding fluorine-containing organic lithium salts to the electrolyte can, on the one hand, promote the formation of a dense SEI film on the surface of high-valence transition metal oxides, reducing the risk of electrolyte oxidation and improving the cycle performance of the battery cell; on the other hand, the combination of organic and inorganic lithium salts can optimize the SEI film composition on the graphite surface, forming a low-impedance and high-toughness SEI film. This can not only increase the lithium-ion insertion / extraction rate in graphite but also effectively mitigate SEI film damage caused by graphite expansion during charging, thereby improving the power performance of the battery cell.
[0057] The battery cells proposed in this application can be used in electrical devices that use the battery cells as a power source or in various energy storage systems that use the battery cells as energy storage elements. Electrical devices can include, but are not limited to, mobile phones, tablets, laptops, electric toys, power tools, electric vehicles, electric cars, ships, spacecraft, etc. Electric toys can include stationary or mobile electric toys, such as game consoles, electric car toys, electric ship toys, and electric airplane toys, etc., while spacecraft can include airplanes, rockets, space shuttles, and spacecraft, etc.
[0058] The first aspect of this application discloses a battery cell, the battery cell comprising a positive electrode sheet, the positive electrode sheet comprising a positive electrode film layer comprising lithium iron phosphate material and a lithium replenishing agent; a negative electrode sheet, the negative electrode sheet comprising a negative electrode film layer comprising a negative electrode active material comprising graphite; a separator membrane located between the positive electrode sheet and the negative electrode sheet; and an electrolyte comprising a lithium salt, the lithium salt comprising an organic lithium salt and an inorganic lithium salt, the organic lithium salt comprising at least one of lithium fluorosulfonylimide, lithium fluorooxalate borate, and lithium fluorooxalate phosphate, the inorganic lithium salt comprising at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, and lithium fluorosulfonate, wherein the mass ratio of the inorganic lithium salt to the organic lithium salt is (6-2):1.
[0059] The battery cell proposed in this application improves the cycle performance of the battery cell by adding a lithium supplement in the positive electrode film layer. To reduce the risk of electrolyte oxidation by high-valence transition metal oxides formed by the lithium supplement, an organic lithium salt is added to the electrolyte. The organic lithium salt can promote the formation of a dense CEI film on the surface of the high-valence transition metal oxides, reducing the direct contact between the transition metal oxides and the electrolyte, reducing the risk of electrolyte oxidation and decomposition, and improving the cycle performance of the battery cell. The combination of organic and inorganic lithium salts can also form a low-resistance, tough SEI film on the negative electrode surface, thereby improving the power performance of the battery cell. Specifically, when the lower limit of the mass ratio of inorganic to organic lithium salt is less than 2:1, the organic lithium salt content is too high, which poses a risk of corrosion of the positive electrode current collector and a significant increase in the internal resistance of the battery cell; when the upper limit of the mass ratio of inorganic to organic lithium salt is greater than 6:1, the organic lithium salt content is too low, and a low-resistance, tough SEI film cannot be formed, which is detrimental to the long life and high power of the battery cell.
[0060] In this application, the test method for the content of organic lithium salt and inorganic lithium salt is as follows: weigh a quantitative amount of electrolyte from the battery cell, dilute it to 100 mL with ultrapure water, and perform automatic ion chromatography for detection, referring to standard JY / T 020-1996 or GB / T6040-2002.
[0061] As an example, the mass ratio of the inorganic lithium salt to the organic lithium salt is (6-2):1, for example, it can be 6:1, 5:1, 4:1, 3.65:1, 3:1 or 2:1, or it can be a range of any of the above values.
[0062] According to some specific embodiments of this application, the mass ratio of the inorganic lithium salt to the organic lithium salt is (4-3):1.
[0063]
Positive Electrode
[0064] The positive electrode includes a positive current collector and a positive electrode film layer located on at least one side of the positive current collector along its thickness direction, the positive electrode film layer including lithium iron phosphate material and lithium replenishment agent.
[0065] In some embodiments, the positive current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer substrate and a metal layer formed on at least one surface of the polymer substrate. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0066] According to some embodiments of this application, the lithium supplement includes Li x M y O z M includes at least one of Ni, Co, V, Cr, Mn, Fe, Mo, Cu, and Zn, where 0 < x ≤ 5, 1 ≤ y ≤ 3, and 2 ≤ z ≤ 8. Therefore, the decomposition of the lithium replenishment agent can compensate for the active lithium ions consumed in the formation of the SEI film, thereby improving the initial efficiency and energy density of the battery cell.
[0067] As an example, x can be 1, 2, 3, 4 or 5, or a range of any of the above values.
[0068] As an example, y can be 1, 1.5, 2, 2.5 or 3, or a range of any of the above values.
[0069] As an example, z can be 2, 3, 4, 5, 6, 7 or 8, or a range of any of the above values.
[0070] According to some embodiments of this application, the lithium replenishing agent includes at least one of Li2NiO2 and Li5FeO4. This improves the lithium replenishment effect.
[0071] According to some embodiments of this application, when all or part of the lithium in the lithium replenishing agent is extracted, the lithium replenishing agent includes Li n NiO m and Li e FeO f At least one of the following, wherein 0 < m ≤ 2, 0 ≤ n ≤ 2, 0 ≤ e ≤ 5, and 0 < f ≤ 4.
[0072] As an example, m can be 0.5, 1, 1.5 or 2, or a range of any of the above values.
[0073] As an example, n can be 0, 0.5, 1, 1.5 or 2, or a range of any of the above values.
[0074] As an example, e can be 0, 1, 2, 3, 4 or 5, or a range of any of the above values.
[0075] As an example, f can be 1, 2, 3, or 4, or a range of any of the above values.
[0076] According to some embodiments of this application, when all the lithium in the lithium replenishing agent is released, the lithium replenishing agent includes NiO. m and Li p FeO q At least one of the following, wherein 0 < m ≤ 2, 0 ≤ p ≤ 1, and 0 < q ≤ 2.
[0077] As an example, m can be 0.5, 1, 1.5 or 2, or a range of any of the above values.
[0078] As an example, p can be 0, 0.2, 0.4, 0.6, 0.8 or 1, or a range of any of the above values.
[0079] As an example, q can be 0.5, 1, 1.5 or 2, or a range of any of the above values.
[0080] This application provides a method for detecting lithium replenishing agents: after discharging a single battery cell to 2.0V at 0.1C, the cell is disassembled, and the positive electrode sheet is scraped to remove powder. The powder is then tested using an X-ray diffractometer (XRD), and at least one characteristic peak corresponding to a lithium replenishing agent is found in the spectrum.
[0081] According to some embodiments of this application, at least a portion of the surface of the lithium iron phosphate has a first carbon coating layer. Based on the total mass of the lithium iron phosphate, the mass percentage of the first carbon coating layer can be 0.5%-1.5%, for example, it can be 0.5%, 0.7%, 0.9%, 1.1%, 1.3%, or 1.5%, or any range of the above values. This improves the electronic conductivity between lithium iron phosphate particles, thereby enhancing the electronic conductivity of the electrode.
[0082] According to some embodiments of this application, at least a portion of the surface of the lithium replenishing agent has a second carbon coating layer. Based on the total mass of the lithium replenishing agent, the mass percentage of the second carbon coating layer can be 1%-5%, for example, 1%, 2%, 3%, 4%, or 5%, or any range of the above values. Thus, the second carbon coating layer on the surface of the lithium replenishing agent can accelerate the release of lithium ions from the lithium replenishing agent, rapidly forming pores on the electrode, allowing the electrolyte to quickly wet the electrode, improving lithium ion transport efficiency, and enhancing the kinetic performance of the battery cell. According to some specific embodiments of this application, based on the total mass of the lithium replenishing agent, the mass percentage of the second carbon coating layer can be 1%-5%. According to some specific embodiments of this application, based on the total mass of the lithium replenishing agent, the mass percentage of the second carbon coating layer can be 2%-4%.
[0083] According to some embodiments of this application, based on the total mass of the positive electrode film, the mass percentage of the lithium replenishing agent can be 0.5%-5%, for example, it can be 0.5%, 1%, 2%, 3%, 4%, or 5%, or any range of the above values. This improves the lithium replenishment effect.
[0084] In some embodiments, the positive electrode film layer may optionally include a binder. As an example, the binder may include at least one selected from polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), PVDF-tetrafluoroethylene-propylene terpolymer, PVDF-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorinated acrylate resin.
[0085] In some embodiments, the positive electrode film may optionally include a conductive agent. As an example, the conductive agent may include at least one selected from superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers. Further options include a combination of superconducting carbon and carbon nanotubes, thereby improving the electronic conductivity of the positive electrode.
[0086] According to some embodiments of this application, the coating weight of the positive electrode film can be 10 mg / cm³. 2 -25mg / cm 2 For example, it can be 10 mg / cm³ 2 12mg / cm 2 14mg / cm 2 16mg / cm 2 18.5 mg / cm 2 20mg / cm 2 22mg / cm 2 24mg / cm 2 Or 25mg / cm 2The values can be any range of the aforementioned values. Therefore, while increasing the energy density of the battery cell, the tortuosity of the positive electrode sheet is reduced, the lithium-ion diffusion rate is increased, and the kinetic performance of the battery cell is improved. According to some specific embodiments of this application, the coating weight of the positive electrode film can be 15 mg / cm³. 2 -20mg / cm 2 .
[0087] It should be noted that the coating weight of the positive electrode film referred to here refers to the coating weight of the positive electrode film on one side of the positive electrode sheet.
[0088] According to some embodiments of this application, the compaction density of the positive electrode film layer can be 2.2 g / cm³. 3 -2.6g / cm 3 For example, it could be 2.2 g / cm³. 3 2.3g / cm 3 2.4g / cm 3 2.5g / cm 3 Or 2.6g / cm 3 The values can be any range of the aforementioned values. Therefore, while increasing the energy density of the battery cell, the tortuosity of the positive electrode sheet is reduced, the lithium-ion diffusion rate is increased, and the kinetic performance of the battery cell is improved. According to some specific embodiments of this application, the compaction density of the positive electrode film is 2.3 g / cm³. 3 -2.5g / cm 3 .
[0089] This application provides a method for testing the coating weight of the positive electrode film: The positive electrode sheet is disassembled from a single battery cell. For example, a single-sided coated positive electrode sheet (if it is a double-sided coated sheet, the positive electrode film layer on one side can be wiped off first) is cut into small circular pieces with an area of S1, weighed, and recorded as M1, and its thickness H1 is measured. Then, the positive electrode film layer of the weighed positive electrode sheet is wiped off, the weight of the positive current collector is weighed and recorded as M0, and its thickness H0 is measured. The single-sided coating weight of the positive electrode film = (M1-M0) / S1, the thickness of the positive electrode film = H1-H0, and the compaction density of the positive electrode film = single-sided coating weight of the positive electrode film / thickness of the positive electrode film.
[0090] In some embodiments, the positive electrode sheet can be prepared by dispersing the above-mentioned components for preparing the positive electrode sheet, such as lithium iron phosphate material, lithium supplementer, conductive agent, binder and any other components, in a solvent (e.g., N-methylpyrrolidone) to form a positive electrode slurry; coating the positive electrode slurry onto the positive electrode current collector, and then obtaining the positive electrode sheet after drying, cold pressing and other processes.
[0091] [Negative electrode plate]
[0092] The negative electrode sheet includes a negative current collector and a negative electrode film layer located on at least one side of the negative current collector. The negative electrode film layer includes a negative electrode active material, which includes graphite.
[0093] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, copper foil may be used as the metal foil. The composite current collector may include a polymer substrate and a metal layer formed on at least one surface of the polymer substrate. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0094] According to some embodiments of this application, the coating weight of the negative electrode film is 5 mg / cm³. 2 -15mg / cm 2 For example, it could be 5 mg / cm³ 2 7mg / cm 2 8.6 mg / cm 2 9mg / cm 2 11mg / cm 2 13mg / cm 2 Or 15mg / cm 2 The values can be any range of the aforementioned values. This increases the energy density of the battery cell. According to some specific embodiments of this application, the coating weight of the negative electrode film can be 7 mg / cm³. 2 -11mg / cm 2 .
[0095] It should be noted that the coating weight of the negative electrode film referred to here refers to the coating weight of the negative electrode film on one side of the negative electrode sheet.
[0096] According to some embodiments of this application, the compaction density of the negative electrode film layer can be 1.2 g / cm³. 3 -1.7g / cm 3 For example, it could be 1.2 g / cm³. 3 1.32g / cm 3 1.4g / cm 3 1.5g / cm 3 1.6g / cm 3 Or 1.7g / cm 3 etc., or a range consisting of any of the above values.
[0097] The test method for the negative electrode coating weight in this application is the same as the test method for the positive electrode coating weight.
[0098] According to some embodiments of this application, the compaction density of the negative electrode film can be the compaction density of the negative electrode film in the negative electrode sheet corresponding to the battery cell at 100% SOC.
[0099] According to some embodiments of this application, the compaction density of the negative electrode film can be the compaction density of the negative electrode film in the negative electrode sheet corresponding to the battery cell at 0% SOC.
[0100] According to some embodiments of this application, the negative electrode film layer comprises graphite, and the volume average particle size Dv50 of the graphite is 8μm-14μm. This reduces the volume average particle size of the graphite, increases the rate of lithium ion insertion and extraction between the graphite layers, reduces the impedance of the battery cell, and improves kinetic performance.
[0101] As an example, the volume average particle size Dv50 of the graphite can be 8μm, 10μm, 12μm or 14μm, or a range of any of the above values.
[0102] In this application, Dv50 refers to the particle size corresponding to a cumulative volume distribution percentage of 50%, for example, measured using a laser particle size analyzer (Malvern Master Size 2000) in accordance with standard GB / T 19077-2016 / ISO 13320:2009.
[0103] According to some embodiments of this application, the negative electrode film layer includes graphite, which has a layered structure. The OI value can measure the ability of graphite material to insert or extract lithium ions, and the OI value of graphite is 2-5. Therefore, by reducing the OI value of graphite, the kinetic performance of the battery is improved.
[0104] As an example, the OI value of the graphite can be 2, 3, 4 or 5, or a range of any of the above values.
[0105] According to some embodiments of this application, the graphite includes artificial graphite. Therefore, artificial graphite has fewer surface active sites than natural graphite, which can improve the lifespan of individual battery cells.
[0106] In some embodiments, the negative electrode film layer may optionally include a binder. The binder may be selected from at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).
[0107] In some embodiments, the negative electrode film may optionally include a conductive agent. The conductive agent may be selected from at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers. More preferably, superconducting carbon and carbon nanotubes may be used in combination to further improve the conductivity of the negative electrode film and the conductivity between the negative electrode film and the negative electrode current collector.
[0108] In some embodiments, the negative electrode film may optionally include other additives, such as thickeners (e.g., sodium carboxymethyl cellulose (CMC-Na)).
[0109] In some embodiments, the negative electrode sheet can be prepared by dispersing the components used to prepare the negative electrode sheet, such as the negative electrode active material, conductive agent, binder and any other components, in a solvent (e.g., deionized water) to form a negative electrode slurry; coating the negative electrode slurry onto the negative electrode current collector, and then obtaining the negative electrode sheet after drying, cold pressing and other processes.
[0110] Electrolyte
[0111] Typically, electrolytes consist of solvents, lithium salts, and additives.
[0112] According to some embodiments of this application, the total mass percentage of the lithium salt in the electrolyte can be 8%-13%. For example, it can be 8%, 9%, 10%, 11%, 12%, or 13%, or any range of the above values. This improves the ionic conductivity of the electrolyte. According to some specific embodiments of this application, the total mass percentage of the lithium salt can be 10%-12%.
[0113] According to some embodiments of this application, the inorganic lithium salt includes lithium hexafluorophosphate. Based on the total mass of the electrolyte, the mass percentage of the inorganic lithium salt can be 7.5%-12%, thereby improving the ionic conductivity of the electrolyte. By keeping the content of the inorganic lithium salt within the above range, a low-resistance and moderately hard SEI film is formed on the negative electrode surface, effectively suppressing electrode expansion during cycling caused by graphite expansion and improving the cycle performance of the battery cell.
[0114] As an example, the mass percentage of the inorganic lithium salt can be 7.5%, 8%, 9%, 10%, 11%, or 12%, or a range of any of the above values.
[0115] According to some embodiments of this application, the organic lithium salt includes at least one of lithium bis(fluorosulfonyl)imide (LIFSI) and lithium bis(trifluorosulfonyl)imide (LITFSI), and the mass percentage of the organic lithium salt can be 1%-4% based on the total mass of the electrolyte. This reduces the impedance of the SEI film, increases the ionic conductivity of the SEI film, and improves the kinetic performance of the battery. Simultaneously, it reduces the probability of fluorine forming aluminum fluoride with the positive electrode current collector due to excessive organic lithium salt content, thus reducing the risk of corrosion of the positive electrode current collector.
[0116] As an example, based on the total mass of the electrolyte, the mass percentage of the organic lithium salt can be 1%, 2%, 3%, or 4%, or a range of any of the above values.
[0117] According to some embodiments of this application, the solvent includes cyclic carbonates and linear carbonates. This increases the dielectric constant of the electrolyte, reduces the viscosity of the electrolyte, and increases the migration rate of lithium ions.
[0118] According to some embodiments of this application, based on the total mass of the electrolyte, the mass percentage of the cyclic carbonate can be 15%-25%, and the mass percentage of the linear carbonate can be 50%-70%. This increases the dielectric constant of the electrolyte, reduces its viscosity, and improves the migration rate of lithium ions.
[0119] As an example, based on the total mass of the electrolyte, the mass percentage of the cyclic carbonate can be 15%, 17%, 19%, 21%, 23%, or 25%, or a range of any of the above values.
[0120] According to some specific embodiments of this application, the mass percentage of the cyclic carbonate can be 22%-25% based on the total mass of the electrolyte.
[0121] As an example, based on the total mass of the electrolyte, the mass percentage of the linear carbonate can be 50%, 55%, 60%, 65%, or 70%, or a range of any of the above values.
[0122] According to some embodiments of this application, the cyclic carbonate includes at least one of ethylene carbonate (EC) or propylene carbonate.
[0123] According to some embodiments of this application, the linear carbonate includes at least one of dimethyl carbonate, ethyl methyl carbonate, and diethyl carbonate.
[0124] According to some embodiments of this application, the linear carbonate includes dimethyl carbonate (DMC) and ethyl methyl carbonate (EMC). Based on the total mass of the electrolyte, the mass percentage of dimethyl carbonate can be 30%-40%, and the mass percentage of ethyl methyl carbonate can be 30%-40%. This reduces the viscosity of the electrolyte.
[0125] As an example, based on the total mass of the electrolyte, the mass percentage of DMC can be 30%, 32%, 34%, 36%, 38%, or 40%, or a range of any of the above values.
[0126] As an example, based on the total mass of the electrolyte, the mass percentage of EMC can be 30%, 32%, 34%, 36%, 38%, or 40%, or a range of any of the above values.
[0127] According to some embodiments of this application, the electrolyte may further include linear carboxylic acid esters, wherein the mass percentage of the linear carboxylic acid esters is 5%-15% based on the total mass of the electrolyte. This improves the conductivity of the electrolyte and enhances the kinetic performance of the battery cell; furthermore, controlling the content of the linear carboxylic acid esters to not exceed 15% improves the high-temperature stability of the electrolyte.
[0128] As an example, the mass percentage of the linear carboxylic acid ester can be 5%, 7%, 9%, 11%, 13%, or 15%, or a range of any of the above values.
[0129] According to some embodiments of this application, the linear carboxylic acid ester includes at least one selected from methyl formate, methyl acetate, ethyl formate, and ethyl acetate. This improves the conductivity of the electrolyte and enhances the kinetic performance of the battery cell.
[0130] According to some embodiments of this application, the lithium replenishment agent has a high decomposition voltage. To improve the high-voltage resistance of the electrolyte, the electrolyte further includes additives, which include at least one of fluorine-containing additives or phosphorus-containing additives. Thus, the above-mentioned additives can preferentially decompose compared to the solvent, and after decomposition, a stable CEI film can be formed, reducing the risk of transition metal dissolution in the cathode material under high-voltage formation conditions, reducing the risk of electrolyte oxidative decomposition, improving the cycle stability of the electrolyte, and improving the cycle performance of the battery cell.
[0131] According to some embodiments of this application, the additives include fluorine-containing additives and phosphorus-containing additives, and the sum of the masses of the fluorine-containing additives and the phosphorus-containing additives accounts for 0.05%-1% based on the total mass of the electrolyte. Therefore, by keeping the sum of the masses of the fluorine-containing additives and the phosphorus-containing additives within the above range, the stability of the CEI film is improved, the risk of oxidative decomposition of the electrolyte during the formation stage is reduced, the cycle stability of the electrolyte is improved, and the cycle performance of the battery cell is enhanced.
[0132] In this application, the types and contents of electrolyte additives can be tested with reference to GB / T 9722-2006 Chemical Reagents - Gas Chromatography. Specifically, a certain amount of electrolyte is tested using a gas chromatograph. By utilizing the different adsorption and desorption capacities of the various components of the electrolyte in the chromatographic column, the components of the electrolyte are separated. The separated sample is then tested using a gas chromatograph-mass spectrometer (GC-MS).
[0133] As an example, the percentage of the sum of the mass of the fluorine-containing additive and the phosphorus-containing additive may be 0.05%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, or 1%, or may be a range of any of the above values.
[0134] According to some specific embodiments of this application, based on the total mass of the electrolyte, the mass percentage of the fluorine-containing additive is 0.05%-0.5%, and the mass percentage of the phosphorus-containing additive is 0.05%-0.5%. This improves the stability of the CEI membrane, reduces the risk of high-voltage oxidation of the electrolyte during the formation stage, enhances the cycle stability of the electrolyte, and improves the cycle performance of the battery cell.
[0135] As an example, the mass percentage of the fluorinated additive can be 0.05%, 0.1%, 0.2%, 0.3%, 0.4%, or 0.5%, or a range of any of the above values.
[0136] As an example, the mass percentage of the phosphorus-containing additive can be 0.05%, 0.1%, 0.2%, 0.3%, 0.4%, or 0.5%, or a range of any of the above values.
[0137] According to some embodiments of this application, the fluorinated additive includes at least one of fluoroethylene carbonate (FEC), difluoroethylene carbonate (DFEC), and perfluoroalkyl ethylene carbonate.
[0138] According to some embodiments of this application, the phosphorus-containing additive includes at least one of tris(trimethylsilyl)phosphate (TMSP), triphenylphosphine oxide (TPPO), tri(2,2,2-trifluoroethyl) phosphate (TFEP), trimethylolpropane (TMP), and 2-trifluoroethoxy-2-oxo-1,3,2-dioxophosphazenecyclopentane (TFEOP).
[0139] According to some embodiments of this application, the additive further includes carbonate additives, including at least one selected from vinylene carbonate (VC), propylene carbonate, and vinyl ethylene carbonate. Therefore, by adding carbonate additives to the electrolyte, a polymer-containing SEI film can be formed on the negative electrode surface, improving the stability of the SEI film and increasing the lifespan of the battery cell.
[0140] According to some embodiments of this application, the carbonate additive includes vinylene carbonate, and the mass percentage of vinylene carbonate can be 0.5%-3% based on the total mass of the electrolyte. Therefore, by adding a carbonate additive to the electrolyte, a polymer-containing SEI film can be formed on the negative electrode surface, improving the stability of the SEI film and increasing the lifespan of the battery cell.
[0141] As an example, based on the total mass of the electrolyte, the mass percentage of vinylene carbonate can be 0.5%, 1%, 1.5%, 2%, 2.5%, or 3%, or a range of any of the above values. According to some specific embodiments of this application, the mass percentage of vinylene carbonate can be 1%-2%.
[0142] According to some embodiments of this application, the electrolyte injection coefficient of the battery cell is 3g / Ah-3.8g / Ah. For example, it can be 3g / Ah, 3.2g / Ah, 3.4g / Ah, 3.6g / Ah, or 3.8g / Ah, or any range of the above values. This improves the battery's kinetic performance and cycle life.
[0143] [Isolation membrane]
[0144] In some embodiments, the battery cell also includes a separator. This application does not impose any particular limitation on the type of separator; any known porous separator with good chemical and mechanical stability can be selected.
[0145] According to some embodiments of this application, the separator includes a base film, at least one side of which has a coating. The base film is made of at least one of polyethylene or polypropylene. This reduces the risk of the separator being oxidized under high pressure conditions.
[0146] According to some embodiments of this application, the coating may be a ceramic coating.
[0147] According to some embodiments of this application, the thickness of the separator can be 7μm-15μm. For example, it can be 7μm, 9μm, 11μm, 13μm or 15μm, or any range of the above values.
[0148] In some implementations, the positive electrode, negative electrode, and separator can be fabricated into an electrode assembly using a winding or stacking process.
[0149] In some embodiments, the battery cell may include an outer packaging. This outer packaging can be used to encapsulate the electrode assembly and electrolyte described above.
[0150] In some embodiments, the outer packaging of the battery cell can be a rigid shell, such as a hard plastic shell, an aluminum shell, or a steel shell. The outer packaging of the battery cell can also be a flexible package, such as a pouch. The material of the flexible package can be plastic; examples of plastics include polypropylene, polybutylene terephthalate, and polybutylene succinate.
[0151] This application does not impose any particular limitation on the shape of the battery cell; it can be cylindrical, square, or any other arbitrary shape. For example, Figure 1 The example shown is a square-structured battery cell 5.
[0152] In some implementations, refer to Figure 2 The outer packaging may include a housing 51 and a cover plate 53. The housing 51 may include a base plate and side plates connected to the base plate, the base plate and side plates forming a receiving cavity. The housing 51 has an opening communicating with the receiving cavity, and the cover plate 53 can be placed over the opening to close the receiving cavity. The positive electrode sheet, negative electrode sheet, and separator can be formed into an electrode assembly 52 by a winding process or a stacking process. The electrode assembly 52 is encapsulated within the receiving cavity. Electrolyte is immersed in the electrode assembly 52. The number of electrode assemblies 52 contained in a single battery cell 5 can be one or more, which can be selected by those skilled in the art according to specific practical needs.
[0153] The second aspect of this application provides a battery device, including the battery cell provided in the first aspect of this application, wherein the battery device is at least one of a battery module, a battery pack, and an energy storage device.
[0154] In some implementations, individual battery cells can be assembled into a battery module. The number of individual battery cells contained in a battery module can be one or more, and the specific number can be selected by those skilled in the art based on the application and capacity of the battery module.
[0155] Figure 3 This is battery module 4, used as an example. (See reference...) Figure 3In battery module 4, multiple battery cells 5 can be arranged sequentially along the length of battery module 4. Of course, they can also be arranged in any other manner. Furthermore, these multiple battery cells 5 can be fixed in place using fasteners.
[0156] Optionally, the battery module 4 may also include a housing with a receiving space in which multiple battery cells 5 are received.
[0157] In some embodiments, the battery modules described above can also be assembled into a battery pack, and the number of battery modules contained in the battery pack can be one or more, the specific number of which can be selected by those skilled in the art according to the application and capacity of the battery pack.
[0158] Figure 4 and Figure 5 This is battery pack 1 as an example. (See reference...) Figure 4 and Figure 5 The battery pack 1 may include a battery box and multiple battery modules 4 disposed within the battery box. The battery box includes an upper body 2 and a lower body 3, with the upper body 2 covering the lower body 3 to form a closed space for accommodating the battery modules 4. The multiple battery modules 4 can be arranged in any manner within the battery box.
[0159] In addition, this application also provides an electrical device, which includes at least one of the battery cell, battery module, or battery pack provided in this application. The battery cell, battery module, or battery pack can be used as a power source for the electrical device, or as an energy storage unit for the electrical device. The electrical device may include, but is not limited to, mobile devices (e.g., mobile phones, laptops, etc.), electric vehicles (e.g., pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc.
[0160] As the electrical equipment, battery cells, battery modules, or battery packs can be selected according to their usage requirements.
[0161] Figure 6 This is an example of an electrical device. The device could be a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. To meet the device's requirements for high power and high energy density batteries, a battery pack or battery module can be used.
[0162] Another example device could be a mobile phone, tablet, or laptop. These devices typically require a slim and lightweight design and can use a single battery cell as their power source.
[0163] To make the technical problems, technical solutions, and beneficial effects solved by the embodiments of this application clearer, the following will provide a more detailed description in conjunction with the embodiments and accompanying drawings. Obviously, the described embodiments are only a part of the embodiments of this application, and not all of them. The following description of at least one exemplary embodiment is merely illustrative and is in no way intended to limit this application or its applications. Based on the embodiments of this application, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this application.
[0164] Example 1
[0165] 1. Positive electrode sheet
[0166] The positive electrode sheet includes a positive current collector aluminum foil, with a positive electrode film layer on both surfaces of the aluminum foil, and a compaction density of 2.39 g / cm³. 3 The coating weight of the single-sided positive electrode film is 18.5 mg / cm³. 2 Based on the total mass of the single-sided positive electrode film, the positive electrode film includes lithium iron phosphate material with a mass ratio of 94.5%, lithium supplementer Li2NiO2 with a mass ratio of 2.5%, conductive agent carbon black with a mass ratio of 0.8%, and binder polyvinylidene fluoride (PVDF) with a mass ratio of 2.2%. The lithium iron phosphate surface has a first carbon coating layer, and based on the total mass of lithium iron phosphate, the mass ratio of the first carbon coating layer is 1.5%.
[0167] 2. Negative electrode plate
[0168] The negative electrode sheet includes a negative current collector copper foil, with a negative electrode film layer on both surfaces of the copper foil, and a compaction density of 1.32 g / cm³. 3 The coating weight of the single-sided negative electrode film is 8.6 mg / cm³. 2 Based on the total mass of the single-sided negative electrode film, the negative electrode film includes 96.6% artificial graphite (OI value of 3.63), 0.4% conductive carbon black, 1.8% binder styrene-butadiene rubber (SBR), and 1.2% thickener sodium carboxymethyl cellulose (CMC-Na).
[0169] 3. Electrolyte
[0170] The electrolyte comprises solvents, electrolyte salts, and additives. The solvents include EC, DMC, and EMC, with a mass ratio of 24:38:38. The additives include TMSP, FEC, and VC, with TMSP accounting for 0.23% of the total electrolyte mass, FEC accounting for 0.12%, and VC accounting for 1.39%. The electrolyte salts are LiPF6 and LIFSI, with LiPF6 accounting for 9.383% and LIFSI accounting for 2.57% of the total electrolyte mass.
[0171] 4. Separating membrane
[0172] Polypropylene film, 12μm thick.
[0173] 5. Battery cell
[0174] A single battery cell includes a positive electrode, a separator, a negative electrode, and an electrolyte.
[0175] Performance testing
[0176] 1. DCR Test
[0177] At 25℃, the battery cell is charged at a constant current of 1 / 3C to 3.65V, then charged at a constant voltage of 3.65V to a current of 0.05C. After resting for 5 minutes, it is discharged at a constant current of 1 / 3C for 90 minutes and then rested for 120 minutes. The voltage V1 is recorded. Then it is discharged at 4C for 30 seconds, and the voltage V2 is recorded. The internal resistance DCR of the battery cell is obtained by dividing (V2-V1) / 4C.
[0178] 2.1000-cycle capacity retention
[0179] At 25°C, the corresponding battery cell is charged to 3.65V at a constant current of 1 / 3C, then charged to 0.05C at a constant voltage of 3.65V, left to rest for 5 minutes, and then discharged to 2.5V at 1 / 3C. The resulting capacity is recorded as the initial capacity C0. The above steps are repeated for the same battery cell, and the discharge capacity C of the battery cell after the nth cycle is recorded. n Then, the battery cell capacity retention rate P after each cycle n =C n / C0×100%. In this test, the first loop corresponds to n=1, the second loop corresponds to n=2, ... the 1000th loop corresponds to n=1000.
[0180] 3. Capacity retention rate after 150 days of storage at 60℃
[0181] At 25℃, the corresponding battery cell was charged at a constant current of 1 / 3C to 3.65V, then charged at a constant voltage of 3.65V to a current of 0.05C, rested for 5 minutes, and then discharged at 1 / 3C to 2.5V. The resulting capacity was recorded as the initial capacity C0. Alternatively, the battery cell was charged at 1 / 3C to 3.65V and then charged at a constant voltage of 0.05C. Afterward, the battery cell was placed in a 60℃ constant temperature oven for 150 days and then discharged at room temperature at 1 / 3C to 2.5V. After being removed, the battery cell was charged at 25℃ at a constant current of 1 / 3C to 3.65V, then charged at a constant voltage of 3.65V to a current of 0.05C, rested for 5 minutes, and then discharged at 1 / 3C to 2.5V. The capacity C was recorded. n The capacity retention rate is (Cn / C0)×100%.
[0182] Example 2, Example 3, Comparative Example 2, Comparative Example 3
[0183] The positive electrode, negative electrode, electrolyte solvent, and additives in the battery cell are the same as in Example 1, except that the mass ratios of LiPF6 and LIFSI are different, and the mass ratios of inorganic lithium salt and organic lithium salt are different.
[0184] Example 4
[0185] The positive electrode, negative electrode, electrolyte solvent, and additives in the battery cell are the same as in Example 1, except that the organic lithium salt is LITFSI.
[0186] Comparative Example 1
[0187] The negative electrode and electrolyte in the battery cell are the same as in Example 1, except that the positive electrode film does not contain lithium replenishing agent.
[0188] The differences between Examples 1-4 and Comparative Examples 1-3 are detailed in Table 1:
[0189] Table 1
[0190]
[0191] As can be seen from the comparison between Examples 1-3 and Comparative Examples 1-3, the battery cell proposed in this application has a lower internal resistance and higher cycle capacity retention and high-temperature capacity retention. This indicates that by adding a lithium supplement to the positive electrode film layer, this application can improve the high-temperature cycle performance of the battery cell; by controlling the relative content of organic lithium salt and inorganic lithium salt in the electrolyte within a reasonable range, the side reactions between the transition metal oxides formed by the lithium supplement and the electrolyte can be reduced, thereby improving the cycle performance of the battery. At the same time, the low SEI impedance formed by the combination of organic and inorganic lithium salts can increase the lithium ion insertion / extraction rate in graphite and improve the power performance of the battery cell.
[0192] As can be seen from Examples 4 and 1, different types of organic lithium salts have the effect of improving the cycle performance and power performance of battery cells.
[0193] Example 5, Example 6
[0194] The positive electrode, negative electrode, electrolyte solvent, and additives in the battery cell are the same as in Example 1, except that the content of TMSP is different.
[0195] Example 7, Example 8
[0196] The positive electrode, negative electrode, electrolyte solvent, and additives in the battery cell are the same as in Example 1, except that the content of FEC is different.
[0197] The differences between Examples 5-8 are detailed in Table 2.
[0198] Table 2
[0199]
[0200] As can be seen from Examples 1 and 5-8, by controlling the content of phosphorus-containing additives and fluorine-containing additives in the electrolyte, the internal resistance, cycle capacity retention rate, and high-temperature capacity retention rate of the battery cell can be adjusted, thereby obtaining a battery cell with both long life and low internal resistance.
[0201] Example 9, Example 10
[0202] The positive electrode, negative electrode, electrolyte salt, and additives in the battery cell are the same as in Example 1. The difference is that the electrolyte solvent also includes methyl acetate (MA), and the content of MA is different, as detailed in Table 3.
[0203] Table 3
[0204]
[0205]
[0206] As can be seen from Examples 1, 9 and 10, by adding different amounts of MA to the electrolyte, the internal resistance of the battery cell can be further reduced, thereby improving the dynamic performance of the battery cell.
[0207] Example 11
[0208] The negative electrode and electrolyte in the battery cell are the same as in Example 1, except that the type of lithium replenishing agent is different.
[0209] Example 12, Example 13
[0210] The negative electrode and electrolyte in the battery cell are the same as in Example 1, except that the compaction density of the positive electrode film is different.
[0211] The types of lithium replenishing agents in Example 11 and the compaction densities of the positive electrode films in Examples 12 and 13 are detailed in Table 4.
[0212] Table 4
[0213]
[0214] As can be seen from Examples 1 and 11, different types of lithium replenishing agents can all improve the battery cycle performance.
[0215] As can be seen from Examples 1, 12 and 13, forming positive electrode film layers with different compaction densities can all yield battery cells with both long lifespan and low internal resistance.
[0216] Examples 14 and 15
[0217] The positive electrode and electrolyte in the battery cell are the same as in Example 1, except that the OI value of the negative electrode graphite is different.
[0218] Examples 16 and 17
[0219] The positive electrode and electrolyte in the battery cell are the same as in Example 1, except that the volume average particle size of the graphite in the negative electrode is different.
[0220] Examples 18 and 19
[0221] The positive electrode and electrolyte in the battery cell are the same as in Example 1, except that the compaction density of the negative electrode film is different.
[0222] The differences between the negative electrode plates in Examples 14-19 are detailed in Table 5.
[0223] Table 5
[0224]
[0225]
[0226] As can be seen from Examples 1, 14 and 15, by reducing the OI value of graphite, the internal resistance of the battery cell can be reduced, and at the same time, the battery cell can have excellent cycle performance.
[0227] As can be seen from Examples 1, 16 and 17, by reducing the volume average particle size of graphite, the internal resistance of the battery cell can be reduced, and at the same time, the battery cell can have excellent cycle performance.
[0228] As can be seen from Examples 1, 18 and 19, forming negative electrode film layers with different compaction densities can all yield battery cells with both long lifespan and low internal resistance.
[0229] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of this application, and not to limit them. Although this application has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features therein. These modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of this application, and they should all be covered within the scope of the claims and specification of this application. In particular, as long as there is no structural conflict, the various technical features mentioned in the embodiments can be combined in any way. This application is not limited to the specific embodiments disclosed herein, but includes all technical solutions falling within the scope of the claims.
Claims
1. A battery cell, characterized in that, include: A positive electrode sheet, wherein the positive electrode sheet includes a positive electrode film layer, the positive electrode film layer includes lithium iron phosphate material and a lithium replenishing agent; A negative electrode sheet, wherein the negative electrode sheet includes a negative electrode film layer, the negative electrode film layer includes a negative electrode active material, and the negative electrode active material includes graphite; the OI value of the graphite is 2-5, and the volume average particle size Dv50 of the graphite is 8μm-14μm; A separator membrane, the separator membrane being located between the positive electrode and the negative electrode; and, The electrolyte comprises a lithium salt, which includes an organic lithium salt and an inorganic lithium salt. The organic lithium salt includes at least one of lithium fluorosulfonylimide, lithium fluorooxalate borate, and lithium fluorooxalate phosphate. The inorganic lithium salt includes at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, and lithium fluorosulfonate. The mass ratio of the inorganic lithium salt to the organic lithium salt is (2-6):
1.
2. The battery cell according to claim 1, characterized in that, The organic lithium salt includes at least one of lithium bis(fluorosulfonyl)imide and lithium bis(trifluorosulfonyl)imide, and the mass percentage of the organic lithium salt is 1%-4% based on the total mass of the electrolyte.
3. The battery cell according to claim 1, characterized in that, The inorganic lithium salt includes lithium hexafluorophosphate, and the inorganic lithium salt accounts for 7.5%-12% of the total mass of the electrolyte.
4. The battery cell according to claim 1, characterized in that, The graphite includes synthetic graphite.
5. The battery cell according to any one of claims 1-4, characterized in that, The lithium supplement includes Li x M y O z M includes at least one of Ni, Co, V, Cr, Mn, Fe, Mo, Cu, and Zn, where 0 < x ≤ 5, 1 ≤ y ≤ 3, and 2 ≤ z ≤ 8.
6. The battery cell according to any one of claims 1-4, characterized in that, The lithium supplement includes at least one of Li2NiO2 and Li5FeO4.
7. The battery cell according to any one of claims 1-4, characterized in that, The lithium supplement includes Li n NiO m Li e FeO f At least one of the following, wherein 0 < m ≤ 2, 0 < n ≤ 2, 0 < e ≤ 5, and 0 < f ≤ 4.
8. The battery cell according to any one of claims 1-4, characterized in that, The lithium supplement includes Li p FeO q , where 0 < p ≤ 1, 0 < q ≤ 2.
9. The battery cell according to any one of claims 1-4, characterized in that, The electrolyte also includes a solvent, which includes cyclic carbonates and linear carbonates.
10. The battery cell according to claim 9, characterized in that, Based on the total mass of the electrolyte, the cyclic carbonate accounts for 15%-25% of the mass, and the linear carbonate accounts for 50%-70% of the mass.
11. The battery cell according to claim 9, characterized in that, The cyclic carbonate includes at least one of ethylene carbonate or propylene carbonate; and / or The linear carbonate includes at least one of dimethyl carbonate, ethyl methyl carbonate, and diethyl carbonate.
12. The battery cell according to claim 9, characterized in that, The linear carbonate includes dimethyl carbonate and ethyl methyl carbonate, and based on the total mass of the electrolyte, the mass percentage of dimethyl carbonate is 30%-40% and the mass percentage of ethyl methyl carbonate is 30%-40%.
13. The battery cell according to claim 9, characterized in that, The electrolyte includes linear carboxylic acid esters, and the mass percentage of the linear carboxylic acid esters is 5%-15% based on the total mass of the electrolyte.
14. The battery cell according to claim 13, characterized in that, The linear carboxylic acid ester includes at least one of methyl formate, methyl acetate, ethyl formate, and ethyl acetate.
15. The battery cell according to claim 1, characterized in that, The electrolyte also includes additives, which include at least one of fluorine-containing additives or phosphorus-containing additives.
16. The battery cell according to claim 15, characterized in that, The additives include fluorine-containing additives and phosphorus-containing additives, and the sum of the masses of the fluorine-containing additives and the phosphorus-containing additives accounts for 0.05%-1% based on the total mass of the electrolyte.
17. The battery cell according to claim 15, characterized in that, Based on the total mass of the electrolyte, the mass percentage of the fluorine-containing additive is 0.05%-0.5%, and the mass percentage of the phosphorus-containing additive is 0.05%-0.5%.
18. The battery cell according to claim 15, characterized in that, The fluorinated additive includes at least one of fluoroethylene carbonate, difluoroethylene carbonate, and perfluoroalkyl ethylene carbonate; and / or The phosphorus-containing additive includes at least one of tris(trimethylsilyl) phosphate, triphenylphosphine oxide, tris(2,2,2-trifluoroethyl) phosphite, trimethylolpropane, tris(2,2,2-trifluoroethyl) phosphate, and 2-trifluoroethoxy-2-oxo-1,3,2-dioxophosphazenecyclopentane.
19. The battery cell according to claim 15, characterized in that, The additives also include carbonate additives, which include at least one of vinylene carbonate, propylene carbonate, and vinyl ethylene carbonate.
20. The battery cell according to claim 19, characterized in that, The carbonate additive includes vinylene carbonate, and the mass percentage of vinylene carbonate is 0.5%-3% based on the total mass of the electrolyte.
21. The battery cell according to claim 1, characterized in that, The lithium iron phosphate has at least a portion of its surface covered by a first carbon coating layer, wherein the mass percentage of the first carbon coating layer is 0.5%-1.5% based on the total mass of the lithium iron phosphate; and / or At least a portion of the surface of the lithium replenishing agent has a second carbon coating layer, and the mass percentage of the second carbon coating layer is 1%-5% based on the total mass of the lithium replenishing agent.
22. The battery cell according to claim 1, characterized in that, Based on the total mass of the positive electrode film, the mass percentage of the lithium replenishing agent is 0.5%-5%.
23. The battery cell according to claim 1, characterized in that, The coating weight of the positive electrode film is 10 mg / cm³. 2 -25mg / cm 2 .
24. The battery cell according to claim 1, characterized in that, The compaction density of the positive electrode film is 2.2 g / cm³. 3 -2.6g / cm 3 .
25. The battery cell according to claim 1, characterized in that, The coating weight of the negative electrode film is 5 mg / cm³. 2 -15mg / cm 2 .
26. The battery cell according to claim 1, characterized in that, The compaction density of the negative electrode film is 1.2 g / cm³. 3 -1.7g / cm 3 .
27. The battery cell according to claim 1, characterized in that, The isolation membrane includes a base membrane, and at least one side of the base membrane has a coating.
28. The battery cell according to claim 1, characterized in that, The thickness of the isolation membrane is 7μm-15μm.
29. The battery cell according to claim 1, characterized in that, The electrolyte injection coefficient of the battery cell is 3g / Ah-3.8g / Ah.
30. A battery device, characterized in that, Includes the battery cell according to any one of claims 1-29, wherein the battery device is at least one of battery module, battery pack, and energy storage device.
31. An electrical appliance, characterized in that, Includes a battery cell according to any one of claims 1-29 or a battery device according to claim 30, wherein the battery cell or the battery device is used to provide electrical energy.
Citation Information
Patent Citations
Lithium supplement additive, positive pole piece, battery and electric device
CN117239104A
Battery monomer, battery and electric device
CN117878410A